Light emitting diode epitaxial wafer and preparation method thereof, LED

By designing a specific electron blocking layer in the epitaxial wafer of a light-emitting diode, the problem of electron-hole concentration mismatch was solved, the hole injection efficiency of the P-type semiconductor layer was improved, and the luminous efficiency of GaN-based LEDs was enhanced.

CN117352618BActive Publication Date: 2026-11-20JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311515375.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-14
Publication Date
2026-11-20
Estimated Expiration
2043-11-14

AI Technical Summary

Technical Problem

In the AlGaInN material system, the mismatch between electron and hole concentrations leads to low luminous efficiency of light-emitting diodes, and the hole injection efficiency of the P-type semiconductor layer is insufficient, resulting in severe electron leakage.

Method used

An electron blocking layer with a specific structure, including an AlN layer and multiple Mg-doped AlGaN/InGaN superlattice layers, is used to optimize electron blocking and hole injection effects by adjusting the Al and In compositions and doping concentrations, thereby improving the hole injection efficiency of the P-type semiconductor layer.

Benefits of technology

This effectively reduces electron leakage, improves hole injection efficiency, and enhances electron-hole matching in multi-quantum-well light-emitting layers, thereby improving the luminous efficiency of GaN-based LEDs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117352618B_ABST
    Figure CN117352618B_ABST
Patent Text Reader

Abstract

The application discloses a light emitting diode epitaxial wafer and a preparation method thereof and an LED, and the light emitting diode epitaxial wafer comprises a substrate, a buffer layer, an N-type semiconductor layer, a stress release layer, a multi-quantum well light emitting layer, an electron blocking layer and a P-type semiconductor layer which are sequentially arranged on the substrate; the electron blocking layer comprises an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer and a third Mg-doped AlGaN / InGaN superlattice layer which are sequentially stacked on the multi-quantum well light emitting layer. The light emitting diode epitaxial wafer provided by the application can improve the hole injection efficiency of the P-type semiconductor layer and improve the electron-hole matching degree in the multi-quantum well light emitting layer, so as to improve the light emitting efficiency of the GaN-based LED.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of optoelectronic technology, and in particular to a light-emitting diode epitaxial wafer and its preparation method, and LEDs. Background Technology

[0002] For the AlGaInN material system, electrons have higher mobility and lower effective mass compared to holes. Electrons are also easier to activate and have a higher concentration, leading to a significant mismatch between electron and hole concentrations injected into the multi-quantum-well (MWI) light-emitting layer. Quantum wells near the N-type semiconductor layer emit almost no light, while electrons can easily inject into the MWI and even penetrate the P-type semiconductor layer, causing electron leakage. Furthermore, obtaining high-quality, high-hole-concentration P-type materials for LEDs is extremely difficult because the ionization rate of Mg in the AlGaInN system is low, resulting in generally low hole concentrations in the P-type semiconductor material. In addition, the electron blocking layer, as the main functional layer of the LED, not only blocks electron injection into the P-type layer for light emission but also blocks hole injection into the MWI, further reducing the hole concentration and exacerbating the electron-hole concentration mismatch problem. Therefore, to improve the luminous efficiency of GaN-based LEDs, it is essential to improve the hole injection efficiency of the P-type material and enhance the electron-hole matching in the MWI. Summary of the Invention

[0003] The technical problem to be solved by the present invention is to provide a light-emitting diode epitaxial wafer that can improve the hole injection efficiency of the P-type semiconductor layer and improve the electron-hole matching degree in the multi-quantum-well light-emitting layer, so as to improve the luminous efficiency of GaN-based LEDs.

[0004] The technical problem to be solved by the present invention is to provide a method for preparing an epitaxial wafer of a light-emitting diode, which has a simple process and can stably produce an epitaxial wafer of a light-emitting diode with good luminous efficiency.

[0005] To solve the above-mentioned technical problems, the present invention provides a light-emitting diode epitaxial wafer, including a substrate, wherein a buffer layer, an N-type semiconductor layer, a stress relief layer, a multiple quantum well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer are sequentially disposed on the substrate.

[0006] The electron blocking layer comprises an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, which are sequentially stacked on the multi-quantum-well light-emitting layer.

[0007] In one embodiment, the Al composition of the undoped AlGaN / InGaN superlattice layer is greater than that of the first Mg-doped AlGaN / InGaN superlattice layer, which is greater than that of the second Mg-doped AlGaN / InGaN superlattice layer, which is greater than that of the third Mg-doped AlGaN / InGaN superlattice layer.

[0008] In one embodiment, the In composition of the undoped AlGaN / InGaN superlattice layer is less than the In composition of the first Mg-doped AlGaN / InGaN superlattice layer, which is less than the In composition of the second Mg-doped AlGaN / InGaN superlattice layer, which is less than the In composition of the third Mg-doped AlGaN / InGaN superlattice layer.

[0009] In one embodiment, the Mg doping concentration of the first Mg-doped AlGaN / InGaN superlattice layer is less than the Mg doping concentration of the second Mg-doped AlGaN / InGaN superlattice layer and the Mg doping concentration of the third Mg-doped AlGaN / InGaN superlattice layer.

[0010] In one embodiment, the thickness of the AlN layer is 3nm to 30nm;

[0011] The undoped AlGaN / InGaN superlattice layer comprises alternating AlGaN and InGaN layers, with the number of alternating stacking periods being 2 to 10.

[0012] The thickness of the AlGaN layer is 2nm to 8nm;

[0013] The Al composition of the AlGaN layer is 0.6 to 1.

[0014] The thickness of the InGaN layer is 2nm to 8nm;

[0015] The In composition of the InGaN layer is 0 to 0.03.

[0016] In one embodiment, the first Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a first undoped AlGaN layer and a first Mg-doped InGaN layer, with the number of alternating stacking periods being 2 to 8.

[0017] The thickness of the first undoped AlGaN layer is 2nm to 8nm;

[0018] The Al composition of the first undoped AlGaN layer is 0.4–0.8.

[0019] The thickness of the first Mg-doped InGaN layer is 2 nm to 8 nm;

[0020] The In composition of the first Mg-doped InGaN layer is 0.03 to 0.06.

[0021] The Mg doping concentration of the first Mg-doped InGaN layer is 3 × 10⁻⁶. 18 atoms / cm 3 ~8×10 18 atoms / cm 3 .

[0022] In one embodiment, the second Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a second undoped AlGaN layer and a second Mg-doped InGaN layer, with the number of alternating stacking periods being 1 to 6.

[0023] The thickness of the second undoped AlGaN layer is 2nm to 8nm;

[0024] The Al composition of the second undoped AlGaN layer is 0.2–0.6.

[0025] The thickness of the second Mg-doped InGaN layer is 2 nm to 8 nm;

[0026] The In composition of the second Mg-doped InGaN layer is 0.06–0.09.

[0027] The Mg doping concentration of the second Mg-doped InGaN layer is 8 × 10⁻⁶. 18 atoms / cm 3 ~1.2×10 19 atoms / cm 3 .

[0028] In one embodiment, the third Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a third undoped AlGaN layer and a third Mg-doped InGaN layer, with the number of alternating stacking periods being 1 to 4.

[0029] The thickness of the third undoped AlGaN layer is 2nm to 8nm;

[0030] The Al composition of the third undoped AlGaN layer is 0 to 0.4.

[0031] The thickness of the third Mg-doped InGaN layer is 2 nm to 8 nm.

[0032] The In composition of the third Mg-doped InGaN layer is 0.09–0.15.

[0033] The Mg doping concentration of the third Mg-doped InGaN layer is 1.2 × 10⁻⁶. 19 atoms / cm 3~5×10 19 atoms / cm 3 .

[0034] To address the above problems, the present invention also provides a method for fabricating a light-emitting diode epitaxial wafer, comprising the following steps:

[0035] S1. Prepare the substrate;

[0036] S2. A buffer layer, an N-type semiconductor layer, a stress relief layer, a multi-quantum-well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer are sequentially deposited on the substrate.

[0037] The electron blocking layer comprises an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, which are sequentially stacked on the multi-quantum-well light-emitting layer.

[0038] Accordingly, the present invention also provides an LED, which includes the above-described light-emitting diode epitaxial wafer.

[0039] Implementing this invention has the following beneficial effects:

[0040] The present invention provides a light-emitting diode epitaxial wafer having an electron blocking layer with a specific structure. This electron blocking layer comprises an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, sequentially stacked on a multi-quantum-well light-emitting layer. This structure design helps to reduce the effect of the electron blocking layer on hole injection into the multi-quantum-well light-emitting layer, thereby improving the hole injection efficiency of the P-type semiconductor layer. Specifically, the high bandgap AlN and AlGaN materials primarily function to block electrons and reduce their mobility, preventing electron injection into the P-type semiconductor layer and causing electron leakage. The low bandgap InGaN material can store some holes and also weakens the blocking effect on holes, thus improving the hole injection efficiency of the P-type semiconductor layer. Furthermore, Mg doping in the first, second, and third Mg-doped AlGaN / InGaN superlattice layers can increase the number of holes participating in light emission in the multi-quantum-well light-emitting layer, thereby further improving the hole injection efficiency and the electron-hole matching degree in the multi-quantum-well light-emitting layer, ultimately improving the luminous efficiency of GaN-based LEDs. Attached Figure Description

[0041] Figure 1This is a schematic diagram of the structure of the light-emitting diode epitaxial wafer provided by the present invention;

[0042] Figure 2 A flowchart illustrating the method for fabricating a light-emitting diode epitaxial wafer provided by the present invention. Detailed Implementation

[0043] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.

[0044] Unless otherwise stated or in case of contradiction, the terms or phrases used herein shall have the following meanings:

[0045] In this invention, "preferred" is merely a description of a more effective implementation method or embodiment, and should be understood as not constituting a limitation on the scope of protection of this invention.

[0046] In this invention, the technical features described in an open-ended manner include both closed-ended technical solutions composed of the listed features and open-ended technical solutions that include the listed features.

[0047] In this invention, numerical ranges are involved, and unless otherwise specified, they include the two endpoints of the numerical range.

[0048] To address the above problems, the present invention provides a light-emitting diode epitaxial wafer, such as... Figure 1 As shown, the substrate includes a substrate 100, on which a buffer layer 200, an N-type semiconductor layer 300, a stress relief layer 400, a multi-quantum-well light-emitting layer 500, an electron blocking layer 600, and a P-type semiconductor layer 700 are sequentially disposed.

[0049] The electron blocking layer 600 includes an AlN layer 610, an undoped AlGaN / InGaN superlattice layer 620, a first Mg-doped AlGaN / InGaN superlattice layer 630, a second Mg-doped AlGaN / InGaN superlattice layer 640, and a third Mg-doped AlGaN / InGaN superlattice layer 650, which are sequentially stacked on the multi-quantum-well light-emitting layer 500.

[0050] In one embodiment, the Al composition of the undoped AlGaN / InGaN superlattice layer is greater than that of the first Mg-doped AlGaN / InGaN superlattice layer, which in turn is greater than that of the second Mg-doped AlGaN / InGaN superlattice layer, which is greater than that of the third Mg-doped AlGaN / InGaN superlattice layer. In another embodiment, the In composition of the undoped AlGaN / InGaN superlattice layer is less than that of the first Mg-doped AlGaN / InGaN superlattice layer, which is less than that of the second Mg-doped AlGaN / InGaN superlattice layer, which is less than that of the third Mg-doped AlGaN / InGaN superlattice layer. In yet another embodiment, the In composition of the undoped AlGaN / InGaN superlattice layer is less than that of the first Mg-doped AlGaN / InGaN superlattice layer, which is less than that of the second Mg-doped AlGaN / InGaN superlattice layer, which is less than that of the third Mg-doped AlGaN / InGaN superlattice layer.

[0051] It should be noted that Al atoms are relatively small, and when they react with NH3 gas to form Al-N, they have a wide band gap, resulting in the strongest blocking effect on electrons and holes. Similarly, In atoms are relatively large, and when they react with NH3 gas to form In-N, they have a small band gap, resulting in the weakest effect on electrons and holes. The main function of the electron blocking layer is to prevent electrons from entering the P-type semiconductor layer and causing electron leakage, but it inevitably also blocks hole injection into the active region. Therefore, the material near the multiple quantum wells should be designed with a wide band gap to enhance the electron blocking effect, while the material near the P-type semiconductor layer should be designed with a small band gap to reduce the hole injection blocking effect. Therefore, the Mg-doped AlGaN / InGaN superlattice layer of this invention is designed with a structure of decreasing Al composition and increasing In composition. At the same time, since In atoms are relatively large, the higher the In composition of InGaN material, the more favorable it is for Mg doping to be incorporated into the lattice. Increasing Mg doping can enhance the hole injection effect of the P-type material.

[0052] The specific structure of the five sublayers of the electron blocking layer 600 is as follows:

[0053] In one embodiment, the thickness of the AlN layer 610 is 3nm to 30nm; exemplary thicknesses of the AlN layer 610 are 6nm, 9nm, 12nm, 15nm, 18nm, 21nm, 24nm, and 27nm, but are not limited thereto. The AlN layer 610 can block electrons and reduce electron mobility, preventing electrons from being injected into the P-type semiconductor layer and causing electron leakage.

[0054] In one embodiment, the undoped AlGaN / InGaN superlattice layer 620 comprises alternating layers of AlGaN and InGaN, with 2 to 10 alternating periods; preferably, 4 to 8 alternating periods. In one embodiment, the thickness of the AlGaN layer is 2 nm to 8 nm; exemplary thicknesses of the AlGaN layer are 3 nm, 4 nm, 5 nm, 6 nm, and 7 nm, but are not limited thereto. In one embodiment, the Al composition of the AlGaN layer is 0.6 to 1; preferably, the Al composition of the AlGaN layer is 0.8 to 1. In one embodiment, the thickness of the InGaN layer is 2 nm to 8 nm; exemplary thicknesses of the InGaN layer are 3 nm, 4 nm, 5 nm, 6 nm, and 7 nm, but are not limited thereto. In one embodiment, the In composition of the InGaN layer is 0 to 0.03; preferably, the In composition of the InGaN layer is 0.01 to 0.02. The AlGaN layer in the undoped AlGaN / InGaN superlattice layer 620 acts as a barrier to electrons and reduces their mobility, preventing electrons from being injected into the P-type semiconductor layer and causing electron leakage. The InGaN layer can store some holes and also weaken the blocking effect on holes, thereby improving the hole injection efficiency of the P-type semiconductor layer.

[0055] In one embodiment, the first Mg-doped AlGaN / InGaN superlattice layer 630 comprises alternating layers of a first undoped AlGaN layer and a first Mg-doped InGaN layer, with 2 to 8 alternating periods; preferably, the number of alternating periods is 3 to 7. In one embodiment, the thickness of the first undoped AlGaN layer is 2 nm to 8 nm; exemplary thicknesses of the first undoped AlGaN layer are 3 nm, 4 nm, 5 nm, 6 nm, and 7 nm, but are not limited thereto. In one embodiment, the Al composition of the first undoped AlGaN layer is 0.4 to 0.8; preferably, the Al composition of the first undoped AlGaN layer is 0.5 to 0.7. In one embodiment, the thickness of the first Mg-doped InGaN layer is 2 nm to 8 nm; exemplary thicknesses of the first Mg-doped InGaN layer are 3 nm, 4 nm, 5 nm, 6 nm, and 7 nm, but are not limited thereto. In one embodiment, the In composition of the first Mg-doped InGaN layer is 0.03–0.06; preferably, the In composition of the first Mg-doped InGaN layer is 0.04–0.05. In one embodiment, the Mg doping concentration of the first Mg-doped InGaN layer is 3 × 10⁻⁶. 18 atoms / cm 3 ~8×10 18 atoms / cm 3Preferably, the Mg doping concentration of the first Mg-doped InGaN layer is 4 × 10⁻⁶. 18 atoms / cm 3 ~7×10 18 atoms / cm 3 The AlGaN layer in the first Mg-doped AlGaN / InGaN superlattice layer 630 acts as a barrier to electrons and reduces their mobility, preventing electrons from being injected into the P-type semiconductor layer and causing electron leakage. The InGaN layer can store some holes and also weakens the blocking effect on holes, thereby improving the hole injection efficiency of the P-type semiconductor layer. Furthermore, the Mg doping in the first Mg-doped AlGaN / InGaN superlattice layer 630 can increase the number of holes participating in light emission in the multi-quantum-well light-emitting layer, further improving the hole injection efficiency and the electron-hole matching degree in the multi-quantum-well light-emitting layer, ultimately improving the luminous efficiency of GaN-based LEDs.

[0056] In one embodiment, the second Mg-doped AlGaN / InGaN superlattice layer 640 comprises alternating layers of a second undoped AlGaN layer and a second Mg-doped InGaN layer, with 1 to 6 alternating periods; preferably, the number of alternating periods is 2 to 5. In one embodiment, the thickness of the second undoped AlGaN layer is 2 nm to 8 nm; exemplary thicknesses of the second undoped AlGaN layer are 3 nm, 4 nm, 5 nm, 6 nm, and 7 nm, but are not limited thereto. In one embodiment, the Al composition of the second undoped AlGaN layer is 0.2 to 0.6; preferably, the Al composition of the second undoped AlGaN layer is 0.3 to 0.5. In one embodiment, the thickness of the second Mg-doped InGaN layer is 2 nm to 8 nm; exemplary thicknesses of the second Mg-doped InGaN layer are 3 nm, 4 nm, 5 nm, 6 nm, and 7 nm, but are not limited thereto. In one embodiment, the In composition of the second Mg-doped InGaN layer is 0.06–0.09; preferably, the In composition of the second Mg-doped InGaN layer is 0.07–0.08. In one embodiment, the Mg doping concentration of the second Mg-doped InGaN layer is 8 × 10⁻⁶. 18 atoms / cm 3 ~1.2×10 19 atoms / cm 3 Preferably, the Mg doping concentration of the second Mg-doped InGaN layer is 9 × 10⁻⁶. 18 atoms / cm 3 ~1×10 19 atoms / cm 3In the second Mg-doped AlGaN / InGaN superlattice layer 640, the AlGaN layer acts as a barrier to electrons and reduces their mobility, preventing electron injection into the P-type semiconductor layer and thus avoiding electron leakage. The InGaN layer can store some holes and also weakens the blocking effect on holes, thereby improving the hole injection efficiency of the P-type semiconductor layer. Furthermore, the Mg doping in the second Mg-doped AlGaN / InGaN superlattice layer 640 can increase the number of holes participating in light emission in the multi-quantum-well light-emitting layer, further improving the hole injection efficiency and the electron-hole matching degree in the multi-quantum-well light-emitting layer, ultimately improving the luminous efficiency of GaN-based LEDs.

[0057] In one embodiment, the third Mg-doped AlGaN / InGaN superlattice layer 650 comprises alternating layers of a third undoped AlGaN layer and a third Mg-doped InGaN layer, with 1 to 4 alternating stacking periods; preferably, the number of alternating stacking periods is 2 to 3. In one embodiment, the thickness of the third undoped AlGaN layer is 2 nm to 8 nm; exemplary thicknesses of the third undoped AlGaN layer are 3 nm, 4 nm, 5 nm, 6 nm, and 7 nm, but are not limited thereto. In one embodiment, the Al composition of the third undoped AlGaN layer is 0 to 0.4; preferably, the Al composition of the third undoped AlGaN layer is 0.1 to 0.3. In one embodiment, the thickness of the third Mg-doped InGaN layer is 2 nm to 8 nm; exemplary thicknesses of the third Mg-doped InGaN layer are 3 nm, 4 nm, 5 nm, 6 nm, and 7 nm, but are not limited thereto. In one embodiment, the In composition of the third Mg-doped InGaN layer is 0.09–0.15; preferably, the In composition of the third Mg-doped InGaN layer is 0.1–0.14. In one embodiment, the Mg doping concentration of the third Mg-doped InGaN layer is 1.2 × 10⁻⁶. 19 atoms / cm 3 ~5×10 19 atoms / cm 3 Preferably, the Mg doping concentration of the third Mg-doped InGaN layer is 2 × 10⁻⁶. 19 atoms / cm 3 ~4×10 19 atoms / cm 3The AlGaN layer in the third Mg-doped AlGaN / InGaN superlattice layer 650 acts as a barrier to electrons and reduces their mobility, preventing electron injection into the P-type semiconductor layer and causing electron leakage. The InGaN layer can store some holes and also weakens the blocking effect on holes, thereby improving the hole injection efficiency of the P-type semiconductor layer. Furthermore, the Mg doping in the third Mg-doped AlGaN / InGaN superlattice layer 650 can increase the number of holes participating in light emission in the multi-quantum-well light-emitting layer, further improving the hole injection efficiency and the electron-hole matching degree in the multi-quantum-well light-emitting layer, ultimately improving the luminous efficiency of GaN-based LEDs.

[0058] Based on the above material and structural designs, the LED epitaxial wafer prepared using this invention can reduce the effect of the electron blocking layer on hole injection into the multi-quantum-well light-emitting layer, thereby improving the hole injection efficiency of the P-type semiconductor layer. Specifically, the high-bandgap AlN and AlGaN materials primarily function to block electrons and reduce their mobility, preventing electron injection into the P-type semiconductor layer and causing electron leakage. The low-bandgap InGaN material can store some holes and also weaken the blocking effect on holes, thus improving the hole injection efficiency of the P-type semiconductor layer. Furthermore, the Mg doping in the first, second, and third Mg-doped AlGaN / InGaN superlattice layers increases the number of holes participating in light emission in the multi-quantum-well light-emitting layer, further improving the hole injection efficiency and electron-hole matching in the multi-quantum-well light-emitting layer, ultimately improving the luminous efficiency of GaN-based LEDs.

[0059] Accordingly, the present invention provides a method for fabricating a light-emitting diode epitaxial wafer, such as... Figure 2 As shown, it includes the following steps:

[0060] S1. Prepare substrate 100;

[0061] S2. A buffer layer 200, an N-type semiconductor layer 300, a stress relief layer 400, a multi-quantum-well light-emitting layer 500, an electron blocking layer 600, and a P-type semiconductor layer 700 are sequentially deposited on the substrate 100.

[0062] The electron blocking layer 600 includes an AlN layer 610, an undoped AlGaN / InGaN superlattice layer 620, a first Mg-doped AlGaN / InGaN superlattice layer 630, a second Mg-doped AlGaN / InGaN superlattice layer 640, and a third Mg-doped AlGaN / InGaN superlattice layer 650, which are sequentially stacked on the multi-quantum-well light-emitting layer 500.

[0063] In one embodiment, the AlN layer 610 is prepared by the following method:

[0064] The temperature of the reaction chamber was controlled at 900℃~1050℃, and the pressure was controlled at 20 torr~300 torr. An N source and an Al source were introduced to grow the AlN layer 610.

[0065] In one embodiment, the undoped AlGaN / InGaN superlattice layer 620 is prepared by the following method:

[0066] The temperature of the reaction chamber was controlled at 900℃~1050℃, the pressure was controlled at 20torr~300torr, and N source, Ga source and In source were introduced to grow InGaN layer;

[0067] The temperature of the reaction chamber was controlled at 900℃~1050℃, the pressure was controlled at 20torr~300torr, and N source, Ga source and Al source were introduced to grow AlGaN layer;

[0068] The InGaN layer and the AlGaN layer are grown alternately to obtain the undoped AlGaN / InGaN superlattice layer 620.

[0069] In one embodiment, the first Mg-doped AlGaN / InGaN superlattice layer 630 is prepared by the following method:

[0070] The temperature of the reaction chamber was controlled at 900℃~1050℃, the pressure was controlled at 20 torr~300 torr, and N source, Ga source, In source and Mg source were introduced to grow the first Mg-doped InGaN layer.

[0071] The temperature of the reaction chamber was controlled at 900℃~1050℃, the pressure was controlled at 20torr~300torr, and N source, Ga source and Al source were introduced to grow the first undoped AlGaN layer.

[0072] The first Mg-doped InGaN layer and the first undoped AlGaN layer are alternately grown to obtain the first Mg-doped AlGaN / InGaN superlattice layer 630.

[0073] In one embodiment, the second Mg-doped AlGaN / InGaN superlattice layer 640 is prepared by the following method:

[0074] The temperature of the reaction chamber was controlled at 900℃~1050℃, the pressure was controlled at 20 torr~300 torr, and N source, Ga source, In source and Mg source were introduced to grow the second Mg-doped InGaN layer.

[0075] The temperature of the reaction chamber was controlled at 900℃~1050℃, the pressure was controlled at 20torr~300torr, and N source, Ga source and Al source were introduced to grow the second undoped AlGaN layer.

[0076] The second Mg-doped InGaN layer and the second undoped AlGaN layer are alternately grown to obtain the second Mg-doped AlGaN / InGaN superlattice layer 640.

[0077] In one embodiment, the third Mg-doped AlGaN / InGaN superlattice layer 650 is prepared by the following method:

[0078] The temperature of the reaction chamber was controlled at 900℃~1050℃, the pressure was controlled at 20 torr~300 torr, and N source, Ga source, In source and Mg source were introduced to grow the third Mg-doped InGaN layer.

[0079] The temperature of the reaction chamber was controlled at 900℃~1050℃, the pressure was controlled at 20torr~300torr, and N source, Ga source and Al source were introduced to grow the third undoped AlGaN layer.

[0080] The third Mg-doped InGaN layer and the third undoped AlGaN layer are alternately grown to obtain the third Mg-doped AlGaN / InGaN superlattice layer 650.

[0081] Accordingly, the present invention also provides an LED comprising the aforementioned light-emitting diode epitaxial wafer. The photoelectric efficiency of the LED is effectively improved, and other electrical properties are also excellent.

[0082] The present invention is further illustrated below with specific embodiments:

[0083] Example 1

[0084] This embodiment provides a light-emitting diode epitaxial wafer, including a substrate, on which a buffer layer, an N-type semiconductor layer, a stress relief layer, a multiple quantum well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer are sequentially disposed;

[0085] The electron blocking layer comprises an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, which are sequentially stacked on the multi-quantum-well light-emitting layer.

[0086] The thickness of the AlN layer is 15 nm;

[0087] The undoped AlGaN / InGaN superlattice layer comprises alternating AlGaN and InGaN layers with a period of 6 alternating layers; the AlGaN layer has a thickness of 5 nm and an Al composition of 0.85; the InGaN layer has a thickness of 5 nm and an In composition of 0.015.

[0088] The first Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a first undoped AlGaN layer and a first Mg-doped InGaN layer, with a period of 5 alternations; the first undoped AlGaN layer has a thickness of 5 nm and an Al composition of 0.6; the first Mg-doped InGaN layer has a thickness of 5 nm, an In composition of 0.045, and a Mg doping concentration of 5 × 10⁻⁶. 18 atoms / cm 3 .

[0089] The second Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of undoped AlGaN and Mg-doped InGaN, with a period of 4 alternations. The thickness of the second undoped AlGaN layer is 5 nm, and the Al composition is 0.4. The thickness of the second Mg-doped InGaN layer is 5 nm, the In composition is 0.075, and the Mg doping concentration is 1 × 10⁻⁶. 19 atoms / cm 3 .

[0090] The third Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a third undoped AlGaN layer and a third Mg-doped InGaN layer, with an alternating stacking period of 2. The thickness of the third undoped AlGaN layer is 5 nm, and the Al composition is 0.2. The thickness of the third Mg-doped InGaN layer is 5 nm, the In composition is 0.12, and the Mg doping concentration is 3 × 10⁻⁶. 19 atoms / cm 3 .

[0091] Example 2

[0092] This embodiment provides a light-emitting diode epitaxial wafer, including a substrate, on which a buffer layer, an N-type semiconductor layer, a stress relief layer, a multiple quantum well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer are sequentially disposed;

[0093] The electron blocking layer comprises an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, which are sequentially stacked on the multi-quantum-well light-emitting layer.

[0094] The thickness of the AlN layer is 5 nm;

[0095] The undoped AlGaN / InGaN superlattice layer comprises alternating AlGaN and InGaN layers, with a period of 4 alternating layers; the AlGaN layer has a thickness of 2 nm and an Al composition of 0.6; the InGaN layer has a thickness of 2 nm and an In composition of 0.01.

[0096] The first Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a first undoped AlGaN layer and a first Mg-doped InGaN layer, with a period of 3 alternating layers; the thickness of the first undoped AlGaN layer is 2 nm, and the Al composition is 0.4; the thickness of the first Mg-doped InGaN layer is 2 nm, the In composition is 0.03, and the Mg doping concentration is 3 × 10⁻⁶. 18 atoms / cm 3 .

[0097] The second Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of undoped AlGaN and Mg-doped InGaN, with a period of 2 alternations. The thickness of the second undoped AlGaN layer is 2 nm, and the Al composition is 0.2%. The thickness of the second Mg-doped InGaN layer is 2 nm, the In composition is 0.06, and the Mg doping concentration is 8 × 10⁻⁶. 18 atoms / cm 3 .

[0098] The third Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a third undoped AlGaN layer and a third Mg-doped InGaN layer, with an alternating stacking period of 1. The thickness of the third undoped AlGaN layer is 2 nm, and the Al composition is 0.1. The thickness of the third Mg-doped InGaN layer is 2 nm, the In composition is 0.09, and the Mg doping concentration is 1.2 × 10⁻⁶. 19 atoms / cm 3 .

[0099] Example 3

[0100] This embodiment provides a light-emitting diode epitaxial wafer, including a substrate, on which a buffer layer, an N-type semiconductor layer, a stress relief layer, a multiple quantum well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer are sequentially disposed;

[0101] The electron blocking layer comprises an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, which are sequentially stacked on the multi-quantum-well light-emitting layer.

[0102] The thickness of the AlN layer is 30 nm;

[0103] The undoped AlGaN / InGaN superlattice layer comprises alternating AlGaN and InGaN layers with 10 alternating stacking periods; the AlGaN layer has a thickness of 8 nm and an Al composition of 0.95; the InGaN layer has a thickness of 8 nm and an In composition of 0.03.

[0104] The first Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a first undoped AlGaN layer and a first Mg-doped InGaN layer, with an alternating stacking period of 8. The thickness of the first undoped AlGaN layer is 8 nm, and the Al composition is 0.8. The thickness of the first Mg-doped InGaN layer is 8 nm, the In composition is 0.06, and the Mg doping concentration is 8 × 10⁻⁶. 18 atoms / cm 3 .

[0105] The second Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of undoped AlGaN and Mg-doped InGaN, with a period of 6 alternations. The thickness of the second undoped AlGaN layer is 8 nm, and the Al composition is 0.6. The thickness of the second Mg-doped InGaN layer is 8 nm, the In composition is 0.09, and the Mg doping concentration is 1.2 × 10⁻⁶. 19 atoms / cm 3 .

[0106] The third Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a third undoped AlGaN layer and a third Mg-doped InGaN layer, with an alternating stacking period of 4. The thickness of the third undoped AlGaN layer is 8 nm, and the Al composition is 0.4. The thickness of the third Mg-doped InGaN layer is 8 nm, the In composition is 0.15, and the Mg doping concentration is 5 × 10⁻⁶. 19 atoms / cm 3 .

[0107] Comparative Example 1

[0108] This comparative embodiment provides a light-emitting diode epitaxial wafer, including a substrate. The substrate is sequentially provided with a buffer layer, an N-type semiconductor layer, a stress relief layer, a multi-quantum-well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer. The electron blocking layer includes an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, which are sequentially stacked on the multi-quantum-well light-emitting layer.

[0109] The Al composition of the undoped AlGaN / InGaN superlattice layer is less than that of the first Mg-doped AlGaN / InGaN superlattice layer, which is less than that of the second Mg-doped AlGaN / InGaN superlattice layer, which is less than that of the third Mg-doped AlGaN / InGaN superlattice layer.

[0110] Comparative Example 2

[0111] This comparative embodiment provides a light-emitting diode epitaxial wafer, including a substrate. The substrate is sequentially provided with a buffer layer, an N-type semiconductor layer, a stress relief layer, a multi-quantum-well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer. The electron blocking layer includes an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, which are sequentially stacked on the multi-quantum-well light-emitting layer.

[0112] The In composition of the undoped AlGaN / InGaN superlattice layer is greater than that of the first Mg-doped AlGaN / InGaN superlattice layer, which is greater than that of the second Mg-doped AlGaN / InGaN superlattice layer, which is greater than that of the third Mg-doped AlGaN / InGaN superlattice layer.

[0113] Comparative Example 3

[0114] This comparative embodiment provides a light-emitting diode epitaxial wafer, including a substrate. The substrate is sequentially provided with a buffer layer, an N-type semiconductor layer, a stress relief layer, a multi-quantum-well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer. The electron blocking layer includes an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, which are sequentially stacked on the multi-quantum-well light-emitting layer.

[0115] The Mg doping concentration of the first Mg-doped AlGaN / InGaN superlattice layer is greater than that of the second Mg-doped AlGaN / InGaN superlattice layer, which is greater than that of the third Mg-doped AlGaN / InGaN superlattice layer.

[0116] Comparative Example 1

[0117] This comparative example provides a light-emitting diode epitaxial wafer, including a substrate, on which a buffer layer, an N-type semiconductor layer, a stress relief layer, a multi-quantum-well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer are sequentially disposed, wherein the electron blocking layer is an AlGaInN layer.

[0118] The epitaxial wafers of light-emitting diodes prepared in Examples 1 to 3, Comparative Examples 1 to 3, and Comparative Example 1 were fabricated into 10mil×24mil chips using the same chip process conditions. 300 LED chips were randomly selected from each example and tested at 120mA / 60mA current. With Comparative Example 1 as a reference, the luminous efficiency improvement rate of each example and comparative example was calculated. The specific test results are shown in Table 1.

[0119] Table 1. Performance test results of LEDs prepared in Examples 1-3, Comparative Examples 1-3, and Comparative Example 1

[0120]

[0121] As shown in the above results, the light-emitting diode epitaxial wafer provided by this invention has an electron blocking layer with a specific structure. This electron blocking layer comprises an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, sequentially stacked on the multi-quantum-well light-emitting layer. This structure design helps to reduce the effect of the electron blocking layer on hole injection into the multi-quantum-well light-emitting layer, thereby improving the hole injection efficiency of the P-type semiconductor layer. Specifically, the high bandgap AlN and AlGaN materials mainly function to block electrons and reduce their mobility, preventing electron injection into the P-type semiconductor layer and causing electron leakage. The low bandgap InGaN material can store some holes and also weaken the blocking effect on holes, thus improving the hole injection efficiency of the P-type semiconductor layer. Furthermore, Mg doping in the first, second, and third Mg-doped AlGaN / InGaN superlattice layers can increase the number of holes participating in light emission in the multi-quantum-well light-emitting layer, thereby further improving the hole injection efficiency and the electron-hole matching degree in the multi-quantum-well light-emitting layer, ultimately improving the luminous efficiency of GaN-based LEDs.

[0122] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A light-emitting diode epitaxial wafer, characterized in that, The substrate includes a buffer layer, an N-type semiconductor layer, a stress relief layer, a multi-quantum-well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer, which are sequentially disposed on the substrate. The electron blocking layer comprises an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, which are sequentially stacked on the multi-quantum-well light-emitting layer. The Al composition of the undoped AlGaN / InGaN superlattice layer is greater than that of the first Mg-doped AlGaN / InGaN superlattice layer, which is greater than that of the second Mg-doped AlGaN / InGaN superlattice layer, which is greater than that of the third Mg-doped AlGaN / InGaN superlattice layer. The In composition of the undoped AlGaN / InGaN superlattice layer is < the In composition of the first Mg-doped AlGaN / InGaN superlattice layer < the In composition of the second Mg-doped AlGaN / InGaN superlattice layer < the In composition of the third Mg-doped AlGaN / InGaN superlattice layer. The Mg doping concentration of the first Mg-doped AlGaN / InGaN superlattice layer is < the Mg doping concentration of the second Mg-doped AlGaN / InGaN superlattice layer is < the Mg doping concentration of the third Mg-doped AlGaN / InGaN superlattice layer.

2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The thickness of the AlN layer is 3nm~30nm; The undoped AlGaN / InGaN superlattice layer comprises alternating AlGaN and InGaN layers, with the number of alternating stacking periods being 2 to 10. The thickness of the AlGaN layer is 2nm~8nm; The Al composition of the AlGaN layer is 0.6~1; The thickness of the InGaN layer is 2nm~8nm; The In composition of the InGaN layer is 0~0.

03.

3. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The first Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a first undoped AlGaN layer and a first Mg-doped InGaN layer, with the number of alternating stacking periods being 2 to 8. The thickness of the first undoped AlGaN layer is 2nm~8nm; The Al composition of the first undoped AlGaN layer is 0.4~0.8; The thickness of the first Mg-doped InGaN layer is 2 nm to 8 nm; The In composition of the first Mg-doped InGaN layer is 0.03~0.06; The Mg doping concentration of the first Mg-doped InGaN layer is 3 × 10⁻⁶. 18 atoms / cm 3 ~8×10 18 atoms / cm 3 .

4. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The second Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of second undoped AlGaN and second Mg-doped InGaN, with the number of alternating stacking periods being 1 to 6. The thickness of the second undoped AlGaN layer is 2nm~8nm; The Al composition of the second undoped AlGaN layer is 0.2~0.6; The thickness of the second Mg-doped InGaN layer is 2 nm to 8 nm; The In composition of the second Mg-doped InGaN layer is 0.06~0.09; The Mg doping concentration of the second Mg-doped InGaN layer is 8 × 10⁻⁶. 18 atoms / cm 3 ~1.2×10 19 atoms / cm 3 .

5. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The third Mg-doped AlGaN / InGaN superlattice layer comprises alternating layers of a third undoped AlGaN layer and a third Mg-doped InGaN layer, with the number of alternating stacking periods being 1 to 4. The thickness of the third undoped AlGaN layer is 2nm~8nm; The Al composition of the third undoped AlGaN layer is 0~0.4; The thickness of the third Mg-doped InGaN layer is 2 nm to 8 nm; The In composition of the third Mg-doped InGaN layer is 0.09~0.15; The Mg doping concentration of the third Mg-doped InGaN layer is 1.2 × 10⁻⁶. 19 atoms / cm 3 ~5×10 19 atoms / cm 3 .

6. A method for fabricating a light-emitting diode epitaxial wafer as described in any one of claims 1 to 5, characterized in that, Includes the following steps: S1. Prepare the substrate; S2. A buffer layer, an N-type semiconductor layer, a stress relief layer, a multi-quantum-well light-emitting layer, an electron blocking layer, and a P-type semiconductor layer are sequentially deposited on the substrate. The electron blocking layer comprises an AlN layer, an undoped AlGaN / InGaN superlattice layer, a first Mg-doped AlGaN / InGaN superlattice layer, a second Mg-doped AlGaN / InGaN superlattice layer, and a third Mg-doped AlGaN / InGaN superlattice layer, which are sequentially stacked on the multi-quantum-well light-emitting layer.

7. An LED, characterized in that, The LED includes a light-emitting diode epitaxial wafer as described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Preparation method for semiconductor light-emitting device

    CN104795472A

  • Light-emitting diode chip manufacturing method and light-emitting diode chip

    JP2018029110A