Coated cutting tool
By depositing α-Al₂O₃ and Ti(C,N) layers with specific orientations on cutting tools, and adjusting the grain size and orientation, the problem of insufficient wear resistance of coated cutting tools during steel cutting is solved, achieving high wear resistance and long service life.
Patent Information
- Application Number
- CN202280036994.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-27
- Filing Date
- 2022-05-25
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-05-25
AI Technical Summary
Existing coated cutting tools have insufficient wear resistance during metal cutting of steel, especially in terms of flank wear and crater wear.
By depositing α-Al₂O₃ and Ti(C,N) layers with specific orientations on cutting tools, adjusting the grain size and orientation of the Ti(C,N) layer, and combining the layer thickness and texture coefficient, the adhesion and orientation degree of the coating can be improved.
It significantly improves the wear resistance of cutting tools, especially in the metal cutting process of steel, extending tool life and reducing wear on the flank face and crater.
Smart Images

Figure CN117355636B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a coated cutting tool comprising a substrate and a coating, wherein the coating is deposited by CVD and comprises a Ti(C,N) layer and an α-Al2O3 layer. Background Technology
[0002] Coated cutting tools are well-known in the metal cutting industry. CVD-coated and PVD-coated cutting tools are the two most common types. These coatings offer advantages such as high chemical resistance and high wear resistance, which are important for achieving long tool life. CVD coatings containing Ti(C,N) layers as well as alumina layers are known to perform well in, for example, the turning or milling of steel.
[0003] EP3034653A1 discloses a coated cutting tool with a wear-resistant coating comprising a 001 oriented α-Al2O3 layer.
[0004] One object of the present invention is to provide a coated cutting tool for metal cutting, the coated cutting tool having very high wear resistance, especially improving resistance to flank wear and crater wear during metal cutting of steel. Summary of the Invention
[0005] At least one of the above objectives is achieved by the cutting tool according to item 1. Preferred embodiments are disclosed in the dependent items.
[0006] This invention relates to a cutting tool comprising a substrate at least partially coated with a coating comprising an α-Al₂O₃ layer, wherein the α-Al₂O₃ layer comprises an O₁ portion extending 1 μm from a bonding layer, wherein the O₁ portion exhibits an orientation such that, when measured using electron backscatter diffraction (EBSD) on a cross-section of the α-Al₂O₃ layer, ≥80%, preferably ≥90%, more preferably ≥95%, and most preferably ≥97% of the analytical region has an orientation within 15 degrees of the surface normal of the α-Al₂O₃ layer. <001> The direction, wherein the surface normal of the α-Al2O3 layer is parallel to the surface normal of the substrate surface.
[0007] This high orientation of the α-Al2O3 layer in the O1 region, that is, in the lowermost part of the α-Al2O3 layer adjacent to the bonding layer, has shown unexpected advantages in improving resistance to primary and secondary flank wear and crater wear during steel turning.
[0008] In one embodiment of the invention, the cutting tool comprises a substrate at least partially coated with a coating comprising a Ti(C,N) layer, an α-Al₂O₃ layer, and a bonding layer therebetween, wherein the Ti(C,N) layer, with a thickness of 3-25 μm, is composed of columnar grains, wherein the average grain size D of the Ti(C,N) layer, as measured by X-ray diffraction using CuKα radiation, is... 422 The grain size D is 25-50 nm. 422 It is calculated based on the Scherrer formula from the full width at half maximum (FWHM) of peak (422):
[0009]
[0010] Where D 422 Where is the average grain size of the Ti(C,N), K is the shape factor and is set to 0.9 here, and λ is the wavelength of CuKα radiation and is set to . B 422 The (422) is the FWHM value of the reflection, θ is the Bragg angle, wherein the Ti(C,N) layer includes a B1 portion adjacent to the bonding layer, and wherein the average grain size of the Ti(C,N) grains in the B1 portion is greater than the average grain size D of the entire Ti(C,N) layer. 422 In the B1 portion of the Ti(C,N) layer, the average grain size of the Ti(C,N) grains is 130-165 nm when measured using TKD (transmission Kikuchi diffraction) in a 5×5 μm analytical region on a planar view extending parallel to the substrate surface.
[0011] In one embodiment of the invention, this increased orientation in the lower portion of the α-Al₂O₃ layer is achieved by altering the deposition process conditions at the end of the Ti(C,N) deposition, causing some fine Ti(C,N) grains to widen and form coarser-grained Ti(C,N) portions. Subsequently, the process conditions are altered again, this time to provide an optimal outer surface for the Ti(C,N) grains. In this way, the outermost surface of the formed Ti(C,N) is similar to the outermost surface of the coarse-grained Ti(C,N), which is known to be a promising layer deposited onto the α-Al₂O₃ layer prior to the bonding layer. If the average grain size in the B1 portion is too small, the adhesion of the subsequently deposited α-Al₂O₃ layer will not increase. If the average grain size in the B1 portion is too large, the orientation of the subsequent α-Al₂O₃ will decrease.
[0012] Due to limited resolution, it is difficult to study the grain size of very fine-grained Ti(C,N) in SEM. Therefore, the average grain size of the fine-grained portion of the Ti(C,N) layer is instead defined via XRD and the Scherrer equation. Although the signal from XRD also includes information from the coarser-grained Ti(C,N)B1 portion, this contribution is considered limited.
[0013] On the other hand, the challenge in studying the grain size in the coarse-grained B1 portion is that it is only a part of the Ti(C,N) layer, thus requiring the selection of a very high-precision method. The planar view study using TKD was chosen because the information obtained includes both information about the grain size and information about the Ti(C,N) grain orientation at a very local scale.
[0014] In one embodiment of the invention, the layer, wherein the α-Al2O3 layer exhibits a texture coefficient TC(hkl) as defined by the Harris formula, measured by X-ray diffraction using CuKα radiation and θ-2θ scanning:
[0015]
[0016] Where I(hkl) is the measured intensity (integrated area) of the (hkl) reflection, I0(hkl) is the standard intensity according to ICDD PDF card No. 00-010-0173, n is the number of reflections used in the calculation, and the (hkl) reflections used are (1 0 4), (1 1 0), (1 1 3), (0 2 4), (11 6), (2 1 4), (3 0 0) and (0 0 12), characterized in that TC(0 0 12)≥7.5, preferably≥7.7, more preferably≥7.8.
[0017] In one embodiment of the invention, the layer, wherein the α-Al2O3 layer exhibits TC(110)≤0.2, preferably≤0.1.
[0018] In one embodiment of the present invention, the Al2O3 layer is an α-Al2O3 layer, preferably with an average thickness of 1 μm-15 μm, more preferably 3-10 μm.
[0019] In one embodiment of the invention, when measured using TKD in a planar view of the Ti(C,N) layer extending parallel to the substrate surface, over a region of at least 5 × 5 μm, the Ti(C,N) layer in the B1 portion of the Ti(C,N) layer exhibits an orientation in which ≥93%, preferably ≥95%, of the analytical region has an angle of less than 15 degrees with the surface normal of the Ti(C,N) layer. <211> The direction, wherein the surface normal of the Ti(C,N) layer is parallel to the surface normal of the substrate surface.
[0020] The Ti(C,N) layer is closest to the bonding layer and thus also closest to the α-Al2O3 layer, having a lateral... <211> Highly oriented portions are considered advantageous in attempting to deposit highly 001 oriented α-Al₂O₃ layers. If less than 93% of the analyzed region has a surface normal to the Ti(C,N) layer within 15 degrees, this is also beneficial. <211> If the orientation is not clear, then the 001 orientation of the subsequent α-Al2O3 layer will be less obvious.
[0021] In one embodiment of the present invention, the thickness of the B1 portion of the Ti(C,N) layer, measured in the growth direction of the coating, is 0.5-1.5 μm, preferably 0.6-0.9 μm, and most preferably 0.6-0.8 μm.
[0022] Fine-grained Ti(C,N) is advantageous as a wear-resistant layer, likely due to its abundant grain boundaries or because the layer's thickness is smoother or more uniform. Therefore, the fine-grained portion of the TiCN layer should be relatively thick. The coarse-grained portion, which contributes to increased adhesion and orientation, should be relatively limited, with the thickness of the B1 portion preferably being 0.5-1.5 μm, more preferably 0.6-0.9 μm, and most preferably 0.6-0.8 μm. If the B1 portion is too thin, adhesion and / or orientation will not be enhanced.
[0023] In one embodiment of the invention, the Ti(C,N) layer exhibits an X-ray diffraction pattern measured using CuKα radiation and θ-2θ scanning, where TC(hkl) is defined according to the Harris formula, where I(hkl) is the measured intensity (integral area) of the (hkl) reflection, I0(hkl) is the standard intensity according to ICDD PDF card No. 42-1489, n is the number of reflections, and the reflections used in the calculation are (1 1 1), (2 0 0), (2 2 0), (3 1 1), (3 3 1), (4 2 0), and (4 22), where TC(422) ≥ 3, preferably ≥ 4.
[0024] In one embodiment of the present invention, the grain size D of Ti(C,N) is... 422The size is 25-40 nm, preferably 25-35 nm. The increased adhesion between the fine-grained Ti(C,N) and the α-Al₂O₃ layer is beneficial for Ti(C,N) layers with very fine grains, for example, when the grain size D of Ti(C,N) is... 422 It is particularly advantageous when the wavelength is 25-40nm or even 25-35nm.
[0025] In one embodiment of the present invention, the average thickness of the Ti(C,N) layer is 4-20 μm, preferably 5-15 μm.
[0026] In one embodiment of the invention, the bonding layer comprises at least one compound selected from titanium carbon oxides, titanium nitrides, and titanium carbon oxynitrides.
[0027] The advantage of a bonding layer of titanium carbon oxide, titanium nitride, or titanium carbon oxynitride is that it can provide an epitaxial relationship between the Ti(C,N) layer and the α-Al2O3 layer.
[0028] In one embodiment of the present invention, the average thickness of the bonding layer is 0.25-2.5 μm, preferably 0.5-2.0 μm.
[0029] In one embodiment of the present invention, the average thickness of the coating is 5.0 μm-30.0 μm, preferably 10-20 μm.
[0030] In one embodiment of the present invention, the substrate is a cemented carbide, a cermet, or a ceramic.
[0031] The atomic ratio of carbon to the sum of carbon and nitrogen (C / (C+N)) in the Ti(C,N) layer of the present invention (measured by electron microprobe analysis) is preferably 0.50-0.65, more preferably 0.55-0.62.
[0032] Other objects and features of the invention will become apparent from the following definitions and embodiments considered in conjunction with the accompanying drawings.
[0033] definition
[0034] The term "cutting tool" in this document is intended to refer to cutting tools suitable for metal cutting applications, such as inserts, end mills, or drills. Applications may include, for example, turning, milling, or drilling of metals such as steel.
[0035] method
[0036] The average grain size of the Ti(C,N) layer, D 422
[0037] To investigate the average grain size of Ti(C,N) grains in the Ti(C,N) layer, X-ray diffraction (XRD) was performed on the flank face using a PANalytical CubiX3 diffractometer equipped with a PIXcel detector. The coated cutting tool was mounted in a sample holder, ensuring that the flank face of the sample was parallel to the reference surface of the sample holder and at an appropriate height. Cu-Kα rays were used for measurements at a voltage of 45 kV and a current of 40 mA. A 1 / 2-degree anti-scattering slit and a 1 / 4-degree diverging slit were used. The diffraction intensity from the coated cutting tool was measured within a 2θ range of 20° to 140°, i.e., from an incident angle θ range of 10° to 70°. Data analysis was performed using PANalytical's X'Pert HighScore Plus software, including background fitting, Cu-Kα2 removal, and distribution fitting.
[0038] The grain size of the layer was calculated using the integral full width at half maximum (FWHM) of the distribution fitting curve obtained from PANalytical's X'Pert HighScore Plus software, according to the Scherrer formula (Eq1) (Birkholz, 2006).
[0039] Average grain size D 422 The full width at half maximum (FWHM) of peak (422) is calculated using the Scherrer formula:
[0040]
[0041] Where D 422 λ is the average grain size of the Ti(C,N) ray, K is the shape factor and is set to 0.9 here, and λ is the wavelength of the CuKα1 ray and is set to 0.9 here. B 422 It is the FWHM value of the reflection (422), and θ is the Bragg angle, i.e. the incident angle.
[0042] The FWHM obtained from the measurements contains both broadening from the instrument and broadening caused by small grain size. To compensate for this, the Gaussian approximation is used (Birkholz, 2006). 422 It is the line width at FWHM after subtracting the instrument width (0.00174533 radians), and is defined in formula (2):
[0043] B 422 =√((FWHM) obs ) 2 -(FWHM ins ) 2 (2)
[0044] Among them B422 It is a broadening (in radians) used for grain size calculation, FWHM obs It measures the widening (in radians), FWHM ins It is an increase in instrument width (in radians).
[0045] Since other possible layers above the Ti(C,N) layer can affect the X-ray intensity entering the Ti(C,N) layer and leaving the entire coating, it is necessary to consider the linear absorption coefficients of the corresponding compounds in the layers to make corrections for these effects. Alternatively, other layers above the Ti(C,N) monolayer can be removed by methods such as chemical etching that do not substantially affect the XRD measurement results.
[0046] Grain size and orientation of the B1 portion of Ti(C,N)
[0047] In the uppermost region of the Ti(C,N) layer, in region B1, which is closest to the bonding layer that attaches the Al2O3 layer to the Ti(C,N) layer, the Ti(C,N) grains are enlarged to improve adhesion. The average grain size of the Ti(C,N) grains in region B1 is analyzed via a planar view. This planar view extends in a plane parallel to the surface of the substrate, thus allowing the study of the width of the columnar grains without interference from, for example, overlapping grains.
[0048] Samples for grain area analysis of the B1 region were produced by fabricating planar views of thin foil specimens of the region of interest using in-situ FIB extraction technology (Langford & Clinton, 2004). The samples were extracted from polished cross-sections. Sample preparation was performed using a Helios NanoLab 650 with a Ga+ ion source.
[0049] The region of interest was marked at the edges by cross-etching using an ion current of 79 pA and an accelerating voltage of 3 kV to ensure that the region of interest was precisely centered on the sample. Subsequently, a protective Pt layer of approximately 2 μm thickness was deposited using an ion current of 430 pA and an accelerating voltage of 30 kV to coat the region. Following the protective Pt deposition, the sample was prepared using a well-known in-situ extraction technique (Langford & Clinton, 2004).
[0050] The sample was thinned to a thickness of <200 nm to ensure electronic transparency.
[0051] Grain size in region B1 was analyzed using transmission Kikuchi diffraction (TKD) in a Helios NanoLab 650 equipped with an Oxford-symmetry EBSD detector. An accelerating voltage of 20 kV and a beam current of 13–26 nA were used. Regions of at least 5 × 5 μm (at least 640 grains) were analyzed in 10 nm steps using Speed 1 binning mode (622 × 512 pixels). The average grain size (equivalent circle) was analyzed using the Aztec Crystal software package (v2.0), with one-time automatic cleaning applied for mild noise reduction. The sample was analyzed with the sample surface parallel to the substrate surface to ensure that coatings outside the planar orientation were parallel to the sample normal. The grain detection threshold was set to 10° and a region of at least 40 pixels.
[0052] Orientation determination is a quantity expressed as a percentage (%) of the deviation of the analysis area from the set axis at a specific angle. For region B1, select... <211> The Ti(C,N) direction is taken as the direction parallel to the surface normal. Orientation is calculated for the region under analysis. <211> The deviation of Ti(C,N) orientation from the specified value is ≤15°. Aztec Crystal software (v2.0) was used to determine the orientation.
[0053] The Ti(C,N) diagram from the Journal of the Electrochemical Society (J. Electrochem. Soc.) [JESOAN], (1950), Vol. 97, pp. 299-304, was used for Ti(C,N) measurements, employing 89 reflectors.
[0054] Orientation of the lowest Al2O3-O1 portion
[0055] The portion of the Al2O3 layer near the bonding layer is highly oriented in this invention. To analyze this region, a cross-section of the coating was prepared, and the Al2O3 grains in the O1 portion extending 1 μm from the bonding layer were studied in detail by EBSD. The polished cross-section was prepared by the following steps: each CNMG120408-PM blade was mounted in AKASE black conductive phenolic resin, then ground to approximately 1 mm, followed by two-step polishing: coarse polishing (9 μm) using diamond slurry and fine polishing (1 μm). A final polishing was performed using a colloidal silica solution.
[0056] The orientation of the lowest portion of Al2O3 is determined as a percentage (%) of the analytical region within a specific angular deviation from the set axis. For the O1 portion, select... <001> The Al2O3 orientation is defined as the direction parallel to the surface normal. Orientation is calculated for the region under analysis. <001> The amount of Al2O3 whose orientation deviates by ≤15°.
[0057] A region at least 80 μm wide was analyzed with a step size of 50 nm using Speed 1 binning mode (622 × 512 pixels). To analyze the orientation of O1, four rectangular portions of O1 were randomly selected along an interface with dimensions of 10 μm wide and 1 μm high. The orientation was calculated as the average of the four rectangular portions. An automatic cleaning step and a zero-solution cleaning at the 5 nearest neighbor level were applied to the data. Aztec Crystal software (v2.0) was used to determine the orientation.
[0058] The orientation of the O1 portion was analyzed using a Zeiss Supra 55 and a Helios NanoLab 650, both equipped with Oxford-symmetry EBSD detectors. An accelerating voltage of 20 kV and a beam current of 13–26 nA were used. The sample was mounted on a 70° pre-tilted sample holder to ensure maximum collection efficiency.
[0059] Alumina (α) in Acta Crystallogr (Sec B) [ACBCAR], Vol. 49B, pp. 973-980, is shown in the figure for Al2O3 measurement using 89 reflectors.
[0060] SEM study
[0061] SEM studies of the polished cross-section and the top surface of the sample were performed using a Carl Zeiss AG-Supra 40 with a 30 μm aperture and an accelerating voltage of 3 kV. Images were acquired using a secondary electron detector.
[0062] X-ray diffraction measurements of Ti(C,N) and Al2O3
[0063] To investigate the texture of the entire layer, X-ray diffraction was performed on the flank face of the cutting tool insert using a PANalytical CubiX3 diffractometer equipped with a PIXcel detector. The coated cutting tool insert was mounted in a sample holder, ensuring that the flank face of the cutting tool insert was parallel to the reference surface of the sample holder and that the flank face was at an appropriate height. Cu-Kα rays were used for the measurements at a voltage of 45 kV and a current of 40 mA. A 1 / 2-degree anti-scattering slit and a 1 / 4-degree diverging slit were used. The diffraction intensity from the coated cutting tool was measured within a 2θ range of 20° to 140°, i.e., within an incident angle θ range of 10° to 70°.
[0064] Data analysis was performed using PANalytical's X'Pert HighScore Plus software, including background subtraction and Cu-K subtraction. α2 Removal and distribution fitting. A general description of the fitting will be given later. The texture factor of the layer is then calculated by comparing the measured intensity data of a specific layer (e.g., Ti(C,N) or α-Al2O3 layer) with the standard intensity data according to the PDF card using the Harris formula (3) disclosed below, with the output from the program (the integral peak area of the distribution fitting curve). Because the thickness of the layer is finite, the relative intensity of a pair of peaks at different 2θ angles differs from the relative intensity of peaks for a bulk sample due to the different path lengths through the layer. Therefore, when calculating the TC value, the linear absorption coefficient of the layer is also taken into account, and a thin film correction is applied to the extracted integral peak area intensity of the distribution fitting curve. Since other possible layers above, for example, the α-Al2O3 layer, may affect the X-ray intensity entering the α-Al2O3 layer and leaving the entire coating, the linear absorption coefficient of the corresponding compound in the layer also needs to be taken into account to correct for these. This also applies to X-ray diffraction measurements of the Ti(C,N) layer if the Ti(C,N) layer is located below, for example, the α-Al2O3 layer. Alternatively, other layers, such as TiN, above the alumina layer can be removed using methods that do not substantially affect XRD measurement results, such as chemical etching.
[0065] To study the texture of the α-Al₂O₃ layer, CuK was used. α X-ray diffraction was performed using radiation, and the texture coefficient TC(hkl) of the columnar grains in different growth directions of the α-Al2O3 layer was calculated according to Harris's formula (3):
[0066]
[0067] Where I(hkl) = the measured (integral area) intensity of the (hkl) reflection, I0(hkl) = the standard intensity according to ICDD PDF card No. 00-010-0173, and n = the number of reflections to be used in the calculation. The (hkl) reflections used in this case are: (1 0 4), (1 1 0), (1 1 3), (0 2 4), (1 1 6), (2 1 4), (3 0 0), and (0 0 12). Before calculating the ratio, the measured integral peak area is corrected for thin films and for any other layers above (i.e., on top) the α-Al2O3 layer.
[0068] The texture factor TC(hkl) of the columnar grains in different growth directions of the Ti(C,N) layer is calculated according to the previously published Harris formula (3), where I(hkl) is the measured (integrated area) intensity of the (hkl) reflection, I0(hkl) is the standard intensity according to ICDD PDF card No. 42-1489, and n is the number of reflections to be used in the calculation. The (hkl) reflections used in this case are (1 1 1), (2 0 0), (2 2 0), (3 1 1), (3 3 1), (4 2 0), and (4 2 2).
[0069] It should be noted that peak overlap is a phenomenon that can occur in X-ray diffraction analysis of coatings comprising, for example, several crystalline layers and / or deposited on a matrix containing a crystalline phase, and this must be taken into account and compensated for. The overlap of peaks from the α-Al₂O₃ layer with peaks from the Ti(C,N) layer may affect the measurements and needs to be considered. It should also be noted that, for example, WC in the matrix may have diffraction peaks close to the relevant peaks of this invention. Attached Figure Description
[0070] Embodiments of the present invention will be described with reference to the accompanying drawings, wherein:
[0071] Figure 1 A scanning electron microscope (SEM) image of a cross-section of an example of the coating of the present invention (sample D) is shown, in which the B1 portion of the Ti(C,N) layer (1), the bonding layer (2), and the O1 portion of the α-Al2O3 layer (3) are shown.
[0072] Figure 2 A scanning electron microscope (SEM) image of a cross-section of an example of the reference coating (sample A) is shown, in which the uppermost Ti(C,N) (1), the bonding layer (2), and the lowermost α-Al2O3 (3) are visible.
[0073] Figure 3 A scanning electron microscope (SEM) image of a cross-section of an example of the comparative coatings (sample G) is shown, which shows the B1 portion of the Ti(C,N) layer (1), the bonding layer (2), and the O1 portion of the α-Al2O3 layer (3).
[0074] Figure 4 A scanning electron microscope (SEM) image of a cross-section of an example of the reference coating (sample B) is shown, in which the uppermost Ti(C,N) (1), the bonding layer (2), and the lowermost α-Al2O3 (3) are visible.
[0075] Figure 5The image shows a scanning electron microscope (SEM) image of the top surface of portion B1 of a sample having a Ti(C,N) layer corresponding to the Ti(C,N) in sample D, where the morphology of the outermost surface of portion B1 is visible.
[0076] Figure 6 The image shows a scanning electron microscope (SEM) image of the top surface of the Ti(C,N) layer in the sample having a Ti(C,N) layer corresponding to the Ti(C,N) in sample B, where the morphology of the outermost surface of the very fine-grained Ti(C,N) is visible.
[0077] Figure 7 The image shows a scanning electron microscope (SEM) image of the top surface of the Ti(C,N) layer in a sample having a Ti(C,N) layer corresponding to that in reference sample A, where the morphology of the outermost surface of the coarse-grained Ti(C,N) is visible.
[0078] Figure 8 This is a schematic overview showing the positions of the layers and portions of the present invention: the Ti(C,N) layer (1), the B1 portion of the Ti(C,N) layer (1), the bonding layer (2), the α-Al2O3 layer (3), the O1 portion of the α-Al2O3 layer (3), and the substrate (4).
[0079] Figure 9 It is a contrast-enhanced TKD image of a planar view of sample D, in which Ti(C,N) grains in the B1 portion are visible. Example
[0080] Exemplary embodiments of the present invention will now be disclosed in more detail and compared with reference embodiments. Coated cutting tools (blades) are manufactured and analyzed and tested in cutting experiments.
[0081] The cemented carbide matrix is manufactured using conventional processes including grinding, mixing, spray drying, pressing, and sintering. The ISO type geometry of the cemented carbide matrix (insert tool) is CNMG-120408-PM. The cemented carbide composition is 7.2 wt% Co, 2.9 wt% TaC, 0.5 wt% NbC, 1.9 wt% TiC, 0.4 wt% TiN, and the remainder WC.
[0082] Prior to coating deposition, the substrate is exposed to a mild blasting process to remove any residues from the sintering process from the substrate surface.
[0083] CVD deposition
[0084] The sintered substrate was CVD coated in an Ionbond Type size 530 radial CVD reactor capable of accommodating 10,000 half-inch cutting blades. Samples for further testing and analysis were selected from the center of the chamber, at a position half the plate radius between the plate center and the periphery. A mass flow controller was selected to allow for setting a high flow rate, such as CH3CN.
[0085] A first innermost coating of approximately 0.2 μm TiN was deposited on all substrates at a process of 400 mbar and 885 °C. A gas mixture of 48.8 vol% H2, 48.8 vol% N2, and 2.4 vol% TiCl4 was used.
[0086] Subsequently, Ti(C,N) layers were deposited, with all samples AG deposited using different Ti(C,N) as follows. Reference sample A was deposited using process steps V and W as shown in Table 1. Before starting process step X, sample BG was temperature-conditioned from 885°C to 870°C in 50 vol% H2 and 50 vol% N2 at 80 mbar. The Ti(C,N) layer of reference sample B was deposited using process step X as shown in Table 1. On sample CG, Ti(C,N) layers were deposited using process steps X, Y, and Z, with deposition times as shown in Tables 1 and 2. Processing times were adjusted so that all samples achieved approximately the same total Ti(C,N) layer thickness.
[0087] Table 1
[0088]
[0089] Table 2
[0090]
[0091] A 0.7–0.9 μm thick bonding layer was deposited on top of the Ti(C,N) layer at 1000 °C via a process consisting of four independent reaction steps. The process consisted of: an 8-minute HTCCVD Ti(C,N) step using TiCl4, CH4, N2, HCl, and H2 at 400 mbar; a second step (Ti(C,N,O)-1) using TiCl4, CH3CN, CO, N2, and H2 at 70 mbar; a third step (Ti(C,N,O)-2) using TiCl4, CH3CN, CO, N2, and H2 at 70 mbar; and a final step (TiN) using TiCl4, N2, and H2 at 70 mbar for 6 minutes. During the third deposition step, as shown in Table 3, the CO gas flow rate increased linearly from the initial value to the final value. All other gas flow rates remained constant, but the concentrations of all gases were slightly affected due to the increased total gas flow rate. Before the subsequent Al2O3 nucleation begins, the bonding layer is oxidized in a mixture of CO2, CO, N2 and H2 for 4 minutes.
[0092] Detailed information on the bonding layer deposition is shown in Table 3.
[0093] Table 3. Deposition of the bonding layer
[0094]
[0095] An α-Al₂O₃ layer was deposited on top of the bonding layer. All α-Al₂O₃ layers were deposited in two steps at 1000 °C and 55 mbar. The first step used 1.2 vol% AlCl₃, 4.7 vol% CO₂, 1.8 vol% HCl, and the balance H₂ to give an α-Al₂O₃ layer of approximately 0.1 μm, while the second step, disclosed below, gave a total α-Al₂O₃ layer thickness of approximately 5 μm. The second step of the α-Al₂O₃ layer was deposited using 1.16% AlCl₃, 4.65% CO₂, 2.91% HCl, 0.58% H₂S, and the balance H₂.
[0096] Coating analysis
[0097] The layer thickness was measured on the rake face of the cutting tool sample using a scanning electron microscope. The layer thickness of the coating on sample AG is shown in Table 4.
[0098] Table 4. Layer Thickness
[0099]
[0100] The grain size of the Ti(C,N) layer was analyzed using the average value throughout the Ti(C,N) layer and in the B1 region near the bonding layer. The results are shown in Table 5.
[0101] The orientation of Ti(C,N) grains in the B1 region of the Ti(C,N) layer and the orientation of α-Al2O3 grains in the O1 region of the α-Al2O3 layer were analyzed. The results are shown in Table 5.
[0102] The grain size of the Ti(C,N) layer in reference sample A was too large for XRD analysis, and the Scherrer formula was not considered valid for grain sizes larger than approximately 0.2 μm. The average grain size of this layer was measured to be greater than 200 nm in the cross-sectional SEM image.
[0103] Table 5. Grain size and orientation of O1 and B1 portions
[0104]
[0105] (na = Unanalyzed)
[0106] The texture coefficients of the Ti(C,N) and α-Al2O3 layers were analyzed using X-ray diffraction, and the results are shown in Tables 6 and 7.
[0107] Table 6. Texture coefficients of the α-Al₂O₃ layer in the samples
[0108] sample TC(104) TC(110) TC(113) TC(024) TC(116) TC(214) TC(300) TC(0012) A 0.02 0.25 0.01 0.07 0.01 0.03 0.00 7.61 B 0.00 0.01 0.00 0.00 0.00 0.00 0.00 7.99 C 0.02 0.03 0.00 0.01 0.01 0.00 0.00 7.94 D 0.01 0.07 0.00 0.02 0.00 0.00 0.00 7.89 E 0.01 0.08 0.00 0.02 0.01 0.00 0.00 7.89 F 0.09 0.09 0.00 0.03 0.06 0.01 0.01 7.70 G 0.03 0.17 0.00 0.05 0.03 0.01 0.00 7.72
[0109] Table 7. Texture coefficient TC(422) of the Ti(C,N) layer in the sample
[0110] sample TC(422) A 3.94 B 3.95 C 3.43 D 4.14 E 4.06 F 3.19 G 3.74
[0111] Performance test
[0112] In two parallel cutting tests (Cutting Test 1 and Cutting Test 2), freshly coated cutting tools were tested in longitudinal turning operations on OVAKO 825B (100CrMo7-3) high-alloy steel. The cutting speed Vc was 220 m / min, the feed rate fn was 0.3 mm / rpm, the depth of cut was 2 mm, and water-soluble cutting fluid was used. Machining continued until the end-of-life criteria were met. One cutting edge of each cutting tool was evaluated.
[0113] When the wear on the flank face is greater than 0.3 mm after one or two passes, or when the area of the crater (exposed substrate) is greater than 0.2 mm. 2 When the tool life standard is met, it is considered to have been reached. Once any one of these standards is met, the sample is considered to have reached its lifespan. The results of the cutting tests are shown in Tables 8 and 9.
[0114] Table 8. Cutting Test 1
[0115]
[0116] Table 9. Cutting Test 2
[0117] sample Time elapsed until the cutting life ends [minutes] Reaching the end of life due to the following reasons A 54 Crescent-shaped pit wear >0.2 D 86 Crescent-shaped pit wear >0.2 E 82 Crescent-shaped pit wear >0.2
[0118] As can be seen from Table 8, all samples D and E of the present invention exhibit high wear resistance, while samples A, F, and G show the formation of crater-like craters due to the lower orientation in the O1 portion. As shown in Table 9, compared with the reference sample (reference sample A) which also has very high performance, samples D and E of the present invention exhibit high resistance to flank wear and high resistance to crater wear in metal cutting of steel.
[0119] The cutting tools were also evaluated by exposure to wet abrasive blasting. Blasting was performed on the rake face of the cutting tool. The blasting slurry consisted of water containing 20% by volume alumina, with the rake face of the cutting tool at a 90° angle to the direction of the blasting slurry. The distance between the nozzle and the cutting tool surface was approximately 145 mm. The pressure of the slurry on the blasting gun was 1.8 bar for all samples, while the air pressure was 2.2 bar. The alumina abrasive was F230 mesh (FEPA 42-2:2006). The average blasting time per unit area was 4.4 seconds. Samples B and C failed the wet blasting test; the coating of sample B showed severe peeling, and sample C showed pinpoint peeling. All other samples withstood the wet blasting test without damage to the coating.
[0120] While the invention has been described in conjunction with various exemplary embodiments, it should be understood that the invention is not limited to the disclosed exemplary embodiments, but rather is intended to cover various modifications and equivalent arrangements as indicated in the appended claims. Furthermore, it should be recognized that any disclosed form or embodiment of the invention can be incorporated, as a general matter of design choice, into any other disclosed or described or suggested form or embodiment. Therefore, it is intended to be limited only to the scope indicated by the appended claims.
Claims
1. A cutting tool comprising a substrate at least partially coated with a coating comprising a Ti(C,N) layer, an α-Al₂O₃ layer, and a bonding layer therebetween, wherein the α-Al₂O₃ layer comprises an O₁ portion extending 1 µm from the bonding layer, wherein the O₁ portion exhibits an orientation such that, when measured using electron backscatter diffraction (EBSD) on a cross-section of the α-Al₂O₃ layer, ≥80% of the analytical region has an orientation within 15 degrees of the surface normal of the α-Al₂O₃ layer. <001> The direction, wherein the surface normal of the α-Al2O3 layer is parallel to the surface normal of the substrate surface. The Ti(C,N) layer, with a thickness of 3-25 µm, is composed of columnar grains, wherein the average grain size D of the Ti(C,N) layer, as measured by X-ray diffraction using CuKα radiation, is... 422 The grain size D is 25-50 nm. 422 It is calculated based on the Scherrer formula from the full width at half maximum (FWHM) of peak (422): Where D 422 Where is the average grain size of the Ti(C,N), K is the shape factor and is set to 0.9 here, λ is the wavelength of CuKα radiation and is set to 1.5405 Å here, B 422 It is the FWHM value of the reflection (422), and θ is the Bragg angle. The Ti(C,N) layer includes a B1 portion adjacent to the bonding layer, wherein the thickness of the B1 portion of the Ti(C,N) layer is 0.5-1.5 µm, and wherein the average grain size of the Ti(C,N) grains in the B1 portion is greater than the average grain size D over the entire thickness of the Ti(C,N) layer. 422 In the B1 portion of the Ti(C,N) layer, when measured using transmission Kikuchi diffraction (TKD) on a planar view extending parallel to the substrate surface in the B1 portion of the Ti(C,N) layer, the average grain size of the Ti(C,N) grains is 130 nm-165 nm.
2. The cutting tool according to claim 1, wherein the α-Al₂O₃ layer exhibits a texture coefficient TC(hkl) as defined by Harris's formula, measured by X-ray diffraction using CuKα radiation and θ-2θ scanning: Where I(hkl) is the measured intensity (integrated area) of the (hkl) reflection, I0(hkl) is the standard intensity according to ICDD PDF card No. 00-010-0173, n is the number of reflections used in the calculation, and the (hkl) reflections used are (10 4), (1 1 0), (1 1 3), (0 2 4), (1 1 6), (2 1 4), (3 0 0), and (0 0 12), characterized in that, TC(0 0 12) ≥7.
5.
3. The cutting tool according to claim 1 or 2, wherein the α-Al2O3 layer exhibits a texture factor TC(110) ≤ 0.
2.
4. The cutting tool according to claim 1 or 2, wherein the average thickness of the α-Al2O3 layer is 1 µm-15 µm.
5. The cutting tool according to claim 1 or 2, wherein, when measured using transmission Kikuchi diffraction (TKD) in a planar view extending parallel to the surface of the substrate, the Ti(C,N) layer in the B1 portion of the Ti(C,N) layer exhibits an orientation such that ≥93% of the analytical region has an angle of less than 15 degrees with the surface normal of the Ti(C,N) layer. <211> The direction, wherein the surface normal of the Ti(C,N) layer is parallel to the surface normal of the substrate surface.
6. The cutting tool according to claim 1 or 2, wherein the Ti(C,N) layer exhibits an X-ray diffraction pattern measured using CuKα radiation and θ-2θ scanning, wherein TC(hkl) is defined according to the Harris formula, wherein I(hkl) is the measured intensity (integral area) of the reflection of (hkl), I0(hkl) is the standard intensity according to ICDD PDF card No. 42-1489, n is the number of reflections, and the reflections used in the calculation are (1 1 1), (2 0 0), (2 2 0), (3 1 1), (3 3 1), (42 0), and (4 2 2), wherein TC(422)≥3.
7. The cutting tool according to claim 1 or 2, wherein the grain size D of Ti(C,N) 422 The wavelength is 25-40 nm.
8. The cutting tool according to claim 1 or 2, wherein the average thickness of the Ti(C,N) layer is 4-20 µm.
9. The cutting tool according to claim 1 or 2, wherein the bonding layer comprises at least one compound selected from titanium carbon oxide, titanium nitride, and titanium carbon oxynitride.
10. The cutting tool according to claim 1 or 2, wherein the average thickness of the bonding layer is 0.25-2.5 µm.
11. The cutting tool according to claim 1 or 2, wherein the average thickness of the coating is 5 µm-30 µm.
12. The cutting tool according to claim 1 or 2, wherein the substrate is cemented carbide, cermet, or ceramic.
Citation Information
Patent Citations
CVD coated cutting tool
CN105714268A