Method for improving organic field effect transistors with two-dimensional material doping and off-center spin coating

By using two-dimensional material doping and eccentric spin coating, the orderliness of P3HT thin films was improved, the problem of low mobility was solved, and organic field-effect transistors with high mobility and low threshold voltage were realized.

CN117355192BActive Publication Date: 2026-11-20XIAN UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311256246.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-26
Publication Date
2026-11-20
Estimated Expiration
2043-09-26

AI Technical Summary

Technical Problem

In existing technologies, P3HT thin films have low order, resulting in low mobility.

Method used

The organic field-effect transistor is improved by using two-dimensional material doping and eccentric spin coating. The specific steps include mixing dichloromethane and 1,2-dichlorobenzene solvent, adding P3HT and molybdenum disulfide powder, forming a highly ordered P3HT thin film by eccentric spin coating and vacuum annealing, and then depositing copper electrodes by evaporation.

Benefits of technology

It significantly improved the orderliness of P3HT films, increased the mobility by 13 times, significantly reduced the threshold voltage, and improved the charge transport efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117355192B_ABST
    Figure CN117355192B_ABST
Patent Text Reader

Abstract

The application discloses a method for improving an organic field effect transistor by using a two-dimensional material for doping and eccentric spin coating, and is specifically implemented according to the following steps: taking a 2cm*2cm silicon wafer, and cleaning the silicon wafer; mixing dichloromethane solvent and 1,2-dichlorobenzene solvent, dividing the mixed solution into two parts, adding P3HT powder to one part to obtain a P3HT mixed solution, and adding molybdenum disulfide powder to the other part, and after ultrasonic separation, taking supernatant; mixing the P3HT mixed solution and the supernatant to obtain a coating solution; coating the coating solution on the silicon wafer by using an eccentric spin coating method, and then performing vacuum annealing to obtain a silicon wafer comprising an active layer; and using a vacuum evaporation method to evaporate an electrode, and the electrode material is copper. The method solves the problems of low order degree and low mobility of a P3HT thin film in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor device technology, specifically relating to a method for improving organic field-effect transistors by doping with two-dimensional materials and eccentric spin coating. Background Technology

[0002] Solution-based fabrication of organic field-effect transistors offers advantages such as low cost, simplicity, and the ability to fabricate large areas. Poly(3-hexylthiophene) (P3HT) material, due to its excellent solubility, makes solution deposition the primary method for preparing its thin films. However, solution-based P3HT film fabrication suffers from low film order and grain boundary defects, leading to low film mobility.

[0003] Currently, many factors influence the mobility of P3HT devices prepared using solution methods, including the interface characteristics between the active and dielectric layers and the dielectric material itself. Through a series of exploratory studies, the performance of P3HT devices has improved. The low orderliness of P3HT films prepared using solution methods is the main reason for the low mobility of P3HT-based devices. To further improve device mobility, improvements are needed in both the fabrication materials and processes. Summary of the Invention

[0004] The purpose of this invention is to provide a method for improving organic field-effect transistors by doping with two-dimensional materials and eccentric spin coating, which solves the problems of low order and low mobility of P3HT thin films in the prior art.

[0005] The technical solution adopted in this invention is a method for improving organic field-effect transistors by doping with two-dimensional materials and eccentric spin coating, specifically implemented according to the following steps:

[0006] Step 1: Take a 2cm x 2cm silicon wafer and clean it.

[0007] Step 2: Mix dichloromethane solvent with 1,2-dichlorobenzene solvent, divide the mixture into two parts, add P3HT powder to one part to obtain P3HT mixed solution, add molybdenum disulfide powder to the other part, and after sonication and separation, take the supernatant.

[0008] Step 3: Mix the P3HT mixed solution with the supernatant to obtain the coating solution;

[0009] Step 4: Spin the coating liquid onto the silicon wafer using an eccentric spin coating method, and then vacuum anneal to obtain a silicon wafer including an active layer.

[0010] Step 5: Deposit the electrode using vacuum evaporation, with copper as the electrode material.

[0011] The invention is further characterized by:

[0012] The specific steps of step 1 are as follows: Clean the 2cm×2cm silicon wafer sequentially with acetone, ethanol, and deionized water using an ultrasonic cleaner for 9 to 11 minutes each.

[0013] Step 2 is as follows:

[0014] Step 2.1: Mix CH2Cl2 and o-DCB in any proportion and divide into two equal portions;

[0015] Step 2.2: Add P3HT powder to one of the mixtures, heat to dissolve, and obtain a P3HT mixed solution with a concentration of 10 mg / ml;

[0016] Step 2.3: Add molybdenum disulfide powder to another mixture at a volume ratio of 1 ml: 10 mg, and sonicate at 20 kHz to 40 kHz for 6 to 7 hours to obtain a molybdenum disulfide dispersion of 10 mg / mL. Centrifuge the dispersion and collect the supernatant.

[0017] The specific process of heating and dissolving in step 2.2 is as follows: place it on a hot plate at 68℃~72℃ and heat for 18min~22min to ensure complete dissolution.

[0018] The specific process for centrifuging the dispersion and obtaining the supernatant in step 2.3 is as follows: Place the 10 mg / mL molybdenum disulfide dispersion in a centrifuge tube, centrifuge at 2.5 k rpm to 3.5 k rpm for 12 min to 18 min, and then take the supernatant.

[0019] Step 3 involves ultrasonically mixing the P3HT mixed solution with the supernatant to obtain a coating solution with a molybdenum disulfide concentration of 0.5% to 10%.

[0020] Step 4 is as follows:

[0021] Step 4.1: Fix the silicon wafer to the edge of the spin coating chuck with tape, drop the coating liquid as the active layer material onto the silicon wafer, start the spin coater to perform eccentric spin coating, spin coating at a speed of 1000rpm~1200rpm for 30s;

[0022] Step 4.2: Place the silicon wafer after homogenization into a vacuum drying oven for annealing. Set the pressure to below 133 Pa and the temperature to 100 °C for annealing for 60 min to 90 min.

[0023] Step 5 is as follows:

[0024] Step 5.1: Place the silicon wafer with the active layer deposited on the substrate of the vacuum evaporation machine, cover it with the mask and ensure it is fixed;

[0025] Step 5.2: Evacuate the vacuum until the pressure is below 5 × 10⁻⁶. -3After the initial evaporation (PA), adjust the evaporation current to 110A-120A. Once the copper material has melted, adjust the current to maintain the evaporation rate. The copper electrode is deposited to a thickness of 70nm to 90nm. After the deposition is completed, the sample needs to be cooled for 30 to 40 minutes to prevent oxidation at room temperature. After cooling, it can be taken out. A copper sheet is attached to the back of the active layer of the silicon wafer as a gate electrode using conductive silver paste. After standing for 24 hours, an organic field-effect transistor is obtained.

[0026] The beneficial effects of this invention are:

[0027] This invention presents a method for improving organic field-effect transistors using two-dimensional material doping and eccentric spin coating. The method effectively improves charge transport efficiency through solution blending; eccentric spin coating enables directional crystal growth, resulting in a highly ordered thin film through a simple process; doping with 2D material MoS2 utilizes the interaction between MoS2 and P3HT, allowing the exfoliated two-dimensional MoS2 to induce the formation of long fiber structures in P3HT, effectively improving the orderliness of the P3HT thin film. Compared to devices prepared without this method, the mobility is increased by 13 times, and the threshold voltage is significantly reduced. Attached Figure Description

[0028] Figure 1(a) is a graph showing the output characteristics of the sample prepared in Example 4;

[0029] Figure 1(b) is a graph showing the output characteristics of the OFET prepared in Example 5;

[0030] Figure 2 The graph shows the changes in electrical parameters caused by variations in the solvent blending ratio in OFET.

[0031] Figure 3 This is a schematic diagram comparing the transfer characteristic curves of Example 5 and Example 6;

[0032] Figure 4(a) is an orientation analysis diagram of the field-effect transistor prepared in Example 5, plotted using GTFiber software;

[0033] Figure 4(b) is an orientation analysis diagram of the field-effect transistor prepared in Example 6, plotted using GTFiber software;

[0034] Figure 5(a) Schematic diagram of the output characteristic curve of Example 1;

[0035] Figure 5(b) is a schematic diagram of the output characteristic curve of Example 2;

[0036] Figure 5(c) is a schematic diagram of the output characteristic curve of Example 3;

[0037] Figure 6 This is a comparative diagram of XRD images from Examples 6, 1, and 2.

[0038] Figure 7 The AFM height map is for Example 6, Example 1, and Example 2. Detailed Implementation

[0039] The present invention will now be described in detail with reference to specific embodiments.

[0040] The two-dimensional material used in this invention is MoS2.

[0041] Example 1

[0042] Silicon wafers were cut into 2cm × 2cm samples using a laser cutter. The samples were then sequentially cleaned with acetone, ethanol, and deionized water using an ultrasonic cleaner for 10 minutes each. Materials were weighed using a calibrated electronic balance. o-DCB was used as the solvent, and the mixture was divided into two equal portions. One portion was mixed with P3HT powder to obtain a 10mg / ml P3HT solution, which was then heated on a 68℃ hot plate for 22 minutes to ensure complete dissolution. A 1ml solution was prepared. Molybdenum disulfide powder was added to the other portion of the mixture at a volume ratio of 1ml:10mg, and the mixture was ultrasonically treated at 20kHz for 7 hours to obtain a 10mg / mL molybdenum disulfide dispersion. The 10mg / mL molybdenum disulfide dispersion was placed in centrifuge tubes and centrifuged at 2.5 ppm. Centrifuge at 1000 rpm for 18 min and collect the supernatant. Sonicate the P3HT mixed solution with the supernatant to obtain a 0.5% molybdenum disulfide coating solution. Use a YQ201500131 spin coater for spin coating. Fix the silicon wafer to the edge of the spin coater with tape. Apply the coating solution as the active layer material onto the silicon wafer. Start the spin coater for eccentric spin coating at 1000 rpm for 30 s. After spin coating, remove the silicon wafer and place it in a DZF-6030B vacuum drying oven for annealing at 120 Pa and 100 °C for 1 h. Place the annealed silicon wafer into a ZHD-300 vacuum resistance evaporator. Place the silicon wafer with the active layer deposited on the substrate of the vacuum evaporator, cover it with the mask, and secure it. Evacuate to a pressure below 5 × 10⁻⁶. -3 After the initial evaporation current was adjusted to 115A, and once the material was completely melted into a liquid state, the baffle above the tungsten boat was removed, and the current was finely adjusted to maintain the evaporation rate. A 70nm thick copper electrode was deposited by vapor deposition. After the deposition was completed, the sample was allowed to cool down for 30 minutes to prevent oxidation at room temperature. Once the electrode deposition was complete, the evaporation power was turned off. A copper sheet was then attached to the back of the active layer of the silicon wafer using conductive silver paste as the gate electrode. After standing for 24 hours, an organic field-effect transistor was obtained.

[0043] Example 2

[0044] A laser beam generated by a laser cutter was used to cut silicon wafers into 2cm × 2cm samples. The samples were then cleaned sequentially with acetone, ethanol, and deionized water using an ultrasonic cleaner for 10 minutes each. The materials were weighed using a calibrated electronic balance. Dichloromethane solvent and 1,2-dichlorobenzene solvent were mixed at a ratio of 5:5. The mixture was divided into two portions. One portion was added to P3HT powder and heated on a hot plate at 69°C for 19 minutes to ensure complete dissolution, resulting in a P3HT mixed solution with a concentration of 10 mg / mL. Molybdenum disulfide powder was added to the other portion of the mixture at a volume ratio of 1 ml:10 mg, and the mixture was ultrasonically treated at 30 kHz for 6.5 hours to obtain a molybdenum disulfide dispersion with a concentration of 10 mg / mL. The 10 mg / mL molybdenum disulfide dispersion was placed in a centrifuge tube and centrifuged at 3.0 krpm for 15 minutes. The supernatant was collected, and the P3HT mixed solution was mixed with the supernatant and ultrasonically dissolved for 30 minutes to ensure complete dissolution, resulting in a coating solution with a molybdenum disulfide concentration of 5%. Spin coating was performed using a YQ201500131 spin coater. The silicon wafer was secured to the edge of the spin coater with tape. The coating liquid, used as the active layer material, was dropped onto the silicon wafer. The spin coater was started for eccentric spin coating at 1100 rpm for 30 seconds. The coated silicon wafer was then placed in a vacuum drying oven for annealing at a pressure of 110 Pa and a temperature of 100 °C for 70 minutes. After spin coating, the silicon wafer was removed and placed in a DZF-6030B vacuum drying oven for annealing at a pressure below 133 Pa and a temperature of 120 °C for 1 hour. The annealed silicon wafer was then placed in a ZHD-300 vacuum resistance evaporation machine. The silicon wafer with the active layer deposited was placed on the substrate of the vacuum evaporation machine, and the mask was placed on top and secured. Initially, the evaporation current was adjusted to 110 A. Once the material was completely melted into a liquid state, the baffle above the tungsten boat was removed, and the current was finely adjusted to maintain the evaporation speed. The copper electrode is deposited to a thickness of 80 nm. After the deposition is completed, the sample needs to be cooled for 35 minutes to prevent oxidation at room temperature. After cooling, it can be taken out. A copper sheet is attached to the back of the active layer of the silicon wafer as a gate electrode using conductive silver paste. After standing for 24 hours, an organic field-effect transistor is obtained.

[0045] Example 3

[0046] A laser beam generated by a laser cutter was used to cut silicon wafers into 2cm × 2cm samples. The samples were then cleaned sequentially with acetone, ethanol, and deionized water using an ultrasonic cleaner for 10 minutes each. Materials were weighed using a calibrated electronic balance. CH2Cl2 and o-DCB were mixed at a ratio of 3:7 and divided into two equal portions. P3HT powder was added to one portion of the mixture, and it was heated on a hot plate at 72°C for 18 minutes to ensure complete dissolution, yielding a P3HT mixed solution with a concentration of 10 mg / mL. Molybdenum disulfide powder was added to the other portion of the mixture at a volume ratio of 1 ml:10 mg, and the mixture was ultrasonically treated at 25 kHz for 6 hours to obtain a 10 mg / mL molybdenum disulfide dispersion. This 10 mg / mL dispersion was placed in a centrifuge tube and centrifuged at 3.5 rpm for 12 minutes, and the supernatant was collected. The P3HT mixed solution and the supernatant were then ultrasonically dissolved for 30 minutes to ensure complete dissolution, yielding a coating solution with a molybdenum disulfide concentration of 10%. Spin coating was performed using a YQ201500131 spin coater. The silicon wafer was secured to the edge of the spin coater with tape. The coating liquid, used as the active layer material, was dropped onto the silicon wafer. The spin coater was started and spin-coated at 1200 rpm for 30 seconds. The coated silicon wafer was then placed in a vacuum drying oven for annealing at a pressure of 125 Pa and a temperature of 100 °C for 90 minutes. The silicon wafer with the active layer deposited was then placed on the substrate of a vacuum evaporation machine, and the mask was placed on top and secured. A vacuum was then drawn until the pressure was below 5 × 10⁻⁶. -3 After pa, adjust the evaporation current to 120A. After the copper material melts, adjust the current to maintain the evaporation rate. The copper electrode is 90nm thick. After the evaporation is completed, the sample needs to be cooled for 40 minutes to prevent oxidation at room temperature. After cooling, it can be taken out. A copper sheet is attached to the back of the active layer of the silicon wafer as a gate electrode using conductive silver paste. After standing for 24 hours, an organic field-effect transistor is obtained.

[0047] Example 4

[0048] This example serves as a control group without any optimization: A laser beam from a laser cutter was used to cut silicon wafers into 2cm × 2cm samples. The samples were then sequentially cleaned with acetone, ethanol, and deionized water using an ultrasonic cleaner for 10 minutes each. Materials were weighed using a calibrated electronic balance. 1,2-Dichlorobenzene was used as the solvent, and P3HT as the solute (P3HT concentration: 10 mg / ml). The prepared solution was ultrasonically dissolved for 30 minutes to ensure complete dissolution. A YQ201500131 spin coater was used for spin coating. The substrate was adsorbed onto the center of the suction cup, and a small amount of solution was dripped onto the silicon wafer surface using a syringe until the surface was completely covered. The spin coater cover was then closed, and the wafer was spin-coated at 1100 rpm for 30 seconds. After spin coating, the silicon wafer was removed and placed in a DZF-6030B vacuum drying oven for annealing at 130 Pa and 120°C for 1 hour. The annealed silicon wafer was placed in a ZHD-300 vacuum resistance evaporation machine, and an 80nm thick copper electrode was deposited using a mask. Initially, the evaporation current was adjusted to around 115A. Once the material was completely melted into a liquid state, the baffle above the tungsten boat was removed, and the current was finely adjusted to maintain the evaporation speed. After the electrode deposition is complete, turn off the evaporation power supply. To avoid electrode oxidation caused by excessive temperature difference between the inside and outside of the chamber, wait 30 minutes for the sample temperature to drop to room temperature to complete the copper electrode deposition. Finally, use conductive silver paste to attach a copper sheet as the gate electrode to the back of the active layer of the silicon wafer, and let it stand in a vacuum environment for 24 hours to complete the fabrication of the entire field-effect transistor.

[0049] Example 5

[0050] Molybdenum disulfide-free, non-eccentric coating: Silicon wafers were cut into 2cm × 2cm samples using a laser beam generated by a laser cutter. The samples were then ultrasonically cleaned for 10 minutes each with acetone, ethanol, and deionized water. Materials were weighed using a calibrated electronic balance. A solvent was prepared by mixing 1,2-dichlorobenzene and dichloromethane in a 5:5 ratio, with P3HT as the solute, to prepare a 10 mg / ml P3HT solution. The mixing ratio of 1,2-dichlorobenzene to dichloromethane was 7:3. The solubility of P3HT polymer in dichloromethane is strongly dependent on the solution temperature; therefore, the solution was heated on a 70°C hot plate for 20 minutes to ensure complete dissolution. The prepared solution was then ultrasonically dissolved for 30 minutes to ensure complete dissolution. Spin coating was performed using a YQ201500131 spin coater. The substrate was held in the center of the suction cup, and a small amount of solution was dripped onto the silicon wafer surface using a syringe until the surface was completely covered. The spin coater cover was then closed, and the wafer was spin-coated at 1100 rpm for 30 seconds. After spin coating, the wafer was removed and placed in a DZF-6030B vacuum drying oven for annealing at 130 Pa and 120 °C for 1 hour. The annealed wafer was then placed in a ZHD-300 vacuum resistance evaporation machine, and an 80 nm thick copper electrode was deposited using a mask. Initially, the evaporation current was set to 115 A. Once the material was completely melted into a liquid state, the baffle above the tungsten boat was removed, and the current was finely adjusted to maintain the evaporation speed. After the electrode deposition is complete, turn off the evaporation power supply. To avoid electrode oxidation caused by excessive temperature difference between the inside and outside of the chamber, wait 30 minutes for the sample temperature to drop to room temperature to complete the copper electrode deposition. Finally, use conductive silver paste to attach a copper sheet as the gate electrode to the back of the active layer of the silicon wafer, and let it stand in a vacuum environment for 24 hours to complete the fabrication of the entire organic field-effect transistor.

[0051] Example 6

[0052] Eccentric molybdenum disulfide-free process: A 4-inch oxide wafer was cut into 2cm × 2cm samples using a laser beam generated by a laser cutter. The samples were then ultrasonically cleaned for 10 minutes each with acetone, ethanol, and deionized water. Materials were weighed using a calibrated electronic balance. A solvent was prepared by mixing 1,2-dichlorobenzene and dichloromethane, with P3HT as the solute, to prepare a 1ml solution with a P3HT concentration of 10mg / ml. The mixing ratio of 1,2-dichlorobenzene to dichloromethane was 7:3. The solution was heated on a 70℃ hot plate for 20 minutes to fully dissolve the solute. The prepared solution was then ultrasonically dissolved for 30 minutes to ensure complete dissolution. A YQ201500131 spin coater was used for spin coating. The substrate was placed on the edge of the spin coater and secured with tape. A small amount of solution was dripped onto the silicon wafer surface using a syringe until the surface was completely covered. The spin coater was then closed, and the wafer was spin-coated at 1100 rpm for 30 seconds. After spin coating, the silicon wafer is removed and placed in a DZF-6030B vacuum drying oven for annealing at a pressure below 133 Pa and a temperature of 120℃ for 1 hour. The annealed silicon wafer is then placed in a ZHD-300 vacuum resistance evaporation machine, where an 80nm thick copper electrode is deposited using a mask. Initially, the evaporation current is adjusted to approximately 115A. Once the material has completely melted into a liquid state, the baffle above the tungsten boat is removed, and the current is finely adjusted to maintain the evaporation speed. After the electrode deposition is complete, turn off the evaporation power supply. To avoid electrode oxidation caused by excessive temperature difference between the inside and outside of the chamber, wait 30 minutes for the sample temperature to drop to room temperature to complete the copper electrode deposition. Finally, use conductive silver paste to attach a copper sheet to the back of the SiO2 as the gate electrode, and let it stand in a vacuum environment for 24 hours to complete the fabrication of the entire OFET.

[0053] Figures 1(a) and 1(b) show the output characteristic curves of Examples 4 and 5, respectively. As can be seen from the figures, when only 1,2-dichlorobenzene is used as the solvent, the saturation source leakage current of the device is relatively small, only 4.3 μA. The saturation leakage current increases significantly when dichloromethane and 1,2-dichlorobenzene are blended.

[0054] Figure 2 These are the electrical characteristic parameters when CH2Cl2 and o-DCB are blended in a binary solvent ratio of 5:5. It can be seen that blending the two solvents improves device performance, with a mobility reaching 0.0134 cm⁻¹. 2 / Vs, compared to 0.0064cm when pure o-dichlorobenzene is used as a solvent 2 / Vs increased by more than two times, and the threshold voltage of 30.46V also showed a significant improvement.

[0055] Figure 3 A comparison of the transfer characteristic curves of Example 5 and Example 6 shows that the device mobility after eccentric spin coating is 0.0641 (cm).2 / Vs) compared to the center spin coating of 0.0214 (cm) 2 The voltage ( / Vs) is significantly improved, while the threshold voltage is also reduced to a certain extent, resulting in better electrical characteristics.

[0056] Figures 4(a) and 4(b) are orientation analysis diagrams generated by GTFiber software in Examples 5 and 6, respectively. It can be observed that the nanofiber orientation in the central spin-coated orientation diagram is randomly distributed and lacks directionality, while the nanofiber orientation in the eccentric spin-coated orientation diagram is more ordered and has stronger directionality. Simultaneously, data extraction reveals that the average orientation of the microcrystals in the central spin-coated film is 75° relative to the horizontal direction, and the order parameter S... 2D Only 0.20. The average orientation of the microcrystals present in the eccentric spin-coated film is -5° relative to the horizontal direction, and the order parameter S 2D The value increased significantly to 0.54. The center spin coating showed greater orderliness.

[0057] Figures 5(a), 5(b), and 5(c) show the output characteristic curves of Examples 1, 2, and 3, respectively. It can be seen that as the MoS2 doping ratio increases, the saturation leakage current of the device first increases and then decreases. Further extraction of parameters such as mobility reveals that the mobility is highest at a MoS2 doping ratio of 5%, reaching 0.0856 (cm²). 2 The threshold voltage is 2V, which is a significant improvement over the undoped state. However, the device performance decreases when the MoS2 doping ratio is further increased.

[0058] Figure 6 The XRD patterns for different MoS2 doping ratios show that the (100) reflection corresponding to the alkyl stacking of the P3HT chain appears at the same diffraction angle in each sample, but the peak intensity is different. The 100 peak intensity is the highest when the MoS2 doping ratio is 5%, indicating that the degree of ordering and crystallization of P3HT is the highest at this time, and the film performance is better.

[0059] Figure 7 AFM height maps for different MoS2 doping ratios also confirm this. The figures show that: ① with 0% doping, the original P3HT film is relatively smooth, forming a ball-and-bar structure. ② With 5% doping, interconnected nanofiber structures are observed in the MoS2-doped film. This indicates that the addition of MoS2 nanosheets induces the formation of long fibers, and the interaction between P3HT and MoS2 monolayer nanosheets enhances interchain order. ③ When the doping ratio continues to increase to 10%, more and more unexfoliated nanosheets are observed, resulting in a less prominent nanofiber structure in the P3HT film. In summary, 5% doping yields the best results.

[0060] Through the above methods, this invention provides an organic field-effect transistor fabrication method based on solvent blending and process improvement. Solution blending effectively enhances charge transport efficiency; eccentric spin coating enables directional crystal growth, resulting in a highly ordered thin film with a simple process; doping with 2D MoS2 utilizes the interaction between MoS2 and P3HT, allowing the exfoliated 2D MoS2 to induce the formation of long fiber structures in P3HT, effectively improving the orderliness of the P3HT thin film. This results in a 13-fold increase in mobility and a significant decrease in threshold voltage compared to devices fabricated without this method. This provides a feasible solution for fabricating high-mobility P3HT thin films.

Claims

1. A method for improving organic field-effect transistors using two-dimensional material doping and eccentric spin coating, characterized in that, The specific steps are as follows: Step 1: Take a 2cm x 2cm silicon wafer and clean it. Step 2: Mix dichloromethane solvent with 1,2-dichlorobenzene solvent, divide the mixture into two parts, add P3HT powder to one part to obtain P3HT mixed solution, add molybdenum disulfide powder to the other part, and after sonication and separation, take the supernatant. Step 3: Mix the P3HT mixed solution with the supernatant to obtain the coating solution; Step 4: Spin the coating liquid onto the silicon wafer using an eccentric spin coating method, and then vacuum anneal to obtain a silicon wafer including an active layer. Step 5: Deposit the electrode using vacuum evaporation, with copper as the electrode material; Step 2 is as follows: Step 2.1: Mix CH2Cl2 and o-DCB at a blending ratio of 5:5 and divide the mixture into two equal portions; Step 2.2: Add P3HT powder to one of the mixtures, heat to dissolve, and obtain a P3HT mixed solution with a concentration of 10 mg / mL; Step 2.3: Add molybdenum disulfide powder to another mixture at a volume ratio of 1 mL: 10 mg, and sonicate at 30 kHz for 6.5 h to obtain a 10 mg / mL molybdenum disulfide dispersion. Centrifuge the dispersion and collect the supernatant. Step 4 is as follows: Step 4.1: Fix the silicon wafer to the edge of the spin coating chuck with tape, drop the coating liquid as the active layer material onto the silicon wafer, start the spin coater to perform eccentric spin coating, spin coating at 1100 rpm for 30 seconds; Step 4.2: Place the coated silicon wafer into a vacuum drying oven for annealing. Set the pressure to 110 Pa and the temperature to 100 °C and anneal for 70 min.

2. The method for improving organic field-effect transistors using two-dimensional material doping and eccentric spin coating according to claim 1, characterized in that, The specific steps of step 1 are as follows: Clean the 2cm×2cm silicon wafer sequentially with acetone, ethanol, and deionized water using an ultrasonic cleaner for 9 to 11 minutes each.

3. The method for improving organic field-effect transistors using two-dimensional material doping and eccentric spin coating according to claim 1, characterized in that, The specific process of heating and dissolving in step 2.2 is as follows: place it on a hot plate at 68℃~72℃ and heat for 18min~22min to ensure complete dissolution.

4. The method for improving organic field-effect transistors using two-dimensional material doping and eccentric spin coating according to claim 1, characterized in that, The specific process for centrifuging the dispersion to obtain the supernatant in step 2.3 is as follows: place the 10 mg / mL molybdenum disulfide dispersion in a centrifuge tube, centrifuge at 2.5 k rpm to 3.5 k rpm for 12 min to 18 min, and then take the supernatant.

5. The method for improving organic field-effect transistors using two-dimensional material doping and eccentric spin coating according to claim 1, characterized in that, Step 3 involves ultrasonically mixing the P3HT mixed solution with the supernatant to obtain a coating solution with a molybdenum disulfide concentration of 5%.

6. The method for improving organic field-effect transistors using two-dimensional material doping and eccentric spin coating according to claim 1, characterized in that, Step 5 is as follows: Step 5.1: Place the silicon wafer with the active layer deposited on the substrate of the vacuum evaporation machine, cover it with the mask and ensure it is fixed; Step 5.2: Evacuate the vacuum until the pressure is below 5 × 10⁻⁶. -3 After pa, adjust the evaporation current to 110A~120A. After the copper material melts, adjust the current to maintain the evaporation rate at 0.8Å / s. The thickness of the evaporated copper electrode is 70nm~90nm. After the evaporation is completed, wait 30min~40min to allow the sample to cool down to prevent oxidation at room temperature. After cooling, it can be taken out. Use conductive silver paste to attach a copper sheet as a gate electrode to the back of the active layer of the silicon wafer. Let it stand for 24 hours to obtain an organic field-effect transistor.

Citation Information

Patent Citations

  • Method for regulating and controlling ordered growth of organic thin film molecules by using magnetic field

    CN107910446A

  • Organic field effect transistors

    US20050023522A1