High durability, high conductivity composite proton exchange membrane, and preparation method and application thereof

By blending perfluorosulfonic acid resin with manganese genistein complex, a composite proton exchange membrane with high durability and high conductivity is formed, which solves the problem of insufficient durability and conductivity of perfluorosulfonic acid proton exchange membranes in fuel cells, and realizes stable operation and performance improvement of fuel cells.

CN117352795BActive Publication Date: 2026-11-24SHANGHAI INST OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311397254.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-26
Publication Date
2026-11-24
Estimated Expiration
2043-10-26

AI Technical Summary

Technical Problem

Existing perfluorosulfonic acid proton exchange membranes suffer from severe chemical degradation during fuel cell operation, resulting in insufficient durability and conductivity, which affects their application performance.

Method used

A composite proton exchange membrane with high durability and high conductivity is formed by blending perfluorosulfonic acid resin with manganese genistein complex, taking advantage of the antioxidant effect of genistein and the ability of manganese ions to decompose H₂O₂.

Benefits of technology

It improves the chemical durability and electrical conductivity of the proton exchange membrane, enhances the operational stability and performance of the fuel cell, and the preparation method is simple and easy to industrialize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117352795B_ABST
    Figure CN117352795B_ABST
Patent Text Reader

Abstract

This invention relates to a high-durability, high-conductivity composite proton exchange membrane, its preparation method, and its application, belonging to the field of proton exchange membrane fuel cell technology. By blending perfluorosulfonic acid resin with a manganese genistein complex to form a membrane, where genistein acts as a free radical scavenger and manganese as a hydrogen peroxide decomposition catalyst, hydroxyl radicals and hydrogen peroxide generated during fuel cell operation can be effectively removed, significantly mitigating the damage to the membrane caused by the harsh operating environment of the fuel cell. Compared with existing technologies, this invention solves the problems of poor chemical durability and low conductivity of perfluorosulfonic acid proton exchange membranes used in fuel cells, and has promising application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of proton exchange membrane fuel cell technology, and in particular relates to a high-durability, high-conductivity composite proton exchange membrane, its preparation method, and its application. Background Technology

[0002] In today's society, with increasing energy shortages and environmental pollution, renewable and clean energy sources such as hydrogen energy have become a focus of attention. Among these, the proton exchange membrane fuel cell (PEMFC) is an energy conversion device that directly converts the chemical energy of hydrogen into electrical energy. PEMFCs offer advantages such as rapid start-up, moderate operating temperature, stable output power, convenient stack assembly and maintenance, long lifespan, and zero pollution, making them particularly promising for applications in the transportation sector and considered the absolute mainstream of future fuel cell development. PEMFCs use hydrogen (H2) as fuel gas, a water-based acidic polymer (perfluorosulfonic acid polymer) as the electrolyte, and platinum (carbon-supported platinum) as the catalyst, achieving an energy conversion efficiency of up to 60%. Despite the numerous advantages of perfluorosulfonic acid proton exchange membranes, significant chemical degradation occurs during fuel cell operation due to the generation of numerous free radicals. Therefore, improving perfluorosulfonic acid proton exchange membranes to enhance their chemical durability and proton conductivity is of great importance.

[0003] Chinese patent CN114388857A discloses a method for preparing a high-durability myricetin-chelated cerium ion composite proton exchange membrane, in which the myricetin-cerium complex is added to a polymer resin solution to obtain the proton exchange membrane. However, the myricetin-cerium complex, as an additive, only improves the chemical durability of the proton exchange membrane and does not effectively improve its conductivity. Therefore, further modification of the perfluorosulfonic acid proton exchange membrane is still needed to improve its application performance in fuel cells. Summary of the Invention

[0004] The purpose of this invention is to provide a high-durability, high-conductivity composite proton exchange membrane, its preparation method, and its application in order to improve the chemical durability and conductivity of proton exchange membranes.

[0005] The objective of this invention can be achieved through the following technical solutions:

[0006] A composite proton exchange membrane includes a perfluorosulfonic acid resin and a manganese genistein complex dispersed in the perfluorosulfonic acid resin, wherein the mass ratio of the manganese genistein complex to the perfluorosulfonic acid resin is 1:(20-100), preferably 1:(32-80), and more preferably 1:(40-80).

[0007] Furthermore, the thickness of the composite proton exchange membrane is 8-30 μm, preferably 10-20 μm, and more preferably 15 μm.

[0008] This invention also provides a method for preparing a composite proton exchange membrane, comprising the following steps:

[0009] S1: Preparation of perfluorosulfonic acid solution: Disperse perfluorosulfonic acid resin in a mixed solvent and stir to obtain perfluorosulfonic acid solution;

[0010] S2: Preparation of genistein manganese complex: Genistein and manganese salt were mixed, heated, centrifuged and dried to obtain genistein manganese complex;

[0011] S3: Preparation of composite proton exchange membrane: The manganese genistein complex obtained in step S2 is added to the perfluorosulfonic acid solution obtained in step S1, and the mixture is stirred, sonicated, and cured to obtain the composite proton exchange membrane.

[0012] Further, in step S1, the mixed solvent comprises isopropanol, water, and N,N-dimethylaniline. Even further, the mass ratio of isopropanol, water, and N,N-dimethylaniline is 5:5:(0.8-1.2), preferably 5:5:1.

[0013] Further, in step S1, the perfluorosulfonic acid resin accounts for 0.5-30% of the total mass of the perfluorosulfonic acid solution, preferably 15-30%, and more preferably 26.7%.

[0014] Furthermore, in step S1, the stirring time is 6-24 hours, preferably 12-24 hours.

[0015] Further, in step S1, the stirring speed is 300-500 rpm, preferably 350-450 rpm, and more preferably 450 rpm.

[0016] Furthermore, in step S2, the manganese salt is required to be soluble in water and capable of generating manganese ions.

[0017] Furthermore, the manganese salt includes one or more of manganese nitrate tetrahydrate, manganese acetate tetrahydrate, and manganese sulfate tetrahydrate, preferably manganese nitrate tetrahydrate.

[0018] Further, in step S2, the molar ratio of genistein to manganese salt is (1-2):1, preferably 1:1. Even further, genistein and manganese salt are mixed in a 50wt% ethanol solution.

[0019] Furthermore, in step S2, the heating temperature is 60-80℃, preferably 60-70℃.

[0020] Furthermore, in step S2, the heating time is 6-12 hours, preferably 9-12 hours.

[0021] Furthermore, in step S2, the centrifugation speed is 8000-12000 rpm, preferably 8000-10000 rpm.

[0022] Further, in step S2, the centrifugation time is 10-30 min, preferably 10-20 min.

[0023] Furthermore, in step S2, the drying temperature is 60-80℃, preferably 60-70℃.

[0024] Furthermore, in step S2, the drying time is 1-3 hours, preferably 2 hours.

[0025] Furthermore, in step S3, the stirring time is 8-16 hours, preferably 12 hours.

[0026] Furthermore, in step S3, the stirring speed is 300-500 rpm, preferably 400 rpm.

[0027] Furthermore, in step S3, the ultrasound duration is 20-60 minutes, preferably 30-60 minutes.

[0028] Furthermore, in step S3, the specific methods for curing include scraping, drying, and annealing.

[0029] Furthermore, the coating speed of the scraping process is 100-200 mm / s, preferably 100-160 mm / s.

[0030] Furthermore, the drying temperature is 60-100℃, preferably 70-100℃.

[0031] Furthermore, the drying time is 1-2 hours.

[0032] Furthermore, the annealing temperature is 120-160℃, preferably 120-140℃.

[0033] Furthermore, the annealing time is 1-2 hours.

[0034] The present invention also provides an application of a composite proton exchange membrane in the fabrication of a fuel cell.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) The present invention provides a composite proton exchange membrane with high durability and high conductivity. The composite proton exchange membrane is prepared by simply blending perfluorosulfonic acid resin with manganese genistein complex, and makes full use of the antioxidant effects of the two to improve the chemical durability and conductivity of the proton exchange membrane.

[0037] (2) The genistein manganese complex in the composite proton exchange membrane of this invention has good free radical scavenging properties. Genistein is derived from natural plants, has antioxidant effects, and is almost insoluble in water, so it is not easy to migrate out of the membrane and cause damage. Metal Mn ions have the ability to decompose H2O2. The two work together to improve the chemical durability of the fuel cell proton exchange membrane.

[0038] (3) The manganese genistein complex in this invention has good chemical stability, and appropriate doping is beneficial to the formation of proton transport channels with low steric hindrance, thereby improving the proton conductivity of the membrane.

[0039] (4) The preparation method of the present invention is simple. It can be prepared by simply mixing perfluorosulfonic acid resin with manganese genistein complex. Furthermore, the synthesis steps of manganese genistein complex are simple and the method is straightforward, laying a solid foundation for large-scale industrial preparation. Attached Figure Description

[0040] Figure 1 This is the X-ray energy dispersive spectroscopy (EDS) spectrum of the manganese isoflavone complex of the present invention.

[0041] Figure 2 The images show Fenton test results for the proton exchange membranes prepared in Examples 1-4 and Comparative Example 1.

[0042] Figure 3 The conductivity of the proton exchange membranes prepared in Examples 1-4 and Comparative Example 1 is shown as a function of temperature. Detailed Implementation

[0043] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0044] Unless otherwise specified, the reagents, methods, instruments, and equipment used in this invention are conventional in the art. Unless otherwise specified, the reagents and materials used in the following examples are all commercially available and of analytical grade. Specifically, the perfluorosulfonic acid resin was purchased from Shandong Dongyue Future Hydrogen Energy Materials Co., Ltd. (EW910), genistein was purchased from Shanghai Adamas Reagent Co., Ltd. (AR), and the coating machine was selected from Guangdong Kejian Instrument Co., Ltd. (KJ-6017B).

[0045] Example 1:

[0046] This embodiment provides a proton exchange membrane and its preparation method, the specific steps of which are as follows:

[0047] (1) Add 8g of perfluorosulfonic acid resin to a mixed solvent of 10g water, 10g isopropanol and 2g of N,N-dimethylaniline, and stir for 24h to obtain a uniform perfluorosulfonic acid solution.

[0048] (2) Weigh 1 mmol of genistein (0.27 g) and add it to 50 ml of ethanol-water solution at a 1:1 mass ratio. Stir until dissolved to obtain a mixed solution. Weigh 1 mmol of manganese nitrate tetrahydrate (0.251 g) and add it to the mixed solution. Heat in a 60°C water bath and stir for 12 h. Then centrifuge at 8000 rpm for 10 min, filter and wash three times with water, and finally dry at 60°C for 2 h to obtain the genistein manganese complex.

[0049] (3) Add 0.1g of manganese genistein complex to the perfluorosulfonic acid solution obtained in step (1), stir for 12h, and then sonicate in an ultrasonic cleaner for 60min to disperse it evenly. Then, coat it in a coating machine at a speed of 100mm / s using a 200μm wire rod. Finally, dry at 70℃ for 1h, anneal at 120℃ for 1h, and allow it to cool naturally to obtain a composite proton exchange membrane with a thickness of 15μm.

[0050] Example 2:

[0051] This embodiment provides a proton exchange membrane and its preparation method, the specific steps of which are as follows:

[0052] (1) Add 8g of perfluorosulfonic acid resin to a mixed solvent of 10g water, 10g isopropanol and 2g of N,N-dimethylaniline, and stir for 24h to obtain a uniform perfluorosulfonic acid solution.

[0053] (2) Weigh 1 mmol of genistein (0.27 g) and add it to 50 ml of ethanol-water solution at a 1:1 mass ratio. Stir until dissolved to obtain a mixed solution. Weigh 1 mmol of manganese nitrate tetrahydrate (0.251 g) and add it to the mixed solution. Heat in a 60°C water bath and stir for 12 h. Then centrifuge at 8000 rpm for 10 min, filter and wash three times with water, and finally dry at 60°C for 2 h to obtain the genistein manganese complex.

[0054] (3) 0.15 g of the manganese genistein complex was added to the perfluorosulfonic acid solution obtained in step (1). After stirring for 12 h, the mixture was ultrasonically cleaned for 60 min to ensure uniform dispersion. Subsequently, it was coated using a coating machine at a speed of 100 mm / s. The coating rod used was 200 μm in diameter. Finally, the membrane was dried at 70 °C for 1 h, annealed at 120 °C for 1 h, and allowed to cool naturally to obtain a composite proton exchange membrane with a thickness of 15 μm.

[0055] Example 3:

[0056] This embodiment provides a proton exchange membrane and its preparation method, the specific steps of which are as follows:

[0057] (1) Add 8g of perfluorosulfonic acid resin to a mixed solvent of 10g water, 10g isopropanol and 2g N,N-dimethylaniline, and stir for 24h to obtain a uniform perfluorosulfonic acid solution.

[0058] (2) Weigh 1 mmol of genistein (0.27 g) and add it to 50 ml of ethanol-water solution at a 1:1 mass ratio. Stir until dissolved to obtain a mixed solution. Weigh 1 mmol of manganese nitrate tetrahydrate (0.251 g) and add it to the mixed solution. Heat in a 60°C water bath and stir for 12 h. Then centrifuge at 8000 rpm for 10 min, filter and wash three times with water, and finally dry at 60°C for 2 h to obtain the genistein manganese complex.

[0059] (3) 0.2 g of the manganese genistein complex was added to the perfluorosulfonic acid solution obtained in step (1). After stirring for 12 h, the mixture was ultrasonically cleaned for 60 min to ensure uniform dispersion. Subsequently, it was coated using a coating machine at a speed of 100 mm / s. The coating rod used was 200 μm in diameter. Finally, the membrane was dried at 70 °C for 1 h, annealed at 120 °C for 1 h, and allowed to cool naturally to obtain a composite proton exchange membrane with a thickness of 15 μm.

[0060] Example 4:

[0061] This embodiment provides a proton exchange membrane and its preparation method, the specific steps of which are as follows:

[0062] (1) Add 8g of perfluorosulfonic acid resin to a mixed solvent of 10g water, 10g isopropanol and 2g N,N-dimethylaniline, and stir for 24h to obtain a uniform perfluorosulfonic acid solution.

[0063] (2) Weigh 1 mmol of genistein (0.27 g) and add it to 50 ml of ethanol-water solution at a 1:1 mass ratio. Stir until dissolved to obtain a mixed solution. Weigh 1 mmol of manganese nitrate tetrahydrate (0.251 g) and add it to the mixed solution. Heat in a 60°C water bath and stir for 12 h. Then centrifuge at 8000 rpm for 10 min, filter and wash three times with water, and finally dry at 60°C for 2 h to obtain the genistein manganese complex.

[0064] (3) 0.25 g of the manganese genistein complex was added to the perfluorosulfonic acid solution obtained in step (1). After stirring for 12 h, the mixture was ultrasonically cleaned for 60 min to ensure uniform dispersion. Subsequently, it was coated using a coating machine at a speed of 100 mm / s. The coating wire used was 200 μm in diameter. Finally, the membrane was dried at 70 °C for 1 h, annealed at 120 °C for 1 h, and allowed to cool naturally to obtain a composite proton exchange membrane with a thickness of 15 μm.

[0065] Comparative Example 1:

[0066] This embodiment provides a proton exchange membrane and its preparation method, the specific steps of which are as follows:

[0067] 8g of perfluorosulfonic acid resin was added to a mixed solvent of 10g water, 10g isopropanol, and 2g N,N-dimethylaniline, and stirred for 24h to obtain a homogeneous perfluorosulfonic acid solution. The solution was then coated using a coating machine at a speed of 100mm / s using a 200μm wire rod. Finally, the coating was dried at 70℃ for 1h, annealed at 120℃ for 1h, and allowed to cool naturally to obtain the composite proton exchange membrane.

[0068] The present invention conducted the following tests on Examples 1-4 and Comparative Example 1:

[0069] 1. Chemical durability test

[0070] Proton exchange membranes were prepared using the methods described in Examples 1-4 and Comparative Example 1, respectively, with 4 ppm Fe... 2+ Fenton's reagent was prepared by adding 0.00366 g of ferrous sulfate heptahydrate to 100 mL of 30 wt% H₂O₂. Then, a 4 cm × 4 cm membrane (dry weight m) was immersed in Fenton's reagent in an 80 °C water bath. The membrane sample was removed every 3 hours, washed three times at 80 °C, and the Fenton solution was replaced each time. The replaced Fenton solution was collected and a total ionic strength buffer was added. The fluoride concentration of the membrane sample was determined using an ion meter. The formula for calculating the fluoride ion release is as follows:

[0071] Fluoride ion release amount = (n×V) / (M×m)

[0072] Where n represents the fluoride concentration, V represents the remaining volume of the Fenton solution, M represents the molar mass of fluorine, and m represents the dry weight of the membrane sample.

[0073] 2. Conductivity test

[0074] The proton conductivity of the proton exchange membranes prepared in Examples 1-4 and Comparative Example 1 was tested according to GB / T 20042.3-2009 Proton Exchange Membrane Fuel Cells Part 3: Test Methods for Proton Exchange Membranes, at a temperature of 80°C and 100% RH.

[0075] 3. Water absorption rate test

[0076] The water absorption rate of the proton exchange membranes prepared in Examples 1-4 and Comparative Example 1 was tested according to GB / T 20042.3-2009 Proton Exchange Membrane Fuel Cells Part 3: Test Methods for Proton Exchange Membranes, at a temperature of 80°C.

[0077] 4. Tensile strength and elongation at break

[0078] The tensile strength and elongation at break of the proton exchange membranes prepared in Examples 1-4 and Comparative Example 1 were tested according to GB / T 20042.3-2009 Proton Exchange Membrane Fuel Cells Part 3: Test Methods for Proton Exchange Membranes.

[0079] Figure 1 EDS characterization of the genistein manganese complex. C, O, and Mn signals were observed in the EDS spectrum, indicating the co-existence of genistein and manganese, thus confirming the successful preparation of the genistein manganese complex.

[0080] Combining Examples 1-4 with Comparative Example 1 and in conjunction with Figure 2 It can be seen that after Fenton degradation treatment, the fluoride ion release of the proton exchange membranes prepared in Examples 1-4 is much lower than that of the proton exchange membrane prepared in Comparative Example 1, indicating that the additive genistein manganese complex plays an effective role in scavenging free radicals and greatly improves chemical durability.

[0081] Combining Examples 1-4 with Comparative Example 1 and in conjunction with Figure 3 It can be seen that the conductivity of Examples 1-3 is higher than that of Comparative Example 1, while the conductivity of Example 4 is slightly lower than that of Comparative Example 1. This indicates that an appropriate amount of additive is beneficial to improving conductivity, while an excessive amount of additive will hinder the improvement of conductivity. It is speculated that the excessive amount of additive may have an effect on the sulfonic acid groups in the film, which may hinder the proton transport channel.

[0082] Table 1 Performance Test Results

[0083]

[0084] Based on Examples 1-4 and Comparative Example 1, and in conjunction with Table 1, it can be seen that the proton exchange membrane containing the additive manganese genistein complex has a higher water absorption rate than the pure membrane, indicating that the additive promotes the water absorption of the proton exchange membrane.

[0085] Based on Examples 1-4 and Comparative Example 1, and in conjunction with Table 1, it can be seen that the tensile strength of Examples 1-4 is higher than that of Comparative Example 1, and the elongation at break of Examples 1-4 is lower than that of Comparative Example 1, indicating that the incorporation of the additive genistein manganese complex improves the strength of the proton exchange membrane.

[0086] This invention utilizes a perfluorosulfonic acid resin blended with a manganese genistein complex to form a membrane. Genistein acts as a free radical scavenger, while manganese acts as a hydrogen peroxide decomposition catalyst. This effectively removes hydroxyl radicals and hydrogen peroxide generated during fuel cell operation, significantly mitigating the damage to the membrane caused by the harsh operating environment of the fuel cell. Simultaneously, appropriate doping with the manganese genistein complex facilitates the formation of proton transport channels with low steric hindrance, thereby improving the membrane's proton conductivity.

[0087] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A method for preparing a high durability, high conductivity composite proton exchange membrane, characterized by, The composite proton exchange membrane comprises perfluorosulfonic acid resin and manganese genistein complex dispersed in perfluorosulfonic acid resin, wherein the mass ratio of manganese genistein complex to perfluorosulfonic acid resin is 1: (20-100). The preparation method includes the following steps: S1: Preparation of perfluorosulfonic acid solution: Disperse perfluorosulfonic acid resin in a mixed solvent and stir to obtain perfluorosulfonic acid solution; S2: Preparation of genistein manganese complex: Genistein and manganese salt were mixed, heated, centrifuged and dried to obtain genistein manganese complex; S3: Preparation of composite proton exchange membrane: The manganese genistein complex obtained in step S2 is added to the perfluorosulfonic acid solution obtained in step S1, and the mixture is stirred, sonicated, and cured to obtain the composite proton exchange membrane.

2. The method for preparing a high-durability, high-conductivity composite proton exchange membrane according to claim 1, characterized in that, In step S1, the mixed solvent includes isopropanol, water, and N,N-dimethylaniline, and the mass ratio of isopropanol, water, and N,N-dimethylaniline is 5:5:(0.8-1.2). The perfluorosulfonic acid resin accounts for 0.5-30% of the total mass of the perfluorosulfonic acid solution.

3. The method for preparing a high-durability, high-conductivity composite proton exchange membrane according to claim 1, characterized in that, In step S1, the stirring time is 6-24 hours and the stirring speed is 300-500 rpm.

4. The method for preparing a high-durability, high-conductivity composite proton exchange membrane according to claim 1, characterized in that, In step S2, the manganese salt includes one or more of manganese nitrate tetrahydrate, manganese acetate tetrahydrate, and manganese sulfate tetrahydrate; The molar ratio of genistein to manganese salt is (1-2):

1.

5. The method for preparing a high-durability, high-conductivity composite proton exchange membrane according to claim 1, characterized in that, In step S2, the heating temperature is 60-80℃, and the heating time is 6-12 hours. The centrifugation speed is 8000-12000 rpm, and the time is 10-30 min; The drying temperature is 60-80℃, and the time is 1-3 hours.

6. The method for preparing a high-durability, high-conductivity composite proton exchange membrane according to claim 1, characterized in that, In step S3, the stirring time is 8-16 hours and the stirring speed is 300-500 rpm. The ultrasound duration is 20-60 minutes.

7. The method for preparing a high-durability, high-conductivity composite proton exchange membrane according to claim 1, characterized in that, In step S3, the specific curing methods include coating, drying, and annealing; The coating speed of the scraping process is 100-200 mm / s; The drying temperature is 60-100℃, and the drying time is 1-2 hours; The annealing temperature is 120-160℃, and the annealing time is 1-2 hours.

8. A high-durability, high-conductivity composite proton exchange membrane, characterized in that, It is obtained by the preparation method described in any one of claims 1-7.

9. A high-durability, high-conductivity composite proton exchange membrane according to claim 8, characterized in that, The thickness of the composite proton exchange membrane is 8-30 μm.

10. The application of the high-durability, high-conductivity composite proton exchange membrane as described in claim 8 in the fabrication of fuel cells.

Citation Information

Patent Citations

  • Preparation method of high-durability myricetin chelated cerium ion composite proton exchange membrane

    CN114388857A

  • Fiber-reinforced stably-doped proton exchange membrane

    CN101728550A

  • Perfluorosulfonic composite proton exchange membrane for fuel cell

    CN101777659A