Method for manufacturing a bonded body and apparatus for manufacturing a bonded body

By using a circular transparent glass plate and a circular sealing component, the problem of uneven pressing pressure caused by the shape of the cover and sealing component of the clamp body is solved, the adhesion between the sealing material and the substrate is improved, and the quality of the joint is ensured.

CN117355492BActive Publication Date: 2026-11-20NIPPON ELECTRIC GLASS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202280032050.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-29
Filing Date
2022-05-17
Publication Date
2026-11-20
Estimated Expiration
2042-05-17

AI Technical Summary

Technical Problem

In the prior art, because the cover and sealing member of the fixture body are quadrilateral, the pressure applied to the laminate is uneven, resulting in insufficient adhesion between the sealing material and the substrate, which easily leads to poor bonding, especially when the substrate is large.

Method used

A circular transparent glass plate is used as the pressing component, and a circular sealing component is set between the base component and the pressing component. The air pressure is reduced in the receiving space by the air pressure adjustment device, so that the pressing component and the sealing component are tightly attached, thereby pressing the laminate evenly and ensuring the tightness of the sealing material and the substrate.

Benefits of technology

By improving the structure and method, the adhesion between the sealing material and each substrate is enhanced, uneven pressing pressure is reduced, poor bonding is avoided, and the quality of the joint is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117355492B_ABST
    Figure CN117355492B_ABST
Patent Text Reader

Abstract

The bonding step in the manufacturing method of the bonded body includes a supporting step of fitting the laminate to a supporting device and a pressing step of pressing the laminate. The pressing member of the supporting device is a transparent glass plate configured in a circular shape. The sealing member of the supporting device is configured to surround the laminate in a circular shape between the pressing member and the base member. In the pressing step, the pressing member and the sealing member are brought into close contact by lowering the air pressure of the accommodation space using an air pressure adjusting device, and the laminate is pressed using the pressing member.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method and apparatus for manufacturing a bonded body by bonding substrates. Background Technology

[0002] As is well known, LED components and other electronic components are housed in hermetically sealed packages to prevent degradation. A hermetically sealed package is, for example, formed by bonding a first substrate, which serves as the base material, to a second substrate made of a glass substrate.

[0003] For example, Patent Document 1 discloses a method for manufacturing a bonded body by sandwiching a sealing material (bonding material) between a first substrate (a component to be bonded) and a second substrate made of a glass component and heating the sealing material.

[0004] In this manufacturing method, a laminate in which a sealing material is disposed between a first substrate and a second substrate is prepared, and the laminate is assembled into a jig and the internal air pressure of the jig is adjusted to press the laminate. Furthermore, while the laminate is pressed, the sealing material is irradiated with a laser, and a joint is formed by the sealing material, thereby manufacturing a joint (see paragraphs 0036 to 0046 of this document).

[0005] The fixture used in this manufacturing method includes a fixture body that supports the laminate and a cover for pressing the laminate. For example... Figure 23 (equivalent to this document) Figure 3 As shown, the fixture body 101 has a recess 102 for receiving the laminate LM and a force-applying part 103 disposed in the recess 102 for placing the laminate LM.

[0006] In addition, such as Figure 23 As shown, the clamp body 101 has a sealing member (backing member) 104 at the front end (upper end) of its peripheral wall portion (refer to paragraph 0041 of this document). The sealing member 104 is configured as a quadrilateral shape in plan view, corresponding to the shape of the peripheral wall portion of the clamp body 101, in a manner that surrounds the force application portion 103 and the laminated body LM.

[0007] The cover of the clamp body, the clamp body 101, and the sealing member 104 are respectively configured in a quadrilateral shape (refer to the document). Figure 4 The cover for the fixture body is placed on the sealing member 104 when it is installed on the fixture body 101.

[0008] In the manufacturing method of the joint in Patent Document 1, the gas in the recess 102 is discharged by a pump, thereby reducing the air pressure in the recess 102, so that the cover of the clamp body can be tightly attached to the sealing member 104, and the cover of the clamp body can be flexed to press the laminate LM.

[0009] Existing technical documents

[0010] Patent documents

[0011] Patent Document 1: Japanese Patent Application Publication No. 2021-31306 Summary of the Invention

[0012] The problem that the invention aims to solve

[0013] In the conventional manufacturing method of the joint described above, the sealing member 104 is formed into a quadrilateral shape, and the cover of the clamp body is also formed into a quadrilateral shape, which may cause the following problems.

[0014] That is, such as Figure 23 As shown, the distance D1 from the middle position P1 of one side of the sealing member 104, which is configured in a quadrilateral shape, to the center O of the laminate LM is different from the distance D2 from the corner position P2 of the sealing member 104 to the center O of the laminate LM. This difference in distances D1 and D2 is a major cause that may result in uneven pressure exerted by the cover of the clamping body on the laminate LM. This uneven pressure becomes more pronounced as the size of the laminate LM increases.

[0015] When uneven pressure is applied to the laminate by the cover of the fixture body as described above, insufficient adhesion between the sealing material located between the first substrate and the second substrate is generated, resulting in poor bonding.

[0016] The present invention was made in view of the above circumstances, and its technical problem is to improve the adhesion between the sealing material and each substrate when a joint is manufactured by irradiating the sealing material sandwiched between substrates with a laser.

[0017] Solution for solving the problem

[0018] This invention provides a method for manufacturing a bond to solve the aforementioned problems. The method manufactures a bond comprising a first substrate, a second substrate, and a sealing layer for bonding the first substrate and the second substrate. The method includes: a lamination step, in which a sealing material is sandwiched between the first substrate and the second substrate, and the first substrate and the second substrate are overlapped to form a laminate; and a bonding step, in which the sealing material in the laminate is irradiated with a laser to form the sealing layer. The bonding step includes: a support step, in which the laminate is assembled onto a support device; a pressing step, in which the laminate is pressed; and a laser irradiation step, in which the sealing material is irradiated with a laser. The laser-supporting device includes: a pressing member that presses the laminate; a base member that supports the pressing member; a sealing member disposed between the pressing member and the base member; a receiving space for the laminate formed between the pressing member and the base member; and a pressure adjusting device that adjusts the pressure of the receiving space. The pressing member is a circular transparent glass plate, and the sealing member is configured to circularly surround the laminate between the pressing member and the base member. In the pressing process, the pressure adjusting device reduces the pressure of the receiving space, thereby causing the pressing member and the sealing member to adhere tightly, and the pressing member presses the laminate.

[0019] According to this structure, by making the pressing member a circular transparent glass plate and configuring the sealing member located between the base member and the pressing member as a circular enclosure of the laminate, the unevenness of the force exerted by the pressing member on the laminate during the pressing process can be minimized. This improves the adhesion of the sealing material in the laminate to each substrate.

[0020] Alternatively, the support device may include a support member that supports the laminate within the receiving space. The support member has a receiving portion that receives the laminate. In the supporting process, the first substrate is received in the receiving portion, and the second substrate is received in the receiving portion such that a portion of the second substrate in the thickness direction extends from the receiving portion toward the pressing member. Here, the receiving portion can be a recess capable of receiving the laminate; there are no particular limitations as long as it allows for positioning of the laminate. For example, multiple positioning protrusions can be provided on the surface of the support member, and the space inside it can be designated as the receiving portion.

[0021] The second substrate constituting the laminate is a glass substrate, and a portion of the thickness direction of the second substrate extends from the receiving portion of the support member, so that the pressing member can reliably contact the second substrate of the laminate during the pressing process and effectively press the laminate.

[0022] Furthermore, the second substrate is housed in the receiving portion by means of a portion other than the portion extending from the receiving portion as described above, thereby preventing positional displacement during the supporting and pressing processes and instead locking it in place with the receiving portion. This allows for precise laser irradiation of the sealing material of the laminate.

[0023] Alternatively, a portion of the second substrate extending from the receiving portion in the thickness direction may be 0.05 to 0.95 times the thickness of the second substrate.

[0024] In this method, the air pressure of the containment space is preferably 100 to 95000 Pa, more preferably 1000 to 85000 Pa.

[0025] Alternatively, the thickness of the pressing member can be 3–10 mm. Furthermore, the Young's modulus of the pressing member is preferably 50–80 GPa, more preferably 60–70 GPa. Thus, during the pressing process, the pressing member can appropriately press the laminate through moderate flexing.

[0026] Alternatively, during the supporting process, dry air can be filled into the receiving space. This allows for a lower moisture content within the cavity formed by the manufactured assembly, preventing performance degradation of electronic components such as LEDs within the hermetically sealed package.

[0027] Furthermore, preferably, the first substrate is a high thermal conductivity substrate and the second substrate is a glass substrate.

[0028] This invention provides a manufacturing apparatus for a bond to solve the aforementioned problems. The apparatus manufactures a bond comprising a first substrate, a second substrate, and a sealing layer for bonding the first and second substrates. The manufacturing apparatus is characterized by comprising: a support device for supporting a laminate, the laminate being formed by sandwiching a sealing material between the first and second substrates and overlapping the first and second substrates; and a laser irradiation device for irradiating the sealing material in the laminate with a laser to form the sealing layer. The support device includes: a pressing member for pressing the laminate; and a base plate. The assembly includes a base member supporting the pressing member; a sealing member disposed between the pressing member and the base member; a receiving space for the laminate formed between the pressing member and the base member; and a pressure adjusting device for adjusting the pressure of the receiving space. The pressing member is a circular transparent glass plate, and the sealing member is configured to circularly surround the laminate between the pressing member and the base member. The manufacturing apparatus for the joint is configured to reduce the pressure of the receiving space using the pressure adjusting device, thereby causing the pressing member and the sealing member to adhere tightly, and to press the laminate using the pressing member.

[0029] According to this structure, by making the pressing member a circular transparent glass plate and configuring the sealing member located between the base member and the pressing member as a circular surrounding laminate, the unevenness of the force exerted by the pressing member on the laminate can be minimized. This improves the adhesion of the sealing material in the laminate to each substrate.

[0030] Invention Effects

[0031] According to the present invention, when a joint is manufactured by irradiating a sealing material sandwiched between substrates with a laser, the adhesion between the sealing material and each substrate can be improved. Attached Figure Description

[0032] Figure 1 This is a top view of the assembly.

[0033] Figure 2 yes Figure 1 A cross-sectional view along line II-II.

[0034] Figure 3 This is a bottom view of the second substrate.

[0035] Figure 4 This is a cross-sectional view showing the manufacturing apparatus for the joint.

[0036] Figure 5 This is a top view showing a portion of the support device.

[0037] Figure 6 yes Figure 5 A sectional view of the line of sight from VI to VI.

[0038] Figure 7 This is a top view of the supporting structure.

[0039] Figure 8 This is a top view of the pressing component.

[0040] Figure 9 This is a top view of the frame.

[0041] Figure 10 This is a cross-sectional view showing a method of mounting a support member onto a base member.

[0042] Figure 11 This is a top view showing the method of mounting the support member onto the base member.

[0043] Figure 12 yes Figure 11 A cross-sectional view along line XII-XII.

[0044] Figure 13 This is a flowchart illustrating the manufacturing method of the joint.

[0045] Figure 14 This is a cross-sectional view showing the lamination process.

[0046] Figure 15 This is a flowchart illustrating the joining process.

[0047] Figure 16 This is a cross-sectional view showing the support process.

[0048] Figure 17 This is a cross-sectional view showing the support process.

[0049] Figure 18 This is a top view showing the manufacturing apparatus for the joint of the second embodiment.

[0050] Figure 19 This is a top view of the supporting structure.

[0051] Figure 20 This is a cross-sectional view showing a method of mounting a support member onto a base member.

[0052] Figure 21 This is a cross-sectional view showing the support process.

[0053] Figure 22 This is a cross-sectional view showing the support process.

[0054] Figure 23 This is a top view showing a portion of a conventional assembly manufacturing apparatus. Detailed Implementation

[0055] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. Figures 1 to 17 A first embodiment of the manufacturing method and manufacturing apparatus for the joint of the present invention is shown.

[0056] Figure 1 as well as Figure 2 An example of a hermetically sealed assembly is provided as a bonding body manufactured by the present invention. The bonding body 1 includes: a first substrate 2, which serves as a substrate; a second substrate 3, which overlaps with the first substrate 2; a plurality of sealing layers 4, which bond the first substrate 2 and the second substrate 3; and an element 5, which is housed between the first substrate 2 and the second substrate 3 and inside the sealing layers 4.

[0057] The first substrate 2 is configured in a rectangular shape, for example, but is not limited to that shape. The first substrate 2 has a first main surface 2a for mounting the element 5 and a second main surface 2b located on the opposite side of the first main surface 2a. The first main surface 2a may have a recess capable of accommodating the element 5.

[0058] The first substrate 2 is made of a high thermal conductivity substrate, such as a silicon substrate, but is not limited to these; it may also be made of other metal substrates, ceramic substrates, semiconductor substrates, or various other substrates. It should be noted that the thickness of the first substrate 2 is in the range of 0.1 to 5.0 mm, but is not limited to this range.

[0059] The thermal conductivity of the first substrate 2 can be higher than that of the second substrate 3. The thermal conductivity of the first substrate 2 at 20°C is preferably 10 to 500 W / m·K, more preferably 30 to 300 W / m·K, even more preferably 70 to 250 W / m·K, particularly preferably 100 to 200 W / m·K, but is not limited to this range.

[0060] The second substrate 3 is, for example, made of a rectangular transparent glass substrate, but is not limited to that shape. The second substrate 3 has a first main surface 3a and a second main surface 3b located on the opposite side of the first main surface 3a.

[0061] As the glass constituting the second substrate 3, for example, alkali-free glass, borosilicate glass, soda lime glass, quartz glass, or crystallized glass with a low coefficient of thermal expansion can be used. The thickness of the second substrate 3 is not particularly limited, but a thickness in the range of 0.01 to 2.0 mm is used, for example. The thermal conductivity of the second substrate 3 at 20°C is preferably 0.5 to 5 W / m·K, but is not limited to this range.

[0062] Multiple sealing layers 4 are formed on the bonding body 1 in a prescribed arrangement pattern. The sealing layers 4 are formed by sandwiching multiple sealing materials between the first substrate 2 and the second substrate 3, irradiating the sealing materials with a laser, and softening and flowing them by heating.

[0063] Figure 3 This is a bottom view showing the second substrate 3 before it is bonded to the first substrate 2. When a sealing material is sandwiched between the first substrate 2 and the second substrate 3, for example, the sealing material 6 can be pre-fixed to the first main surface 3a of the second substrate 3. It is not limited to this; the sealing material can be pre-fixed to the first substrate 2, or a sheet-like sealing material can be sandwiched between the first substrate 2 and the second substrate 3.

[0064] Various materials can be used as sealing materials. Among them, from the viewpoint of improving sealing strength, composite materials (glass frits) containing bismuth-based glass powder and refractory filler powder are preferred. Not only bismuth-based glass, but also glass powders such as silver phosphate glass and tellurium glass can be used as sealing materials.

[0065] As a refractory filler powder, various materials can be used, among which, preferably, it is composed of one or more materials selected from cordierite, zircon, tin oxide, niobium oxide, zirconium phosphate ceramics, zinc siliceous ore, β-lithium nepheline, and β-quartz solid solution.

[0066] like Figure 1 As shown, the sealing layer 4 is configured as a closed curve in a way that spatially joins the housing element 5. In this invention, the term "closed curve" is used not only for shapes composed solely of curves, but also for shapes composed of a combination of curves and straight lines, and shapes composed solely of straight lines (e.g., quadrilateral shapes, other polygonal shapes).

[0067] The thickness of the sealing layer 4 is preferably 1 μm to 20 μm, more preferably 3 to 8 μm. The width W of the sealing layer 4 is preferably 50 to 2000 μm, more preferably 100 to 1000 μm.

[0068] Component 5 is mounted on the first main surface 2a of the first substrate 2. Furthermore, component 5 is disposed within the space (cavity) defined by the first main surface 2a of the first substrate 2, the first main surface 3a of the second substrate 3, and the sealing layer 4. Various components, such as deep ultraviolet LEDs (Light Emitting Diodes), MEMS (Micro Electro Mechanical Systems) components, and CCD (Charge Coupled Device) components, can be used as component 5.

[0069] Figures 4 to 12 The manufacturing apparatus 7 for the joint 1 is shown. (Example) Figure 4As shown, the manufacturing apparatus 7 includes: a support device 8 that supports a laminate LM, which is formed by laminating a first substrate 2 and a second substrate 3 with a sealing material 6 in between; and a laser irradiation device 9 that forms a sealing layer 4 by irradiating the sealing material 6 of the laminate LM with a laser L.

[0070] like Figures 4 to 9 As shown, the support device 8 includes: a support member 10 that supports the laminate LM; a pressing member 11 that presses the laminate LM; a base member 12 that supports the pressing member 11; a fixing mechanism 13 that fixes the support member 10 to the base member 12; a frame 14 that fixes the pressing member 11 to the base member 12; a sealing member 15 disposed between the pressing member 11 and the base member 12; a receiving space 16 for the laminate LM that is formed between the pressing member 11 and the base member 12; and a pressure adjusting device 17 that adjusts the pressure of the receiving space 16.

[0071] The support member 10 is disposed together with the laminate LM in the receiving space 16. The support member 10 is, for example, made of metal (stainless steel, etc.) and is constructed of a circular plate member (see reference). Figure 7 The material and shape of the support member 10 are not limited to this embodiment. The support member 10 has a first surface 10a and a second surface 10b located on the opposite side of the first surface 10a. The first surface 10a has a receiving portion 18 for receiving the laminated body LM. In this embodiment, the receiving portion 18 is composed of a recess capable of receiving the laminated body LM, but the structure of the receiving portion 18 is not particularly limited as long as it can position the laminated body LM. For example, multiple positioning protrusions can be provided on the first surface 10a of the support member 10, and the space inside it can be used as the receiving portion 18.

[0072] like Figure 8 As shown, the pressing member 11 is, for example, a circular transparent glass plate. The thickness of the pressing member 11 is preferably 3 to 10 mm. The Young's modulus of the pressing member 11 is preferably 50 to 80 GPa, more preferably 60 to 70 GPa. Thus, in the pressing process described later, the pressing member can appropriately press the laminate using moderate flexural force. The pressing member 11 has a first surface 11a that contacts the sealing member 15 and the laminate LM, and a second surface 11b that contacts the frame 14.

[0073] The base member 12 is made of metal (e.g., stainless steel), but may also be made of other materials. The base member 12 has walls 19 for forming the receiving space 16 and a bottom 20.

[0074] Figure 5A top view of a base member 12 to which a support member 10 is fixed by a fixing mechanism 13 is shown. The wall portion 19 of the base member 12 is cylindrical, but is not limited to this shape. A support portion 21 for mounting a sealing member 15 is formed at the midpoint of the inner side of the wall portion 19. The support portion 21 is the surface opposite to the pressing member 11 mounted on the base member 12. A top-view annular groove 21a for mounting the sealing member 15 is formed in the support portion 21.

[0075] like Figure 4 as well as Figure 5 As shown, the wall portion 19 has an end face 19a (upper surface), inner peripheral faces 19b and 19c, and an outer peripheral face 19d.

[0076] The frame 14 is fixed to the end face 19a of the wall portion 19 by means of a fixing member 22. The fixing member 22 is composed of, for example, a bolt or screw member, and has a head 22a and a shaft portion 22b. A plurality of threaded holes 23 are formed on the end face 19a for engaging with the shaft portion 22b of the fixing member 22.

[0077] The inner peripheral surfaces 19b and 19c of the wall portion 19 include: a first inner peripheral surface 19b, which functions as a guide surface for guiding the pressing member 11 toward the support portion 21; and a second inner peripheral surface 19c, through which the support member 10 can pass. The diameter of the first inner peripheral surface 19b is larger than the diameter of the pressing member 11. The diameter of the second inner peripheral surface 19c is larger than the diameter of the support member 10.

[0078] The bottom 20 of the base member 12 is formed on the inner side of the cylindrical wall 19. The bottom 20 is composed of a circular surface when viewed from above.

[0079] like Figures 4 to 6 As shown, the fixing mechanism 13 includes: an elastic member 24 that supports the support member 10; a fixing member 25 that fixes the support member 10 to the base member 12; an insertion hole 26 formed in the support member 10 and allowing a portion of the fixing member 25 to pass through; a locking recess 27 formed in the support member 10 and locking a portion of the fixing member 25; and a guide groove 28 formed in the support member 10 and allowing the fixing member 25 to move relative to each other between the insertion hole 26 and the locking recess 27.

[0080] An elastic member 24 is mounted on the bottom 20 of the base member 12. Multiple elastic members 24 are disposed on the bottom 20. The elastic member 24 is, for example, a compression coil spring, but is not limited thereto; it may also be made of other springs, rubber, or other materials. Multiple mounting recesses 29 are formed on the bottom 20 to accommodate a portion of the elastic member 24. One end of the elastic member 24 is inserted into the mounting recess 29, and the other end of the elastic member 24 protrudes from the bottom 20. The elastic member 24 has the function of applying force to the support member 10 under the action of its elastic restoring force.

[0081] The fixing member 25 is composed of, for example, bolts or screws, and has a head 25a and a shaft portion 25b. The head 25a has a larger diameter than the shaft portion 25b. The shaft portion 25b has an external thread 30. The shaft portion 25b is fixed to the bottom 20 of the base member 12. A threaded hole 31 is formed in the bottom 20 of the base member 12 for the shaft portion 25b to be inserted.

[0082] like Figure 7 As shown, the through hole 26 is circular in top view, but is not limited to this shape. The through hole 26 has a diameter larger than that of the head 25a, so that the head 25a and the shaft portion 25b of the fixing member 25 can pass through.

[0083] The locking recess 27 has a sidewall surface 27a into which the head 25a of the fixing member 25 can be inserted, and a bottom surface 27b into which the head 25a is locked. The sidewall surface 27a is circular in plan view, but is not limited to this shape. The sidewall surface 27a has a diameter larger than that of the head 25a to avoid contact with the head 25a of the fixing member 25. The bottom surface 27b is configured to contact the head 25a.

[0084] The guide groove 28 extends through the support member 10 along its thickness direction so that the shaft portion 25b of the fixing member 25 passes through it. The guide groove 28 is connected to the bottom surface 27b of the insertion hole 26 and the locking recess 27 of the fixing member 25 such that the shaft portion 25b of the fixing member 25 can move relative to it between the insertion hole 26 and the locking recess 27. Specifically, one end of the guide groove 28 communicates with the inner circumferential surface of the insertion hole 26. The other end of the guide groove 28 is located at the center of the bottom surface 27b of the locking recess 27.

[0085] The guide groove 28 is configured as an arc or a straight line when viewed from above. By rotating the support member 10 about its center, the guide groove 28 allows the shaft portion 25b of the fixing member 25 to move relative to each other between the through hole 26 and the locking recess 27.

[0086] like Figure 9As shown, the frame 14 is a plate-shaped member configured as a ring when viewed from above. The frame 14 is fixed to the end face 19a of the wall portion 19 of the base member 12 by the fixing member 22. The frame 14 includes: a through hole 32 through which the shaft portion 22b of the fixing member 22 passes; a locking recess 33 that receives the head 22a of the fixing member 22; a cylindrical portion 34; and an opening 35.

[0087] like Figure 4 as well as Figure 9 As shown, the insertion holes 32 and locking recesses 33 are concentric in plan view. Multiple insertion holes 32 and locking recesses 33 are formed in the frame 14. The cylindrical portion 34 is cylindrical in shape, corresponding to the shape of the wall portion 19 of the base member 12. The diameter of the inner circumferential surface of the cylindrical portion 34 is larger than the diameter of the outer circumferential surface 19d of the wall portion 19 of the base member 12. The opening portion 35 is circular in plan view. The diameter of the opening portion 35 is smaller than the diameter of the pressing member 11.

[0088] The sealing member 15 is made of an elastic component such as rubber (e.g., an O-ring). Figure 4 as well as Figure 5 As shown, the sealing member 15 is disposed in the annular groove 21a formed in the support portion 21 of the base member 12. The sealing member 15 seals the receiving space 16 by being in close contact with the pressing member 11.

[0089] like Figure 8 As shown, the sealing member 15 is configured to form a circular surrounding laminate LM between the pressing member 11 and the base member 12. The diameter of the circular shape of the sealing member 15 is smaller than the diameter of the pressing member 11 and larger than the diameter of the support member 10.

[0090] The receiving space 16 of the laminate LM is a space formed by the pressing member 11, the base member 12, and the sealing member 15. The receiving space 16 is airtight by tightly pressing the pressing member 11 against the sealing member 15 mounted on the support portion 21 of the base member 12. The receiving space 16 can accommodate the laminate LM, the support member 10, and the fixing mechanism 13.

[0091] like Figure 4 As shown, the air pressure regulating device 17 mainly comprises: a flow path 36 formed in the base member 12, which allows gas to flow out of the receiving space 16; a pipe 37 connected to the flow path 36; a regulating valve 38 disposed in the middle of the pipe 37; and a pump 39. The flow path 36 includes a suction port 36a formed in the bottom 20 of the base member 12 and an exhaust port 36b formed on the outer surface of the base member 12. The air pressure regulating device 17 uses the pump 39 to draw air from the receiving space 16, thereby reducing the air pressure in the receiving space 16 and making the receiving space 16 a negative pressure relative to the atmosphere.

[0092] As the laser irradiation device 9, it is suitable to use a laser irradiation device that irradiates semiconductor lasers, but it is not limited to this. It can also use devices that irradiate various lasers such as YAG lasers, green lasers, and ultrashort pulse lasers.

[0093] The following describes the method of fixing the support member 10 to the base member 12 using the fixing mechanism 13. First, as Figure 10 As shown, with the shaft portion 25b of the fixing member 25 installed into the threaded hole 31 of the base member 12, the support member 10 is brought closer to the base member 12 from above. Then, while lowering the support member 10, as... Figure 11 as well as Figure 12 As shown, the through hole 26 passes through the head 25a and shaft 25b of the fixing member 25. In this case, the upper end of the elastic member 24 mounted on the base member 12 contacts the second surface 10b of the support member 10.

[0094] Then, the head 25a of the fixed component 25 is as follows Figure 12 As shown, the support member 10 protrudes from its first surface 10a and is pressed against the elastic member 24. The elastic member 24 contracts while elastically deforming. As a result, the elastic member 24 generates an elastic restoring force that overcomes the force pressing on the support member 10.

[0095] Next, while maintaining the head's 25a protrusion, as in Figure 11 As indicated by the arrow, the support member 10 is rotated counterclockwise when viewed from above. This causes the shaft portion 25b, passing through the through hole 26, to move relative to the locking recess 27 via the guide groove 28. Figure 12 As shown by the double-dotted line, the head 25a of the fixing member 25, which moves relative to the locking recess 27 via the guide groove 28, is located above the locking recess 27.

[0096] Subsequently, when the force pressing the support member 10 against the elastic member 24 is released, the support member 10 is pushed up under the force of the elastic member 24. As a result, the head 25a of the fixing member 25 enters the locking recess 27. The locking recess 27 contacts the head 25a through its bottom surface 27b, thereby locking it against the fixing member 25. It is desirable that in this state, the elastic member 24 does not return to its free length, but continues to exert force on the support member 10 under the action of its elastic restoring force.

[0097] The force exerted by the elastic member 24 on the support member 10 causes the fixing member 25 to rotate about its axis and change the position of the head 25a in the axial direction, thereby enabling adjustment. In order to enable this position adjustment, the end of the shaft portion 25b of the fixing member 25 is preferably not located at the bottom of the threaded hole 31 formed in the base member 12, but at the middle of the threaded hole 31.

[0098] When the support member 10 is removed from the base member 12, the support member 10 is pressed against the elastic member 24, causing the elastic member 24 to contract, and the support member 10 is moved downwards such that the head 25a of the fixing member 25 protrudes from the locking recess 27. Then, the support member 10 is rotated clockwise in plan view. As a result, the shaft portion 25b of the fixing member 25 engages with the guide groove 28. Then, through the relative movement of the support member 10 and the fixing member 25, the shaft portion 25b is positioned in the through hole 26.

[0099] Next, the support member 10 is lifted by means of the head 25a of the fixing member 25 from the first surface 10a side toward the second surface 10b side through the through hole 26. As a result, the support member 10 is removed from the base member 12.

[0100] As described above, the support member 10 can be easily installed or removed from the base member 12 using the fixing mechanism 13. Furthermore, by adjusting the position of the fixing member 25 relative to the threaded hole 31, the fixing position of the support member 10 can be adjusted according to the thickness of the laminate LM.

[0101] The following is for reference Figures 13 to 17 The method for manufacturing the assembly 1 using the manufacturing apparatus 7 with the above-described structure will be described. For example... Figure 13 As shown, this method includes a lamination process S1 and a bonding process S2.

[0102] like Figure 14 As shown, in the lamination process S1, firstly, the first substrate 2 and the second substrate 3 are overlapped with their first main surface 2a facing each other. It should be noted that an element 5 is pre-installed on the first main surface 2a of the first substrate 2. The first substrate 2 and the second substrate 3 are then laminated with the element 5 located inside the sealing material 6 to form a laminate LM.

[0103] like Figure 15 As shown, the joining process S2 includes a supporting process S21, a pressing process S22, and a laser irradiation process S23.

[0104] In the supporting process S21, the laminated body LM formed by the lamination process S1 is assembled onto the supporting device 8. That is, as shown in the figure. Figure 16As shown, firstly, the laminate LM is housed in the receiving portion 18 of the base member 12 supporting the member 10, which is mounted by the fixing mechanism 13.

[0105] like Figure 17 As shown, the thickness dimension TLM of the laminate LM is preferably larger than the depth dimension D of the receiving portion 18. The laminate LM is received in the receiving portion 18 such that a portion of the thickness direction of the second substrate 3 extends from the receiving portion 18 toward the pressing member 11. The dimension PD1 of the portion of the thickness direction of the second substrate 3 extending from the recess is preferably 0.05 to 0.95 times the thickness dimension T of the second substrate 3 (0.05T≤PD1≤0.95T).

[0106] Next, the pressing member 11 is placed on the sealing member 15 mounted on the support portion 21 of the base member 12. Thus, the first surface 11a of the pressing member 11 contacts the sealing member 15. In this case, it is preferable that the pressing member 11, the sealing member 15, and the laminate LM are arranged concentrically. Alternatively, in this state, the first surface 11a of the pressing member 11 may also contact the second main surface 3b of the second substrate 3 in the laminate LM.

[0107] Next, the frame 14 is placed on the end face 19a of the wall portion 19 in the base member 12, and the frame 14 is fixed to the wall portion 19 using the fixing member 22. That is, the through hole 32 of the frame 14 is aligned with the threaded hole 23 of the wall portion 19 of the base member 12, and after the shaft portion 22b of the fixing member 22 is passed through the through hole 32, the shaft portion 22b is engaged with the threaded hole 23, and the fixing member 22 is tightened. In this state, the frame 14 and the sealing member 15 together hold the pressing member 11. In addition, the opening 35 of the frame 14 exposes a portion of the second surface 11b of the pressing member 11 toward the laser irradiation device 9. Thus, the assembly of the laminate LM to the support device 8 is completed. Thus, the laminate LM is housed together with the support member 10 in the receiving space 16.

[0108] It should be noted that, alternatively, in the support process S21, dry air may be filled into the receiving space 16, for example. Dry air refers to a gas that has had moisture removed through a drying process, meaning a gas that does not produce water even when the pressure changes. As dry air, for example, a gas obtained by drying the gas in the environment in which the manufacturing apparatus 7 is located, or high-purity nitrogen gas, may be used.

[0109] For example, preferably, the support device 8 is arranged in a working space filled with dry air, and the above-described support process S21 is performed in the working space, thereby filling the receiving space 16 with dry air. As a result, not only the receiving space 16, but also the space between the first substrate 2 and the second substrate 3 in the laminate LM and inside the sealing material 6 (the receiving space of the element 5) is filled with dry air.

[0110] In the subsequent pressing step S22, the pump 39 draws the gas in the receiving space 16 through the flow path 36 of the pressure adjusting device 17 and discharges it to the outside. This reduces the air pressure in the receiving space 16, creating a negative pressure relative to the atmosphere. Under this negative pressure, the first surface 11a of the pressing member 11 is pressed tightly against the sealing member 15, pressing the second substrate 3 of the laminate LM. It should be noted that in the pressing step S22, the pressure within the receiving space 16 can be adjusted by operating the adjusting valve 38. The air pressure in the receiving space 16 is preferably 100–95000 Pa, more preferably 1000–85000 Pa.

[0111] Preferably, in the pressing process S22, the pressing member 11 flexes in a manner that presses the laminate LM due to the negative pressure of the receiving space 16 relative to the atmosphere.

[0112] like Figure 4 As shown, in the laser irradiation step S23, the sealing material 6 of the laminate LM is irradiated with laser L from the laser irradiation device 9, thereby heating the sealing material 6 (heating step). Laser L irradiates the sealing material 6 through the pressing member 11 and the second substrate 3. In the bonding step S2, the sealing material 6 is heated to a temperature above its softening point or at its softening flow temperature under the irradiation of laser L. Laser L irradiates in a manner that surrounds the closed curve of the sealing material 6.

[0113] The wavelength of laser L is preferably 600–1600 nm. Semiconductor lasers are suitable for use, but are not limited to this; various lasers such as YAG lasers, green lasers, and ultrashort pulse lasers can also be used.

[0114] Heating is performed using laser L, which softens and flows the sealing material 6, followed by curing. This forms a sealing layer 4 that hermetically bonds the first substrate 2 and the second substrate 3. Through the above process, a bonded body 1 comprising the first substrate 2, the second substrate 3, and the sealing layer 4 is manufactured. The bonded body 1 is removed from the support member 10 after the frame 14 and the pressing member 11 are removed from the base member 12.

[0115] According to the manufacturing method and manufacturing apparatus 7 of the assembly 1 of this embodiment described above, the pressing member 11 of the support device 8 is configured as circular, and the sealing member 15 is configured to surround the laminate LM in a circular shape between the pressing member 11 and the base member 12. This minimizes uneven pressing pressure of the pressing member 11 on the laminate LM compared to cases where the pressing member (clamp body cover) and the sealing member (backing member) are quadrilateral. Consequently, poor bonding caused by insufficient adhesion between the sealing material 6 in the laminate LM and each substrate 2, 3 can be reduced.

[0116] Figures 18 to 22 The second embodiment of the present invention is shown. In this embodiment, the structure of the laminate LM and the structure of the support device 8 of the manufacturing apparatus 7 are different from those of the first embodiment.

[0117] like Figure 18 As shown, the pressing member 11 of the support device 8 has a protrusion 40 that is inserted into the receiving portion 18 of the support member 10. The protrusion 40 is formed on the first surface 11a of the pressing member 11. The protrusion 40 is cylindrical, but is not limited to this shape. The protrusion dimension PD2 of the protrusion 40 is smaller than the depth dimension D of the receiving portion 18 (see reference). Figure 21 The protrusion 40 has a pressing surface 41 that contacts the second main surface 3b of the second substrate 3 of the laminate LM.

[0118] like Figure 19 As shown, the support member 10 of the support device 8 has a receiving portion 18 that is circular in top view. The laminate LM is configured to be circular in top view (not shown) to engage with the receiving portion 18. That is, the first substrate 2 and the second substrate 3 of the laminate LM are configured as circular plates.

[0119] like Figures 18 to 22 As shown, the fixing mechanism 13, in addition to the elastic member 24 and fixing member 25 identical to those in the first embodiment, also has an insertion hole 26 and a locking recess 27 formed in the support member 10. It should be noted that the support member 10 in this embodiment does not have the guide groove 28 found in the first embodiment.

[0120] The diameter of the through hole 26 is larger than the diameter of the shaft portion 25b of the fixing member 25, but smaller than the diameter of the head 25a. Therefore, the through hole 26 allows the shaft portion 25b of the fixing member 25 to pass through, but the head 25a cannot pass through.

[0121] The locking recess 27, like in the first embodiment, has a side wall surface 27a that is circular when viewed from above and a bottom surface 27b that locks the head 25a of the fixing member 25. The locking recess 27 and the through hole 26 are concentric when viewed from above.

[0122] In this embodiment, the support member 10 is installed on the base member 12 as follows. First, as... Figure 20 As shown, with the fixing member 25 of the fixing mechanism 13 removed from the threaded hole 31 of the base member 12, the support member 10 is placed on the elastic member 24 installed on the base member 12.

[0123] Next, from a top view, align the through hole 26 of the support member 10 with the threaded hole 31 of the base member 12, and pass the shaft portion 25b of the fixing member 25 through the through hole 26. Then, engage the shaft portion 25b with the threaded hole 31. This brings the head 25a of the fixing member 25 into contact with the bottom surface 27b of the locking recess 27, thus locking the support member 10. Through these steps, the support member 10 is fixed to the base member 12 by the fixing mechanism 13.

[0124] like Figure 18 , Figure 21 as well as Figure 22 As shown, the support device 8 includes an adjustment plate 42 that engages with the receiving portion 18. In this embodiment, one adjustment plate 42 is shown, but multiple adjustment plates 42 may also be used. The adjustment plate 42 is made of, for example, a circular glass plate or a metal plate. The adjustment plate 42 is placed on the bottom of the receiving portion 18 to adjust the depth of the receiving portion 18. Not limited to this usage, the adjustment plate 42 may also be made of transparent glass and used to overlap with the second main surface 3b of the second substrate 3 in the laminate LM received in the receiving portion 18.

[0125] The fixing mechanism 13 and the adjusting plate 42 of this embodiment can also be used in the support device 8 of the first embodiment.

[0126] The following describes the differences between the manufacturing method of the joint in this embodiment and that in the first embodiment. For example... Figure 21 As shown, in the manufacturing method of the joint in this embodiment, in the support process S21, the adjustment plate 42 is housed in the housing portion 18 of the support member 10, and then the laminate LM is housed in the housing portion 18.

[0127] like Figure 22 As shown, the depth dimension D of the receiving portion 18 in this embodiment is larger than the thickness dimension TLM of the laminate LM. Therefore, the laminate LM is not a part of the second substrate 3 that extends out from the receiving portion 18, but is entirely received within the receiving portion 18.

[0128] Next, the pressing member 11 is placed on the sealing member 15 mounted on the base member 12. At this time, the protrusion 40 of the pressing member 11 is inserted into the receiving portion 18 of the support member 10. The pressing surface 41 of the protrusion 40 contacts the second main surface 3b of the second substrate 3 housed in the laminate LM housed in the receiving portion 18.

[0129] In the pressing process S22, the pressing surface 41 presses the second substrate 3 of the laminate LM. In the subsequent laser irradiation process S23, the laser L passes through the protrusion 40 of the pressing member 11 and the second substrate 3 of the laminate LM to irradiate the sealing material 6.

[0130] The other structures in this embodiment are the same as in the first embodiment. Common reference numerals are used to label the components that are the same in this embodiment as in the first embodiment.

[0131] It should be noted that the present invention is not limited to the structure of the above-described embodiments, nor is it limited to the effects described above. Various modifications can be made to the present invention without departing from its spirit.

[0132] Explanation of reference numerals in the attached figures

[0133] 1. Connector

[0134] 2 First substrate

[0135] 3 Second substrate

[0136] 4 Sealing Layer

[0137] 6. Sealing materials

[0138] 8 Support device

[0139] 10 Supporting components

[0140] 11 Pressing Components

[0141] 12 Base components

[0142] 15 Sealing components

[0143] 16 Containment Space

[0144] 17. Air pressure regulating device

[0145] 18 Containment Department

[0146] L laser

[0147] LM stack

[0148] The dimension of a portion of the thickness direction of the second substrate of PD1 protruding from the receiving portion.

[0149] S1 Lamination Process

[0150] S2 Joining Process

[0151] S21 Support process

[0152] S22 Pressing Process

[0153] S23 Laser irradiation process.

Claims

1. A method for manufacturing a bond, comprising manufacturing a bond having a first substrate, a second substrate, and a sealing layer for bonding the first substrate and the second substrate, The method for manufacturing the joint is characterized in that... The method for manufacturing the joint includes: In the lamination process, a sealing material is sandwiched between the first substrate and the second substrate, and the first substrate and the second substrate are overlapped to form a laminate. The bonding process involves irradiating the sealing material in the laminate with a laser to form the sealing layer. The joining process includes: a supporting process, assembling the laminate onto a supporting device; a pressing process, pressing the laminate; and a laser irradiation process, irradiating the sealing material with laser light. The support device includes: a pressing member that presses the laminated body; a base member that supports the pressing member; a sealing member disposed between the pressing member and the base member; a receiving space for the laminated body formed between the pressing member and the base member; a pressure adjusting device that adjusts the pressure of the receiving space; a support member that supports the laminated body within the receiving space; and a fixing mechanism that fixes the support member to the base member. The pressing member is a circular, transparent glass plate. The sealing member is configured to circularly surround the laminate between the pressing member and the base member. In the pressing process, the air pressure is reduced in the receiving space using the air pressure adjusting device, thereby causing the pressing member to adhere tightly to the sealing member, and the pressing member is used to press the laminate. The fixing mechanism includes: a fixing member having a head and a shaft portion; a locking recess formed in the support member and locking the head of the fixing member; and an elastic member disposed in the base member and supporting the support member. The support member has a surface that contacts the elastic member of the base member. The fixing mechanism, with the fixing member engaged with the base member, causes the fixing member to rotate around its axis and changes the position of the head in the axial direction of the fixing member, thereby adjusting the force exerted by the elastic member on the support member.

2. The method for manufacturing the joint according to claim 1, wherein, The support member has a receiving portion for accommodating the laminated body. In the supporting process, the first substrate is housed in the housing portion, and the second substrate is housed in the housing portion such that a portion of the thickness direction of the second substrate extends from the housing portion toward the pressing member.

3. The method for manufacturing the joint according to claim 2, wherein, A portion of the second substrate extending from the receiving portion in the thickness direction is 0.05 to 0.95 times the thickness of the second substrate.

4. The method for manufacturing the joint according to any one of claims 1 to 3, wherein, The air pressure of the containment space is set to 100-95000 Pa.

5. The method for manufacturing the joint according to any one of claims 1 to 3, wherein, The thickness of the pressing component is 3 to 10 mm.

6. The method for manufacturing the joint according to any one of claims 1 to 3, wherein, The Young's modulus of the pressing component is 50-80 GPa.

7. The method for manufacturing the joint according to any one of claims 1 to 3, wherein, In the supporting process, dry air is filled into the receiving space.

8. A method for manufacturing a joint according to any one of claims 1 to 3, wherein, The first substrate is a high thermal conductivity substrate, and the second substrate is a glass substrate.

9. A manufacturing apparatus for a bond, comprising manufacturing a bond having a first substrate, a second substrate, and an sealing layer for bonding the first substrate and the second substrate. The manufacturing apparatus for the assembly is characterized in that... The apparatus for manufacturing the bond comprises: a support device that supports a laminate, the laminate being formed by sandwiching a sealing material between a first substrate and a second substrate and overlapping the first substrate and the second substrate; and a laser irradiation device that irradiates the sealing material in the laminate with a laser to form the sealing layer. The support device includes: a pressing member that presses the laminate; a base member that supports the pressing member; a sealing member disposed between the pressing member and the base member; a receiving space for the laminate formed between the pressing member and the base member; and a pressure adjusting device that adjusts the pressure of the receiving space. A support member that supports the laminate within the receiving space; and a fixing mechanism that secures the support member to the base member. The pressing member is a circular, transparent glass plate. The sealing member is configured to circularly surround the laminate between the pressing member and the base member. The manufacturing apparatus for the joint is configured to reduce the air pressure in the receiving space using the air pressure adjustment device, thereby causing the pressing member to adhere tightly to the sealing member, and pressing the laminate using the pressing member. The fixing mechanism includes: A fixing member having a head and a shaft portion; a locking recess formed in the supporting member and locking the head of the fixing member; And an elastic member, which is disposed on the base member and supports the support member. The support member has a surface that contacts the elastic member of the base member. The fixing mechanism is configured such that, with the fixing member engaged with the base member, the fixing member rotates around its axis and changes the position of the head in the axial direction of the fixing member, thereby adjusting the force exerted by the elastic member on the support member.

Citation Information

Patent Citations

  • Device for producing and method for producing laminate body

    CN104093569A

  • Method and device for producing joint body

    JP2021031306A

  • Bonded body manufacturing method and bonded body manufacturing device

    JP2021062983A

  • Airtight package manufacturing method and airtight package

    WO2017199491A1