Preparation method of low-leakage-current rare earth high-entropy nanometer composite insulating material

By preparing rare-earth high-entropy nanocomposite insulating materials, and utilizing the thermodynamic effects and structural distortions of high-entropy materials, the problem of high leakage current in existing magnesium oxide electrical insulating materials under harsh environments was solved, and an insulating material with low leakage current and high insulation performance was achieved.

CN117352243BActive Publication Date: 2026-11-20YINGKOU INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311102164.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-30
Publication Date
2026-11-20
Estimated Expiration
2043-08-30

AI Technical Summary

Technical Problem

Existing pure-phase magnesium oxide electrical insulation materials cannot meet the needs of high-end electrical insulation materials, especially in harsh service environments where leakage current is high, necessitating the development of superior insulation materials.

Method used

By preparing rare-earth high-entropy nanocomposite insulating materials, utilizing the thermodynamic high-entropy effect and structural lattice distortion of high-entropy materials, and using Y(NO₃)₃, La(NO₃)₃, Ce(NO₃)₃, Gd(NO₃)₃, Mg(NO₃)₂, glycine, and ethylene glycol as raw materials, a (Y)₃ high-entropy nanocomposite insulating material was prepared. 0.25 La 0.25 Ce 0.25 Gd 0.25 ₂O₃-MgO high-entropy nanocomposite powder enhances phonon scattering to reduce leakage current.

Benefits of technology

It achieves low leakage current performance of materials under harsh service environments, improves insulation performance, and exhibits excellent electrical insulation performance indicators such as low leakage current and high insulation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

A method for preparing a low-leakage-current rare-earth high-entropy nanocomposite insulating material is disclosed. This invention relates to a method for preparing an insulating material, using Y(NO3)3, La(NO3)3, Ce(NO3)3, Gd(NO3)3, Mg(NO3)2, glycine, and ethylene glycol as main raw materials, according to the final product (Y... 0.25 La 0.25 Ce 0.25 Gd 0.25 The solutions were prepared by mixing O₂O₃ and MgO in volume ratios of 15:85, 25:75, 35:65, 45:55, and 50:50. The resulting mixtures were then heated, stirred, dried, calcined, ball-milled, dried again, and sieved to obtain the target nanocomposite insulating powder. The high-entropy nanocomposite insulating material underwent electrical performance testing at 1050℃ (155 V, 860 W, 15 minutes). The results showed that the material had a leakage current of only 0.056 mA, an insulation resistance of 80 MΩ after 10 minutes of high-temperature furnace treatment, a moisture resistance of 5.5 MΩ, and a hot resistance of 3.5 MΩ, demonstrating excellent electrical insulation properties and improving the safety of electrical insulation materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing insulating materials, and more particularly to a method for preparing a composite insulating material of rare-earth high-entropy nanomaterials with low leakage current. Background Technology

[0002] Magnesium oxide is widely used in electrical materials and fillers for electromagnetic devices due to its excellent high-temperature stability, corrosion resistance, high thermal conductivity, and large coefficient of thermal expansion. In particular, its excellent insulation properties make it even more promising for use in insulating fillers.

[0003] With the continuous improvement of technology, the service environment of electrical insulation materials is becoming increasingly harsh, which puts forward higher requirements for the service performance of electrical insulation materials. The electrical insulation performance of the commonly used pure phase magnesium oxide can no longer meet the current high-end requirements of insulation material fillers. Therefore, it is urgent to develop an insulation material with better insulation performance. Summary of the Invention

[0004] The purpose of this invention is to provide a method for preparing rare-earth high-entropy nanocomposite insulating materials with low leakage current. This method utilizes the high-entropy effect in thermodynamics and lattice distortion in the structure of high-entropy materials to prepare a rare-earth high-entropy nanocomposite insulating material system, thereby enhancing phonon scattering and reducing the leakage current of the material.

[0005] The objective of this invention is achieved through the following technical solution: A method for preparing a low-leakage-current rare-earth high-entropy nanocomposite insulating material, wherein the composite insulating material is prepared from rare-earth high-entropy nanocomposite powder using Y(NO3)3, La(NO3)3, Ce(NO3)3, Gd(NO3)3, Mg(NO3)2, glycine and ethylene glycol as raw materials, wherein the rare-earth high-entropy nanocomposite powder contains (Y 0.25 La 0.25 Ce 0.25 Gd 0.25 The volume ratio of O2 to MgO is 15:85, 25:75, 35:65, 45:55, and 50:50. The specific preparation steps are as follows: S1: The formulation includes Y 3+ La 3+ Ce 3+ Gd 3+ Mg 2+ A solution of metal ion nitrates, the five are arranged according to the final product (Y). 0.25 La 0.25 Ce 0.25 Gd 0.25The volume ratios of 2O3 and MgO were 15:85, 25:75, 35:65, and 50:50, and the mixture was stirred at room temperature. S2: Add glycine to the solution prepared in S1 according to the molar ratio of metal cation to glycine of 1:0.5~1.2 to form a mixed solution; S3: Add ethylene glycol to the mixed solution of S2 according to the molar ratio of metal cation to ethylene glycol of 1:0.01~0.07 to form a new mixed solution; S4: Heat and stir the mixed solution obtained in step S3 in a 90°C water bath until the mixed solution forms a colorless, transparent, viscous solution; S5: The colorless, transparent, viscous solution obtained in step S4 is dried at 110℃ to obtain a precursor. Finally, the precursor is calcined at 400℃~800℃ for 2~8 h to obtain a preliminary (Y) 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3-MgO high-entropy nanocomposite powder; S6: The high-entropy nanocomposite powder obtained in step S5 is further ball-milled and sieved to finally obtain the target rare-earth high-entropy insulating material.

[0006] The method for preparing a low-leakage-current rare-earth high-entropy nanocomposite insulating material, wherein step S1 involves preparing a material containing Y... 3+ La 3+ Ce 3+ Gd 3+ Mg 2+ A metal cation nitrate solution with adjustable concentration to ensure that the five solutions are formulated according to the final product (Y). 0.25 La 0.25 Ce 0.25 Gd 0.25 The 2O3 and MgO can be mixed in a volume ratio of 15:85, 25:75, 35:65, 45:55, or 50:50.

[0007] In the method for preparing a low-leakage-current rare-earth high-entropy nanocomposite insulating material, the molar ratio of metal cations to glycine in step S2 is adjustable, and the ratio can be controlled within the range of 1:0.5~1.2.

[0008] In the method for preparing a low-leakage-current rare-earth high-entropy nanocomposite insulating material, the molar ratio of metal cations to ethylene glycol in step S3 is adjustable, and the ratio can be controlled within the range of 1:0.01~0.07.

[0009] In the method for preparing a low-leakage-current rare-earth high-entropy nanocomposite insulating material, the calcination temperature of the precursor in step S4 is adjustable, and the temperature can be controlled within the range of 400℃ to 800℃. At the same time, the calcination time is also adjustable, and the calcination time can be controlled within the range of 2 to 8 hours.

[0010] This invention relates to a rare-earth high-entropy nanocomposite insulating material system ((Y 0.25 La 0.25 Ce 0.25 Gd 0.25 The composition design of the rare earth element (γ₂O₃-MgO) follows two principles: 1. The difference in ionic radii between rare earth elements should be as small as possible to facilitate the formation of a single solid solution. 2. Each individual rare earth element should have the same sesquioxide structure. The (γ₂O₃-MgO) in this invention... 0.25 La 0.25 Ce 0.25 Gd 0.25 The average grain size of the 2O3-MgO high-entropy nanocomposite powder is less than 20 nm. It enhances phonon scattering, reduces leakage current, and improves insulation performance through the high-entropy effect in thermodynamics and lattice distortion in structure. Attached Figure Description

[0011] Figure 1 The XRD pattern of the rare earth high-entropy nanocomposite powder obtained in Example 1 of this invention; Figure 2 This is a transmission electron morphology image of the rare earth high-entropy nanocomposite powder obtained in Example 1 of the present invention. Detailed Implementation

[0012] To better explain and facilitate understanding of the present invention, the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0013] The advantages and effects of this invention are: This invention provides a method for preparing a low-leakage-current rare-earth high-entropy nanocomposite insulating material. This method uses Y(NO3)3, La(NO3)3, Ce(NO3)3, Gd(NO3)3, Mg(NO3)2, glycine, and ethylene glycol as main raw materials, and obtains the material via a glycine sol-gel combustion method. 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3-MgO high-entropy nanocomposite powder.

[0014] The features and effects of the present invention are described below with reference to specific embodiments. Example 1

[0015] Table 1 shows the insulation properties of the rare earth high-entropy nanocomposite powder obtained in Example 1 of this invention.

[0016] (1) Prepare 1 mol / LY 3+ La 3+ Ce 3+ Gd 3+ Mg 2+ A nitric acid solution containing metal cations, the five components are arranged according to the final product (Y). 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3 and MgO were mixed in a volume ratio of 15:85 to obtain a mixed solution.

[0017] (2) Add glycine to the above mixed solution according to the molar ratio of metal cation to glycine 1:0.5 to obtain a new mixed solution.

[0018] (3) Add ethylene glycol to the mixed solution in step (2) according to the molar ratio of metal cation to ethylene glycol of 1:0.01.

[0019] (4) The solution from step (3) is continuously heated and stirred at 90°C until the mixed solution forms a colorless, transparent, viscous solution. The high-entropy nanocomposite powder is ball-milled for 48-60 h. The slurry after ball milling is dried in an oven at 100-120°C for 3-5 h and then sieved through a 200-mesh sieve to obtain the high-entropy nanocomposite powder.

[0020] (5) The colorless, transparent, viscous solution was placed in a drying oven and dried at 110°C for 72 h to obtain the precursor.

[0021] (6) The precursor was calcined in a muffle furnace at 800-900℃ for 2 h to obtain the preliminary target powder, which was then ball-milled and sieved to finally obtain (Y 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3-MgO rare earth high-entropy nanocomposite powder.

[0022] Figure 1 The (Y) prepared in Example 1 0.25 La 0.25 Ce 0.25 Gd 0.25 XRD patterns of 2O3-MgO rare earth high-entropy nanocomposite powder, from Figure 1 It can be seen that the phase composition of this high-entropy nanocomposite powder consists of cubic phases Y₂O₃ and MgO, with no other impurity phases appearing, indicating that (Y₂O₃)₃ is a solid phase. 0.25 La 0.25 Ce 0.25Gd 0.25 )2O3 formed a homogeneous solid solution.

[0023] Figure 2 The (Y) prepared in Example 1 0.25 La 0.25 Ce 0.25 Gd 0.25 Microscopic morphology images of 2O3-MgO rare earth high-entropy nanocomposite powder, from Figure 2 It can be seen that the high-entropy nanocomposite powder is approximately spherical and has fine grains, about 20 nm in size.

[0024] Table 1 shows the (Y) prepared in Example 1 of this paper. 0.25 La 0.25 Ce 0.25 Gd 0.25 The insulation properties of the 2O3-MgO rare earth high-entropy nanocomposite powder were investigated. The powder was sealed within a hollow tube containing resistance wire, and its electrical performance was tested at 1050℃, 155 V, 860 W, and for 15 minutes. Table 1 shows that the leakage current of this high-entropy nanocomposite powder is only 0.056 mA, the insulation resistance is 80 MΩ after 10 minutes in the furnace, 5.5 MΩ in the humid state, 3.5 MΩ in the hot state, and the hot withstand voltage is 3040 V, indicating that this material possesses excellent electrical insulation performance.

[0025] Table 1 (Y) 0.25 La 0.25 Ce 0.25 Gd 0.25 Electrical insulation performance indicators of 2O3-MgO Operating temperature / °C Voltage / V Power / W Time / min Leakage current / mA Insulation after reflow / MΩ Moisture insulation / MΩ Hot insulation / MΩ 1050 155 860 15 0.056 80 5.5 3.5 Example 2: (1) Prepare 1 mol / LY 3+ La 3+ Ce 3+ Gd 3+ Mg 2+ A nitric acid solution containing metal cations, the five components are arranged according to the final product (Y). 0.25 La 0.25 Ce 0.25 Gd 0.25 2O3 and MgO were mixed in a volume ratio of 25:75 to obtain a mixed solution.

[0026] (2) Add glycine to the above mixed solution according to the molar ratio of metal cation to glycine 1:0.8 to obtain a new mixed solution.

[0027] (3) Add ethylene glycol to the mixed solution in step (2) according to the molar ratio of metal cation to ethylene glycol of 1:0.02.

[0028] (4) The solution from step (3) is continuously heated and stirred at 90°C until the mixed solution forms a colorless, transparent, viscous solution. The high-entropy nanocomposite powder is ball-milled for 60 h. The slurry after ball milling is dried in an oven at 120°C for 3 h and then sieved through a 200-mesh sieve to obtain the high-entropy nanocomposite powder.

[0029] (5) The colorless, transparent, viscous solution was placed in a drying oven and dried at 110°C for 72 h to obtain the precursor.

[0030] (6) The precursor was calcined in a muffle furnace at 700°C for 4 h to obtain the preliminary target powder, which was then ball-milled and sieved to finally obtain (Y 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3-MgO rare earth high-entropy nanocomposite powder.

[0031] Example 3: (1) Prepare 1 mol / LY 3+ La 3+ Ce 3+ Gd 3+ Mg 2+ A nitric acid solution containing metal cations, the five components are arranged according to the final product (Y). 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3 and MgO were mixed in a volume ratio of 35:65 to obtain a mixed solution.

[0032] (2) Add glycine to the above mixed solution according to the molar ratio of metal cation to glycine of 1:1.0 to obtain a new mixed solution.

[0033] (3) Add ethylene glycol to the mixed solution in step (2) according to the molar ratio of metal cation to ethylene glycol of 1:0.06.

[0034] (4) The solution from step (3) is continuously heated and stirred at 90°C until the mixed solution forms a colorless, transparent, viscous solution. The high-entropy nanocomposite powder is ball-milled for 60 h. The slurry after ball milling is dried in an oven at 120°C for 3 h and then sieved through a 200-mesh sieve to obtain the high-entropy nanocomposite powder.

[0035] (5) The colorless, transparent, viscous solution was placed in a drying oven and dried at 110°C for 72 h to obtain the precursor.

[0036] (6) The precursor was calcined in a muffle furnace at 400°C for 8 h to obtain the preliminary target powder, which was then ball-milled and sieved to finally obtain (Y 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3-MgO rare earth high-entropy nanocomposite powder.

[0037] Example 4: (1) Prepare 1 mol / LY 3+ La 3+ Ce 3+ Gd 3+ Mg 2+ A nitric acid solution containing metal cations, the five components are arranged according to the final product (Y). 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3 and MgO were mixed in a volume ratio of 45:55 to obtain a mixed solution.

[0038] (2) Glycine was added to the above mixed solution according to the molar ratio of metal cation to glycine of 1:0.9 to obtain a new mixed solution.

[0039] (3) Add ethylene glycol to the mixed solution in step (2) according to the molar ratio of metal cation to ethylene glycol of 1:0.07.

[0040] (4) The solution from step (3) is continuously heated and stirred at 90°C until the mixed solution forms a colorless, transparent, viscous solution. The high-entropy nanocomposite powder is ball-milled for 60 h. The slurry after ball milling is dried in an oven at 120°C for 3 h and then sieved through a 200-mesh sieve to obtain the high-entropy nanocomposite powder.

[0041] (5) The colorless, transparent, viscous solution was placed in a drying oven and dried at 110°C for 72 h to obtain the precursor.

[0042] (6) The precursor was calcined in a muffle furnace at 700°C for 4 h to obtain the preliminary target powder, which was then ball-milled and sieved to finally obtain (Y 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3-MgO rare earth high-entropy nanocomposite powder.

[0043] Example 5: (1) Prepare 1 mol / LY 3+ La 3+ Ce 3+ Gd 3+Mg 2+ A nitric acid solution containing metal cations, the five components are arranged according to the final product (Y). 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3 and MgO were mixed in a volume ratio of 50:50 to obtain a mixed solution.

[0044] (2) Add glycine to the above mixed solution according to the molar ratio of metal cation to glycine of 1:1.2 to obtain a new mixed solution.

[0045] (3) Add ethylene glycol to the mixed solution in step (2) according to the molar ratio of metal cation to ethylene glycol of 1:0.06.

[0046] (4) The solution from step (3) is continuously heated and stirred at 90°C until the mixed solution forms a colorless, transparent, viscous solution. The high-entropy nanocomposite powder is ball-milled for 60 h. The slurry after ball milling is dried in an oven at 120°C for 3 h and then sieved through a 200-mesh sieve to obtain the high-entropy nanocomposite powder.

[0047] (5) The colorless, transparent, viscous solution was placed in a drying oven and dried at 110°C for 72 h to obtain the precursor.

[0048] (6) The precursor was calcined in a muffle furnace at 500°C for 7 h to obtain the preliminary target powder, which was then ball-milled and sieved to finally obtain (Y 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3-MgO rare earth high-entropy nanocomposite powder.

[0049] It should be understood that the above description of specific embodiments of the present invention is only for illustrating the technical approach and features of the present invention, and is intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. However, the present invention is not limited to the specific embodiments described above. All changes or modifications made within the scope of the claims of the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for preparing a composite insulating material of rare-earth high-entropy nanomaterials with low leakage current, characterized in that, This composite insulating material is prepared from rare earth high-entropy nanocomposite powder using Y(NO3)3, La(NO3)3, Ce(NO3)3, Gd(NO3)3, Mg(NO3)2, glycine, and ethylene glycol as raw materials. The rare earth high-entropy nanocomposite powder contains (Y... 0.25 La 0.25 Ce 0.25 Gd 0.25 The volume ratio of O2 to MgO is 15:85, 25:75, 35:65, 45:55, and 50:

50. The specific preparation steps are as follows: S1: The formulation includes Y 3+ La 3+ Ce 3+ Gd 3+ Mg 2+ A solution of metal ion nitrates, the five are arranged according to the final product (Y). 0.25 La 0.25 Ce 0.25 Gd 0.25 The 2O3 and MgO were mixed in volume ratios of 15:85, 25:75, 35:65, 45:55, and 50:50 and stirred at room temperature. S2: Add glycine to the solution prepared in S1 according to the molar ratio of metal cation to glycine of 1:0.5~1.2 to form a mixed solution; S3: Add ethylene glycol to the mixed solution of S2 according to the molar ratio of metal cation to ethylene glycol of 1:0.01~0.07 to form a new mixed solution; S4: Heat and stir the mixed solution obtained in step S3 in a 90°C water bath until the mixed solution forms a colorless, transparent, viscous solution; S5: The colorless, transparent, viscous solution obtained in step S4 is dried at 110℃ to obtain a precursor. Finally, the precursor is calcined at 400℃~800℃ for 2~8 h to obtain a preliminary (Y) 0.25 La 0.25 Ce 0.25 Gd 0.25 )2O3-MgO high-entropy nanocomposite powder; S6: The high-entropy nanocomposite powder obtained in step S5 is further ball-milled and sieved to finally obtain the target rare-earth high-entropy insulating material.

Citation Information

Patent Citations

  • Glass or glass-eramic product with high temperature-stable, low-energy layer

    CN103443043A

  • Heat-conducting insulating organosilicon resin adhesive for LED packaging and preparation method thereof