Drug-loaded polymer embolization microspheres and preparation method thereof

By cross-linking polymers containing hydroxyl and ionic groups to prepare drug-loaded microspheres, the problems of insufficient drug loading stability, expansion performance and compressive elasticity of existing microspheres are solved, achieving efficient drug release and reducing the number of treatments.

CN117357686BActive Publication Date: 2026-11-20ZHUHAI LIVZON MICROSPHERE TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311196159.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-15
Publication Date
2026-11-20
Estimated Expiration
2043-09-15

AI Technical Summary

Technical Problem

Existing drug-loadable embolized microspheres have shortcomings in terms of drug loading stability, expansion performance, and compressive elasticity, which affect the efficacy of chemotherapy and the treatment burden on patients.

Method used

Drug-loaded microspheres are prepared by cross-linking polymers containing hydroxyl and ionic groups with a cross-linking agent to form a microsphere framework, encapsulating the ionic group compounds, and then using reverse suspension polymerization to improve the drug loading stability, expansion performance, and compressive elasticity of the microspheres.

Benefits of technology

This invention enables the development of microspheres with good drug-loaded stability, strong drug-loading capacity, and good compressibility, which can slowly release drugs at the target lesion site, reducing the number of treatments and lowering the burden on patients.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to a kind of high molecular microspheres obtained by wrapping the high molecular compound containing ion group with the high molecular compound containing hydroxyl group, which uses polyvinyl alcohol as base material, and crosslinking microspheres with polyaldehyde such as glutaraldehyde, while embedding carboxyl-containing polyacrylate or polymethacrylate.The microspheres of the present application are regular in shape, size controllable, good in suspension and deformation elasticity, and have good drug loading performance and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of medical devices, specifically to a drug-loadable embolic microsphere encapsulated with sodium polyacrylate and its preparation method. Background Technology

[0002] Transcatheter arterial chemoembolization (TACE) involves selectively or superselectively inserting a catheter into the target artery supplying the tumor under X-ray and contrast agent guidance. An appropriate amount of embolic agent is then injected at a suitable rate, causing occlusion of the target artery and inducing ischemic necrosis of the tumor tissue. Depending on the embolic agent, it can be divided into conventional TACE (C-TACE) and drug-eluting microsphere embolization (DEB-TACE). Although C-TACE has demonstrated its efficacy and clinical value through years of clinical application, its drawbacks include the rapid clearance of iodized oil in some patients, failing to achieve long-term embolization; and the rapid release of the drug in iodized oil, preventing the drug from maintaining a high concentration within the tumor tissue for an extended period. Consequently, some patients often require multiple interventional treatments, which can place a significant burden on the patient's liver function.

[0003] In recent years, the emergence of a new weapon, "drug-eluting microspheres," also known as "drug-loadable embolic microspheres," has further improved the efficacy of TACE in some patients. "Drug-eluting microspheres" are a novel embolic substance capable of adsorbing and carrying chemotherapy drugs. They are non-degradable in the body. After entering tumor blood vessels, they can provide long-term embolization of tumor vessels and allow chemotherapy drugs to act on the tumor interior for an extended period. The combined effect of these two factors can achieve better local control.

[0004] Currently available drug-loaded microspheres include DC Bead from Biocompatibles (UK), HepaSphere from Biosphere (USA), and CalliSpheres from Hengrui Group. These marketable drug-loaded embolic microspheres primarily use polyvinyl alcohol (PVA) as the main material. By modifying PVA and grafting double-bonded monomers onto its molecular chains, these monomers polymerize and cross-link with monomers containing ionic functional groups, forming charged embolic microspheres that thus achieve drug loading. However, data indicates that these microspheres suffer from stability issues after drug loading. Furthermore, while these embolic microspheres possess a certain drug loading capacity and compressive elasticity, their cross-linking is achieved through the polymerization of PVA grafted with monomers containing ionic functional groups. The more PVA monomers grafted, the more ionic functional groups the microsphere contains, resulting in a stronger drug loading capacity. However, this also leads to a higher degree of cross-linking, poorer compressibility, and decreased expansion performance and drug loading speed. This mutual constraint limits the optimization of the drug-loading performance and compressibility of embolization microspheres. Therefore, in order to achieve more ideal drug loading performance, new microspheres are needed to overcome this limitation. Summary of the Invention

[0005] The first aspect of the present invention provides a polymer microsphere, wherein the raw materials for preparing the polymer microsphere include a polymer compound containing hydroxyl groups, a polymer compound containing ionic groups, and a crosslinking agent;

[0006] The hydroxyl-containing polymeric compound is selected from one or more of polyvinyl alcohol, chitosan, or starch;

[0007] The polymeric compound containing ionic groups is selected from one or more of polyacrylic acid, sodium polyacrylate, polymethacrylic acid, and their salts.

[0008] Alternatively, the present invention provides a polymer microsphere comprising a cross-linked polymeric compound containing hydroxyl groups and a polymeric compound containing ionic groups; the cross-linked polymeric compound containing hydroxyl groups is formed by reacting raw materials containing the polymeric compound containing hydroxyl groups and a cross-linking agent; the polymeric compound containing hydroxyl groups is selected from one or more of polyvinyl alcohol, chitosan, or starch; the polymeric compound containing ionic groups is selected from one or more of polyacrylic acid, sodium polyacrylate, polymethacrylic acid, and their salts. This microsphere exhibits good water absorption and swelling properties, drug loading rate, drug loading capacity, and compressibility.

[0009] The polymer microspheres are formed by cross-linking hydroxyl-containing polymers with a cross-linking agent to form a spherical skeleton. The spherical skeleton encapsulates polymers containing ionic groups. Compared with microspheres formed by directly cross-linking hydroxyl-containing polymers with ionic groups, this method helps improve the compressibility, expansion performance, and drug loading speed of the microspheres.

[0010] A second aspect of this invention provides a method for preparing polymer microspheres, comprising the following steps:

[0011] A cross-linked aqueous solution is formed by combining a polymer containing hydroxyl groups and a polymer containing ionic groups.

[0012] The crosslinking aqueous solution is added to an organic solvent containing a dispersant, and a crosslinking agent is added to carry out a crosslinking reaction;

[0013] The hydroxyl-containing polymeric compound is selected from one or more of polyvinyl alcohol, chitosan, or starch;

[0014] The polymeric compound containing ionic groups is selected from one or more of polyacrylic acid, sodium polyacrylate, polymethacrylic acid, and their salts. This preparation method is simple, and drug-loadable embolic microspheres can be prepared through a single cross-linking reaction.

[0015] A third aspect of the present invention provides a drug-loaded polymer microsphere, which is obtained by loading an antitumor drug onto microspheres prepared by the above method; the antitumor drug is preferably a charged antitumor drug, more preferably doxorubicin or pirarubicin.

[0016] The fourth aspect of the present invention provides the application of the microspheres prepared by the above method or the above drug-loaded polymer microspheres in the preparation of embolic agents, particularly in the field of transcatheter arterial chemoembolization.

[0017] The beneficial effects of this invention are as follows:

[0018] ① Good stability after drug loading: The embolization microspheres of the present invention have very good stability after drug loading. After 7 days, the purity is above 95%, and after 14 days, the purity is above 88%.

[0019] ② Strong drug loading capacity: The embolic microspheres of this invention contain ionic functional groups (negatively charged carboxyl groups), which can be mixed with charged drugs before clinical use, adsorbing and enriching the charged drugs, thereby achieving drug loading function, and slowly releasing the drugs upon entering the target lesion site. The microspheres have strong hydrophilicity, good swelling capacity and rapid adsorption and drug loading capacity, and high drug loading capacity, completing drug loading within 15 minutes;

[0020] ③ Good compressibility: The embolization microspheres of the present invention can pass smoothly through microcatheters with an inner diameter smaller than the diameter of the embolization microspheres themselves. After being compressed by 20% of their own diameter, the microspheres still maintain their integrity and can quickly return to their original size after the external force is removed.

[0021] ④ The embolization microspheres of the present invention can be obtained with an average particle size of greater than or equal to 100 μm after swelling, which meets the clinical requirements for the particle size of embolization microspheres. Attached Figure Description

[0022] Figure 1 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 1.

[0023] Figure 2 This is a light microscopic image of the drug-loaded microspheres prepared in Example 1.

[0024] Figure 3 The image shows a transverse scan of the drug-loaded microspheres prepared in Example 1, taken from the top to the maximum cross-section, under a laser confocal microscope.

[0025] Figure 4 This is a transverse scan of a DC Bead after drug loading, taken from the top to the maximum cross-section, under a laser confocal microscope.

[0026] Figure 5 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 2.

[0027] Figure 6 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 3.

[0028] Figure 7 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 4-1.

[0029] Figure 8 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 4-2.

[0030] Figure 9 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 5-1.

[0031] Figure 10 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 5-2.

[0032] Figure 11 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 6-1.

[0033] Figure 12 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 6-1.

[0034] Figure 13 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 7.

[0035] Figure 14 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 8.

[0036] Figure 15 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 9.

[0037] Figure 16 Scanning electron microscope image of the microspheres prepared in Example 10.

[0038] Figure 17 Scanning electron microscope image of the microspheres prepared in Example 11.

[0039] Figure 18 Scanning electron microscope image of the microspheres prepared in Example 12.

[0040] Figure 19 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Example 13-1.

[0041] Figure 20 The image shows a scanning electron microscope (SEM) image of the microspheres prepared in Examples 13-2.

[0042] Figure 21 The drug loading curves of doxorubicin loaded onto microspheres prepared in Examples 1, 2, and 3 are shown.

[0043] Figure 22 The in vitro release curves of the microspheres prepared in Example 2 and DC bead. Detailed Implementation Plan

[0044] Microspheres

[0045] In one aspect, the present invention provides a polymer microsphere, wherein the raw materials for preparing the polymer microsphere include a polymer compound containing hydroxyl groups, a polymer compound containing ionic groups, and a crosslinking agent;

[0046] The hydroxyl-containing polymeric compound is selected from one or more of polyvinyl alcohol, chitosan, or starch;

[0047] The polymeric compound containing ionic groups is selected from one or more of polyacrylic acid, sodium polyacrylate, polymethacrylic acid, and their salts.

[0048] The presence of ionic groups can be due to the polymer compound itself having ionic groups or being capable of ionizing in solution. The polyacrylic acid and polymethacrylic acid are capable of ionizing in aqueous solution, which is used to adsorb and enrich charged drugs.

[0049] In one embodiment, the ionic group is a carboxyl group.

[0050] In one embodiment, both the polymer containing hydroxyl groups and the polymer containing ionic groups are water-soluble polymers.

[0051] In one embodiment, the polymer microspheres are formed by cross-linking a polymer compound containing hydroxyl groups with a cross-linking agent to form a spherical framework, and the spherical framework encapsulates a polymer compound containing ionic groups.

[0052] In one embodiment, the crosslinking agent is selected from polyaldehyde crosslinking agents, such as dialdehyde crosslinking agents, and more particularly, glutaraldehyde.

[0053] In one embodiment, the raw materials for preparing the polymer microspheres also include a dispersant.

[0054] In one embodiment, the dispersant is selected from one or more of the Tween series compounds and the modified cellulose series compounds, more preferably cellulose acetate butyrate or cellulose acetate.

[0055] In one embodiment, the dispersant is one or more of the Tween series compounds, such as Tween 20 or Tween 80.

[0056] In one embodiment, the dispersant is one or more of a series of modified cellulose compounds, such as cellulose acetate butyrate or cellulose acetate.

[0057] In one embodiment, the mass ratio of the polymer containing hydroxyl groups to the polymer containing ionic groups is (0.1-10):1, preferably (0.5-5):1, for example, 3:2 or 3:1.

[0058] Preferably, the mass ratio of the dispersant to the hydroxyl-containing polymer is (0.1-20):(1-4), for example, (4-5):(1-4) or (4-5):3.

[0059] Preferably, the mass ratio of the crosslinking agent to the hydroxyl-containing polymer compound is (0.05-10):1, for example (0.05:1)-1, and further can be (0.1-0.6):1 or (0.2-0.6):1, for example 0.2:1, 0.3:1, 0.6:1, 1:1, 1.5:1 or 2:1.

[0060] In one embodiment, the mass ratio of the crosslinking agent to the hydroxyl-containing polymer compound is greater than 0.07:1.

[0061] In one embodiment, the mass ratio of the crosslinking agent to the hydroxyl-containing polymer compound is less than 1:1.

[0062] In one embodiment, the hydroxyl-containing polymer compound may be low-viscosity polyvinyl alcohol and / or high-viscosity polyvinyl alcohol.

[0063] In one embodiment, the viscosity of the hydroxyl-containing polymer compound is 1 mPa·s-50 mPa·s, preferably 20 mPa·s-40 mPa·s, for example, 4.5 mPa·s-6.1 mPa·s or 25.5 mPa·s-34.5 mPa·s;

[0064] Preferably, the molecular weight of the polymer containing ionic groups is 5,000-5,000,000, more preferably 100,000-1,000,000, further preferably 100,000-500,000, and even more preferably 100,000-300,000. For example, it can also be 50,000-4,500,000 or 100,000-5,000,000, more preferably 1,000,000-5,000,000. For example, it can be 100,000, 150,000, 200,000, 250,000, 300,000, 350,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,500,000, 2,000,000, 2,500,000, 3,000,000, 3,500,000, 4,000,000, 4,500,000, 5,000,000, or any value between these two.

[0065] In one embodiment, the degree of alcoholysis of the hydroxyl-containing polymer is less than 95%, which facilitates its better solubility in aqueous solution.

[0066] The degree of alcoholysis of the hydroxyl-containing polymer is further less than 90%, for example, it can be 85%-90%, 86.5%-89.0%, 87%-89.0%, 78% or 88%.

[0067] In one embodiment, the polymer microspheres are prepared by reverse suspension polymerization.

[0068] In one embodiment, the polymer microspheres are prepared by reverse suspension polymerization comprising the following steps:

[0069] A cross-linked aqueous solution is formed by combining a polymer containing hydroxyl groups and a polymer containing ionic groups.

[0070] The crosslinking aqueous solution is added to an organic solvent containing a dispersant, and a crosslinking agent is added to carry out a crosslinking reaction.

[0071] The cross-linked aqueous solution contains a water-soluble polymer compound with hydroxyl groups at a mass content of 1-10%, more preferably 2-7%, for example 7%, 6%, 5%, 4.5%, 4%, 3%, 2% or 2.25%.

[0072] In the cross-linked aqueous solution, the mass content of the polymer compound containing ionic groups is 0.5%-5%, and more preferably 0.5%-4%, for example, 4%, 3%, 2%, 1.5%, 1%, 0.75%, or 0.5%.

[0073] In the organic solvent containing the dispersant, the mass content of the dispersant is 0.5%-4%, preferably 2%-3%.

[0074] Alternatively, it can be the mass content of the organic solvent containing the dispersant obtained by dissolving 3-8g of dispersant in 150-200mL of organic solvent.

[0075] Preferably, the mass content of the dispersant is equivalent to the mass content of the organic solvent containing the dispersant obtained by dissolving 4-5g of the dispersant in 180mL of organic solvent.

[0076] In some embodiments, the organic solvent is selected from one or more ester solvents, preferably acetate solvents, and more preferably ethyl acetate and / or butyl acetate.

[0077] Preferably, the organic solvent does not include hydrocarbon solvents, which is beneficial for preparing more rounded microspheres with less adhesion, and avoids the microspheres from blocking the catheter and affecting the embolization effect on the target blood vessel during the introduction of the interventional catheter into the diseased target blood vessel; or the microspheres are prone to rupture, resulting in uncontrollable drug release.

[0078] In one embodiment, the hydrocarbon solvent may include, for example, liquid paraffin.

[0079] In one embodiment, the crosslinked aqueous solution is obtained by mixing an aqueous solution of a polymer containing hydroxyl groups and an aqueous solution of a polymer containing ionic groups.

[0080] The preparation method of the aqueous solution includes: dispersing a polymeric compound containing hydroxyl groups into water and heating and stirring.

[0081] In one embodiment, the mass content of the hydroxyl-containing polymer in the aqueous solution is 5-25%, for example, it can be 5-20%, 10-20%, 11-20%, 10-15%, 10%, 15%, or the mass content of the hydroxyl-containing polymer is greater than or equal to 10%.

[0082] Furthermore, the preparation method includes dispersing a certain amount of a hydroxyl-containing polymer compound into an appropriate amount of purified water, heating to 70-100°C, and continuously stirring for, for example, 1-5 hours to obtain an aqueous solution of the hydroxyl-containing polymer compound.

[0083] In one embodiment, the mass content of the polymer containing ionic groups in the aqueous solution is 5-25%, for example, it can be 5-20%, 5-15%, 10-20%, 11-20%, 10-15%, 8%, 10%, 15%, or the mass content of the polymer containing hydroxyl groups is greater than or equal to 10%.

[0084] The preparation method of aqueous solution II includes: dispersing a polymeric compound containing ionic groups into water and heating and stirring.

[0085] Further, the preparation method includes: dispersing a certain amount of a polymer compound containing ionic groups into an appropriate amount of purified water, heating to 70-100°C, and continuously stirring for, for example, 1-5 hours to obtain an aqueous solution of the polymer compound containing ionic groups.

[0086] In one embodiment, the crosslinked aqueous solution is an acidic solution.

[0087] Preferably, the pH of the crosslinked aqueous solution is less than or equal to 5, and more preferably less than or equal to 4.

[0088] In one embodiment, the method for preparing the cross-linked aqueous solution includes: mixing solution one and solution two in a certain proportion, adding an appropriate amount of water to dilute to a certain concentration, and adjusting the pH to acidic.

[0089] The above mixed solution was ultrasonicated to obtain a uniformly dispersed white suspension, namely the cross-linked aqueous solution.

[0090] In one embodiment, the mixing ratio of solution one and solution two in the crosslinked aqueous solution is (1:1)-(15:1), preferably (1:1)-(6:1);

[0091] Alternatively, any ratio in which the mass ratio of the polymer containing hydroxyl groups to the polymer containing ionic groups in the crosslinked aqueous solution is (0.1-10):1.

[0092] In one embodiment, the method for preparing the organic solvent containing the dispersant includes: adding the dispersant to the organic solvent and stirring until dissolved.

[0093] Crosslinking reaction

[0094] In one embodiment, the crosslinking reaction includes: slowly adding a crosslinking aqueous solution dropwise to an organic solvent containing a dispersant, adding an appropriate amount of crosslinking agent, and stirring the reaction to obtain the polymer microspheres.

[0095] In one embodiment, during the crosslinking reaction, the volume of the crosslinking aqueous solution is smaller than the volume of the organic solvent, which is beneficial for preparing dispersed, non-adhesive microspheres.

[0096] Preferably, the volume ratio of the aqueous solution to the organic solvent is 1:(2-10), and more preferably it is 1:(3-9) or 1:(4-8); for example, it can be 1:4 or 1:8.

[0097] In one embodiment, the crosslinking agent is glutaraldehyde. Further, the crosslinking agent is dissolved in a solvent and added in the form of a crosslinking agent solution. The concentration of the crosslinking agent in the crosslinking agent solution is 40-60%, preferably 50%.

[0098] In one embodiment, the reaction temperature of the crosslinking reaction is greater than 20°C, and further greater than 30°C.

[0099] In one embodiment, the reaction temperature of the crosslinking reaction is less than 70°C, and further less than 60°C, which is beneficial to balancing the spheroidization reaction rate and morphology of the microspheres, resulting in more spherical microspheres.

[0100] In one embodiment, the reaction temperature of the crosslinking reaction is 20-70°C, and may further be 30-60°C, 30-50°C, or 40°C.

[0101] In one embodiment, the crosslinking reaction takes longer than 2 hours.

[0102] In one embodiment, the reaction time of the crosslinking reaction is less than 6 hours, for example, it can be 2 hours to 6 hours, 4 hours to 6 hours, or 2 hours to 4 hours.

[0103] In one embodiment, after the crosslinking reaction is completed, a post-processing step is further included. The post-processing includes: after the reaction is completed, collecting the solid, then soaking the solid in an alcohol solvent, filtering, repeating the soaking 0-3 times, washing with an ester solvent, and drying to form dried embolic microspheres.

[0104] In one embodiment, the preparation of the polymer microspheres further includes an alkali washing step of the dry polymer microspheres obtained by the crosslinking reaction, which helps to improve the adsorption performance of polyacrylate groups in the polymer microspheres, thereby increasing the drug loading of the microspheres.

[0105] The alkaline washing includes the step of immersing the polymer microspheres obtained by the cross-linking reaction in a sodium hydroxide solution.

[0106] In one embodiment, the alkaline washing process further includes washing with water, boiling with water, and sieving to obtain expanded embolic microspheres.

[0107] In one embodiment, the average particle size of the microspheres after swelling is greater than or equal to 100 μm.

[0108] In one embodiment, the water content of the microspheres after swelling is greater than 80%, further greater than 90%, and further greater than 95%.

[0109] Preferably, the water content of the microspheres after swelling is less than 98%.

[0110] In one embodiment, the microspheres have an average particle size of 50 μm or greater after drying.

[0111] In one embodiment, the elastic modulus of the microspheres is greater than or equal to 7 kPa, and further greater than or equal to 8 kPa or 14 kPa.

[0112] Preparation method

[0113] A method for preparing polymer microspheres, comprising the following steps:

[0114] A cross-linked aqueous solution is formed by combining a polymer containing hydroxyl groups and a polymer containing ionic groups.

[0115] The crosslinking aqueous solution is added to an organic solvent containing a dispersant, and a crosslinking agent is added to carry out a crosslinking reaction;

[0116] The hydroxyl-containing polymeric compound is selected from one or more of polyvinyl alcohol, chitosan, or starch;

[0117] The polymeric compound containing ionic groups is selected from one or more of polyacrylic acid, sodium polyacrylate, polymethacrylic acid, and their salts.

[0118] In one embodiment, the preparation method includes a one-step crosslinking reaction.

[0119] In one embodiment, the crosslinked aqueous solution does not contain an antitumor drug.

[0120] In one embodiment, the organic solvent is selected from one or more of n-heptane or ester solvents, preferably an acetate solvent, more preferably ethyl acetate and / or butyl acetate;

[0121] Preferably, the organic solvent does not include hydrocarbon solvents.

[0122] Preferably, the cross-linked aqueous solution is an acidic solution; the pH of the aqueous solution is preferably less than or equal to 5.

[0123] Preferably, the volume of the crosslinked aqueous solution is smaller than the volume of the organic solvent.

[0124] Preferably, the volume ratio of the aqueous solution to the organic solvent is 1:(2-10), more preferably 1:(4-8).

[0125] Preferably, the reaction temperature of the crosslinking reaction is less than 70°C, more preferably 20-70°C or 30-50°C.

[0126] Preferably, the reaction time of the crosslinking reaction is greater than 2 hours, more preferably 2-4 hours or 4-6 hours.

[0127] The hydroxyl-containing polymer, the ionic polymer, the organic solvent, the crosslinking agent, the dispersant, and their ratios and the conditions of the crosslinking reaction are adapted to the aforementioned microsphere portion.

[0128] Drug-loaded polymer microspheres

[0129] In another aspect, the present invention provides a drug-loaded polymeric microsphere, which is obtained by loading an antitumor drug onto the microspheres described above or the microspheres prepared by the above method.

[0130] The antitumor drug is preferably a charged drug, and the drug-loaded polymer microspheres are prepared by enriching and adsorbing the charged drug.

[0131] In one embodiment, the antitumor drug is preferably doxorubicin or pirarubicin.

[0132] The drug loading of the microspheres of the present invention is greater than 70%, and more particularly greater than 85% or 95%.

[0133] In one embodiment, the drug-loaded polymer microspheres are obtained by contacting the polymer microspheres with the antitumor drug.

[0134] In one embodiment, the contact can be achieved by dissolving the polymer microspheres and the antitumor drug together in an aqueous solution to allow the microspheres to adsorb the antitumor drug.

[0135] In one embodiment, the adsorption time does not exceed 60 minutes, and more specifically does not exceed 30 minutes or 15 minutes.

[0136] In another aspect, the present invention provides microspheres prepared by the above preparation method or the application of the above microspheres in the preparation of embolic agents, preferably, the embolic agent is a transcatheter arterial chemoembolic agent.

[0137] The method for preparing embolic microspheres of the present invention can obtain embolic microspheres through a one-step crosslinking reaction without the need for pre-grafting treatment of materials.

[0138] I. Definition

[0139] In this invention, unless otherwise stated, the scientific and technical terms used herein have the meanings commonly understood by those skilled in the art. Furthermore, the related terms and laboratory procedures used herein are all widely used terms and routine procedures in the respective fields. To better understand this invention, definitions and explanations of related terms are provided below.

[0140] As used herein and unless otherwise stated, the terms “about” or “approximately” mean within 10% of a given value or range. Where an integer is required, the term means within 10% of a given value or range, rounded up or down to the nearest integer.

[0141] In the description herein, references to “some embodiments,” “some implementations,” or “some implementations” describe a subset of all possible embodiments. However, it is understood that “some embodiments” may be the same subset or different subsets of all possible embodiments and may be combined with each other without conflict.

[0142] As used herein and unless otherwise stated, the terms “comprising,” “including,” “having,” “containing,” and their grammatically equivalent forms, including their grammatical equivalents, should generally be understood as open-ended and non-restrictive, e.g., not excluding other unlisted elements or steps.

[0143] As used herein, the term "reverse suspension polymerization" refers to a method in which reverse reactants are dispersed in an oil-soluble medium, an aqueous monomer solution is used as an aqueous phase droplet or particle, and a water-soluble initiator is dissolved in the aqueous phase to initiate polymerization.

[0144] As used herein, the term "swelling" refers to the phenomenon where a polymer expands in volume in a solvent. For example, ion exchange resins are hydrophilic polymers, and their volume often increases when dry ion exchange resin is immersed in water.

[0145] As used herein, the term "mass content" refers to the percentage of the mass of a specific substance in a solution relative to the total mass of the solution. For example, a 3% mass content of a water-soluble polymer containing hydroxyl groups in a crosslinked aqueous solution means that the mass of the water-soluble polymer containing hydroxyl groups accounts for 3% of the total mass of the crosslinked aqueous solution.

[0146] II. Examples

[0147] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below. The described embodiments should not be considered as limitations on the invention. All other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0148] Before providing a further detailed description of the embodiments of the present invention, the nouns and terms involved in the embodiments of the present invention will be explained, and the nouns and terms involved in the embodiments of the present invention shall be interpreted as follows.

[0149] The raw materials and equipment used in the specific implementation scheme disclosed herein are all known products and were obtained by purchasing commercially available products.

[0150] Example 1:

[0151] Step ①: Prepare a 15% polyvinyl alcohol solution: Add 85 mL of purified water to a 250 mL beaker, heat to 90 °C, weigh 15 g of polyvinyl alcohol (degree of hydrolysis 86.5%-89.0%, viscosity 4.5 mPa·s-6.1 mPa·s), slowly add it to the hot water, and stir until dissolved to obtain a 15% polyvinyl alcohol solution.

[0152] Step ②: Prepare a 10% sodium polyacrylate solution: Add 90 mL of purified water to a 250 mL beaker, heat to 85 °C, weigh 10 g of sodium polyacrylate (molecular weight 150,000), slowly add it to the hot water, and stir until dissolved to obtain a 10% sodium polyacrylate solution.

[0153] Step ③: Prepare an organic solvent (oil phase) containing a dispersant: Add 180 mL of butyl acetate to a 250 mL beaker, weigh 4.32 g of cellulose acetate butyrate, and stir until dissolved at room temperature to form a homogeneous oil phase.

[0154] Step 4: Prepare cross-linked aqueous solution (aqueous phase): Weigh 20g of polyvinyl alcohol solution from step ① and 10g of sodium polyacrylate solution from step ② into a 100mL beaker, stir to mix evenly, add 19g of purified water, add concentrated hydrochloric acid to adjust the pH of the solution to 4, and obtain a white suspension. Use an ultrasonic cell disruptor to perform multiple pulse ultrasonic treatments to obtain a uniformly dispersed white suspension.

[0155] Step 5: Preparation of embolic microspheres: The aqueous phase was slowly added dropwise to the oil phase while stirring to form a uniformly dispersed emulsion. 1.8 mL of 50% glutaraldehyde solution was added, and the mixture was continuously stirred at 40°C and 450 rpm for 4 hours. After stirring was stopped, the reaction system was filtered to remove the oil phase. The mixture was then soaked in 200 mL of pharmaceutical-grade ethanol for 10 minutes, and the ethanol was removed by filtration. This step was repeated twice. The mixture was then washed twice with 100 mL of ethyl acetate and dried under vacuum overnight. Scanning electron microscopy images of the obtained microspheres are shown below. Figure 1 .

[0156] Step 6: Soak the dried embolization microspheres in 50 mL of 1% sodium hydroxide solution for 10 min, filter to remove the sodium hydroxide solution, wash with purified water until the pH of the washing solution is 7, then boil the wet microspheres in 100 mL of purified water for 10 min, and filter through sieves with different pore sizes to obtain wet microspheres with different particle size ranges.

[0157] In step ④, the mass ratio of polyvinyl alcohol to sodium polyacrylate is 3:1.

[0158] The optical micrograph of the prepared wet bulb is shown in the image below. Figure 2 The transverse scan image from the top to the maximum cross-section under a laser confocal microscope after loading a multi-xonometric star is shown below. Figure 3 The transverse scanning image of the marketed product DCBead microspheres after drug loading, from the top to the maximum cross-section, is shown in the laser confocal microscope. Figure 4 .

[0159] The prepared microspheres are round, smooth, and well dispersed. After drug loading, the drug is adsorbed on the surface and evenly distributed.

[0160] If necessary, reactive blue can be used to selectively stain the microspheres to enhance their visibility. The specific staining method is as follows: Take 10 mL of fully hydrated microspheres, remove the supernatant purified water, weigh 0.1 g of reactive blue and dissolve it in 20 mL of water, weigh 0.08 g of sodium hydroxide and dissolve it in the reactive blue aqueous solution. After fully dissolving, mix the solution with 10 mL of microspheres and stir. Continue staining for 60 min. Filter the solution to remove the staining solution, and then wash it several times with purified water until free reactive blue is no longer detectable.

[0161] Example 2:

[0162] Compared to Example 1, Example 2 used high-viscosity polyvinyl alcohol (86.5%-89.0% degree of alcoholysis, viscosity 25.5 mPa·s-34.5 mPa·s). When preparing the aqueous phase, 22.5 g of a pre-prepared 10% polyvinyl alcohol solution and 15 g of a 10% sodium polyacrylate (molecular weight 150,000) solution were weighed and added to a 100 mL beaker, and stirred until homogeneous. 11.25 g of purified water was added, and concentrated hydrochloric acid was added to adjust the pH of the solution to 4, resulting in a white suspension. This suspension was then subjected to multiple pulsed sonication using an ultrasonic cell disruptor to obtain a uniformly dispersed white suspension. When preparing embolic microspheres by adding the aqueous phase to the oil phase and resuspending it at 40°C, 1.35 mL of 50% glutaraldehyde solution was added. In step ④, the mass ratio of polyvinyl alcohol to sodium polyacrylate was 3:2. Except for the above, the remaining steps were the same as in Example 1. A scanning electron microscope image of the microspheres before drying is shown below. Figure 5 The prepared microspheres are round, smooth, and well dispersed.

[0163] Example 3:

[0164] Compared to Example 1, Example 3 used high-viscosity polyvinyl alcohol (degree of hydrolysis 86.5%-89.0%, viscosity 25.5 mPa·s-34.5 mPa·s) and high-molecular-weight sodium polyacrylate (molecular weight 4,500,000). When preparing the aqueous phase, 22.5 g of the prepared 10% polyvinyl alcohol solution and 7.5 g of the 10% sodium polyacrylate solution were weighed and added to a 100 mL beaker, and stirred until homogeneous. 18.0 g of purified water was added, and concentrated hydrochloric acid was added to adjust the pH of the solution to 4, resulting in a white suspension. This suspension was then subjected to multiple pulsed sonication using an ultrasonic cell disruptor to obtain a uniformly dispersed white suspension. When preparing embolic microspheres by adding oil to the aqueous phase for phase re-suspension, 1.35 mL of 50% glutaraldehyde solution was added. In step ④, the mass ratio of polyvinyl alcohol to sodium polyacrylate was 3:1. Except for the above, the remaining steps were the same as in Example 1. The scanning electron microscope image of the microspheres before drying is shown below. Figure 6 The prepared microspheres are round, smooth, and well dispersed.

[0165] Example 4:

[0166] Compared with Example 2, the reaction temperature of Example 4-1 was set to 30°C and the reaction temperature of Example 4-2 was set to 60°C, while the other reaction conditions remained unchanged.

[0167] The results showed that the scanning electron microscope images of the microspheres before drying were as follows: Figure 7 (Example 4-1) Figure 8 (Example 4-2) It can be seen that when the reaction temperature is lowered to 30℃, the reaction rate slows down, and the spherical shape is not significantly different from that at the usual 40℃. When the temperature is raised to 60℃, the spherical formation is too fast, and the shape is not round enough.

[0168] Example 5:

[0169] Compared to Example 2, the volume ratio of the aqueous phase to the oil phase was adjusted from 1:4 to 1:1 (Example 5-1) and 1:8 (Example 5-2). In Example 5-1, the volume of the oil phase was changed to 45 mL, while the proportion of cellulose acetate butyrate in the oil phase remained unchanged. In Example 5-2, the volume of the aqueous phase (crosslinked aqueous solution) was halved to 22.5 mL, the concentrations of polyvinyl alcohol and sodium polyacrylate in the aqueous phase remained unchanged, and the amount of 50% glutaraldehyde added was halved to 0.675 mL. Except for the above, all other reaction conditions and steps were the same as in Example 2.

[0170] Results: Scanning electron microscopy images of the microspheres before drying are shown in the figures below. Figure 9 (Example 5-1) Figure 10(Example 5-2) It can be seen that when the volume ratio of water phase to oil phase is adjusted from 1:4 to 1:1, some of the spheres are agglomerated and the particle size distribution varies greatly. When adjusted to 1:8, the difference compared with 1:4 is not significant, and the particles are relatively dispersed.

[0171] Example 6:

[0172] Compared with Example 2, the reaction time was adjusted to 2 hours (Example 6-1) and 6 hours (Example 6-2), while other reaction conditions remained unchanged. During the reaction, a small amount of oil phase was taken out for thin-layer chromatography analysis. Based on the colorimetric reaction of 2,4-dinitrophenylhydrazine with the crosslinking agent glutaraldehyde, it was determined whether glutaraldehyde had reacted completely.

[0173] Results: Scanning electron microscopy images of the microspheres before drying are shown in the figures below. Figure 11 (Example 6-1) Figure 12 (Example 6-2) It can be seen that the spherical morphology is not significantly different between the reaction time of 2h and 6h and the usual 4h. According to the colorimetric reaction, glutaraldehyde still remains in the oil phase after 2h of reaction, while after 4h of reaction, glutaraldehyde has completely reacted and there is no residue.

[0174] Example 7:

[0175] Compared to Example 2, the oil phase was replaced with n-heptane instead of butyl acetate. The oil phase contained 180 mL of n-heptane and 3.60 g of Span 80. The remaining reaction conditions were the same as in Example 2.

[0176] Results: Scanning electron microscopy images of the prepared microspheres before drying are shown below. Figure 13 After switching to n-heptane, the spherical particles adhered significantly, resulting in poorer roundness. This posed a risk of rupture and catheter blockage, and also affected the embolization effect on the target vessel.

[0177] Example 8:

[0178] Compared to Example 2, the butyl acetate in the oil phase was replaced with liquid paraffin, and 3.6g of SPAN 80 was added to the oil phase. The remaining steps were the same as in Example 2.

[0179] Results: Scanning electron microscopy images of the prepared microspheres are shown in [the image]. Figure 14 As can be seen, the generated microspheres are stuck together and have a significantly smaller particle size, mostly between 5 and 10 μm.

[0180] Example 9:

[0181] Compared to Example 2, the hydrochloric acid used to adjust the pH value was changed from being added to the aqueous phase to being added to the oil phase after forming a homogeneous mixture in the aqueous phase, while the other reaction conditions remained unchanged.

[0182] Results: Scanning electron microscopy images of the prepared microspheres before drying are shown below. Figure 15When the aqueous phase is added to the oil phase to form a uniform mixture, hydrochloric acid is added to adjust the pH value. Some of the prepared microspheres have pores of different sizes on their surface, and many microspheres with irregular shapes and mutual adhesion appear.

[0183] Example 10:

[0184] Compared with Example 2, when processing the crudely prepared microspheres, the step of soaking in sodium hydroxide solution is omitted. After boiling in purified water, the microspheres are sieved and filtered through different sieves to obtain microspheres with different particle size ranges.

[0185] Results: Scanning electron microscopy images of the prepared microspheres before drying are shown below. Figure 16 By omitting the step of alkali washing of the crude microspheres, the drug loading of the prepared microspheres is reduced by nearly 30% compared with Example 2 under the same conditions, as detailed in Table 2.

[0186] Example 11:

[0187] Compared to Example 2, the dispersant cellulose acetate butyrate was not added, and the remaining steps were the same as in Example 2.

[0188] Scanning electron microscope images of the prepared microspheres are shown below. Figure 17 As can be seen, the generated microspheres are clearly stuck together, and many broken spheres are easily produced during washing.

[0189] Example 12:

[0190] Compared to Example 2, cellulose acetate butyrate was replaced with Span 80, and the remaining steps were the same as in Example 2.

[0191] Results: Scanning electron microscope images of the prepared microspheres are shown below. Figure 18 As can be seen, while the generated microspheres are clearly adhered to each other, many microspheres show signs of collapse and indentation.

[0192] Example 13:

[0193] Compared to Example 2, Example 13-1 reduced the amount of crosslinking agent glutaraldehyde, and the volume of added glutaraldehyde was reduced from 1.35 ml to 0.3375 ml. Compared to Example 2, Example 13-2 increased the amount of crosslinking agent glutaraldehyde to an excess, and the volume of added glutaraldehyde was reduced from 1.35 ml to 4.50 ml.

[0194] Results: Scanning electron microscope images of the microspheres prepared in Example 13-1 are shown below. Figure 19 As can be seen, the generated microspheres did not exhibit adhesion and maintained a good morphology. Table 1 shows the water content, and Table 2 shows the drug loading. Excessive reduction in glutaraldehyde content significantly increased the water content and reduced the drug loading capacity. Scanning electron microscopy images of the microspheres prepared in Example 13-2 are shown below. Figure 20As can be seen, the generated microspheres did not exhibit adhesion; however, some microspheres had irregular shapes. Table 1 shows the water content, and Table 2 shows the drug loading capacity. Increasing the glutaraldehyde content significantly reduced the water content and also worsened the drug loading capacity.

[0195] Comparative Example 1

[0196] The experiment was repeated according to the material ratio range specified in Example 4 of CN114917399A for polyvinyl alcohol and sodium polyacrylate, with the active pharmaceutical ingredient added to the aqueous phase and the drug loaded during the preparation process. This patented method requires the active pharmaceutical ingredient and excipients to be mixed during the preparation process.

[0197] Results: Significant loss of the active pharmaceutical ingredient (API) was observed during the preparation process, with a large amount of red API precipitating onto the microspheres. The actual drug loading and encapsulation efficiency were both very low. Furthermore, the drug loading process, limited by the storage conditions of the API, was detrimental to the subsequent sterilization and preservation of the microspheres. Compared to the method in this patent, which involves preparing blank microspheres and then re-adsorbing the API, the method disclosed in CN114917399A resulted in the loss of more than half of the API during the preparation process, with a drug loading of less than 50%.

[0198] Furthermore, over 80% of the microspheres prepared by this patent have a particle size distribution concentrated between 5-10 μm. Based on a conventional expansion ratio of 2-5, the expanded size would be far less than 100 μm. The "Guidelines for the Diagnosis and Treatment of Primary Liver Cancer (2022 Edition)" recommends a commonly used embolization microsphere size range of 100-300 μm, and 300-500 μm (after expansion) in the TACE procedure and classification section. The microsphere size disclosed in this patent is inferred to be far less than 100 μm after expansion, even less than 70 μm, which is unfavorable for clinical use after swelling.

[0199] Test Example 1: Moisture Content Test

[0200] The wet bulbs prepared in the example were placed in water. 1g of fully hydrated embolic microspheres were placed in a vial. The weight of the embolic microspheres was recorded as m0, and the total weight of the embolic microspheres and the vial was recorded as m1. The vials were baked at 100℃ for 15h. The total weight of the embolic microspheres and the vial was weighed again and recorded as m2. The samples were baked at 100℃ for another 0.5h, and the total weight of the embolic microspheres and the vial was weighed again and recorded as m3. If the difference between m2 and m3 was less than 0.3mg, it was considered constant weight. The water content was calculated according to the following formula. The water content results of the embolic microspheres are shown in Table 1.

[0201]

[0202] Table 1. Water content test results of embolization microspheres

[0203] experimental group Moisture content % Example 1 94.30% Example 2 95.60% Example 3 95.74% Example 4-1 94.12% Example 4-2 94.03% Example 5-1 94.23% Example 5-2 95.04% Example 6-1 95.55% Example 6-2 94.47% Example 7 94.71% Example 8 94.43% Example 9 95.71% Example 13-1 98.74% Example 13-2 81.26% CalliSpheres 95.05%

[0204] Moisture content can reflect swelling capacity to a certain extent. Lower moisture content indicates poorer swelling capacity, while higher moisture content indicates better swelling capacity. The embolic microspheres prepared in this invention have a moisture content comparable to that of Hengrui CalliSpheres embolic microspheres already on the market.

[0205] Test Example 2: Drug Loading Test

[0206] 10 mg of doxorubicin hydrochloride lyophilized powder was placed in a vial, 4 mL of purified water was added, and the mixture was shaken to dissolve. 20 μL of the solution was taken and diluted to obtain the 0 min sample. Based on the water content of the embolic microspheres prepared in each example, embolic microspheres equivalent to 10 mg of their dry weight were added to the above doxorubicin hydrochloride solution. The mixture was shaken and mixed frequently. At 15 min, 30 min, and 60 min, 20 μL of each sample was taken and diluted. The UV absorbance of the sample at 483 nm was measured using a UV spectrophotometer, and the drug loading of the embolic microspheres at different drug loading times was calculated. The drug loading test results of the embolic microspheres are shown in Table 2. The drug loading curves of the microspheres prepared in Examples 1, 2, and 3 are shown in Table 2. Figure 21 .

[0207] Table 2. Results of doxorubicin adsorption on embolization microspheres

[0208]

[0209]

[0210] Example 2 used a polyvinyl alcohol to sodium polyacrylate excipient ratio of 3:2, while the corresponding excipient ratio in Examples 1 and 3 was 3:1. Example 2 introduced more drug-carrying ionic groups, resulting in stronger drug loading capacity, and the experimental results were largely in line with theoretical expectations.

[0211] Test Example 3: Compressibility Test

[0212] Using an SMS TA.XT PlusC property testing instrument, 1 mL of the embolic microspheres prepared in each example was drawn from the sample using a dropper and dropped into the groove of a custom-made iron plate. Excess solution and microspheres were removed, and the remaining microspheres were spread evenly in the groove. The testing requirements were as follows: a 5 mm diameter P / 5 cylindrical probe was used, the sensing element was 5 kg, the speed was 1 mm / s, the compression control mode was used, and the microspheres were compressed to 20% of their diameter. The elastic modulus of the embolic microspheres was then tested. The test results are shown in Table 3. Each sample was measured at least 3 times, and the average value was taken.

[0213] Table 3. Test results of elastic modulus of embolized microspheres

[0214]

[0215] The elastic modulus is the ratio of stress to strain; the higher the value, the less easily it deforms. Embolizing microspheres require a certain range of deformation capacity. The elastic modulus of the microspheres prepared by this invention is superior to that of the commercially available microsphere product DC Bead.

[0216] Test Example 4: In Vitro Release Test

[0217] Take the drug-loaded microspheres of doxorubicin hydrochloride from Example 2, loaded according to the method described in Test Example 2, and transfer them all to a 500 mL Nalgene bottle. Rinse with 500 mL of release medium (0.9% sodium chloride), place at 37°C and rotate at 500 rpm, and take 1 mL samples at 1 h, 2 h, 3 h, 4 h, 17 h, 24 h, 48 h, and 72 h for determination by high performance liquid chromatography. Add 1 mL of isothermal release medium as needed.

[0218] Chromatographic conditions: An octadecylsilane-bonded silica gel column was used as the chromatographic column, and gradient elution was performed using 0.1% trifluoroacetic acid aqueous solution as solution A and acetonitrile-methanol-trifluoroacetic acid (800:200:1) as solution B. The column temperature was 35℃ and the detection wavelength was 254nm.

[0219] Using the same processing and testing conditions, the product was compared with the commercially available DC Bead microspheres. The in vitro release comparison curves are shown below. Figure 22 The microspheres prepared by this invention have comparable in vitro release performance to the aforementioned microsphere DC Bead, with a release rate exceeding 90% after 72 hours.

[0220] Table 4. In vitro release test results of embolic microspheres

[0221] sample 1h 2h 3h 4h 17h 24h 48h 72h Example 2 26.05% 34.87% 40.54% 43.19% 68.43% 77.38% 87.87% 92.23% DC bead 24.29% 38.86% 51.31% 61.77% 81.67% 87.90% 92.14% 92.40%

[0222] Test Example 5: Stability after drug loading

[0223] Drug-loaded microspheres containing doxorubicin hydrochloride were placed at 37°C according to the method described in Test Example 2. During the test, they were transferred to a 500 mL Nalgene bottle and eluted at 37°C and 500 rpm for 7 h by rotating in 500 mL of KCl-saturated ethanol solution (200 g of potassium chloride was weighed into 1 L of ultrapure water, dissolved, and then 1 L of anhydrous ethanol was added to saturate the solution). After 7 h, 1 mL of the solution was taken, centrifuged, and determined by high performance liquid chromatography. The changes in the main peak doxorubicin and impurity peaks (such as impurities produced by the decomposition of doxorubicin) were statistically analyzed.

[0224] Chromatographic conditions: An octadecylsilane-bonded silica column was used. Gradient elution was performed using 0.1% trifluoroacetic acid aqueous solution as solution A and acetonitrile-methanol-trifluoroacetic acid (800:200:1) as solution B. The column temperature was 35℃ and the detection wavelength was 254nm. After adsorption, elution was performed with KCl-ethanol at 37℃ for 7 h at 500 rpm. The changes in the main peak and impurity peaks were statistically analyzed.

[0225] Table 5. Percentage of main peak of active pharmaceutical ingredient and impurity peak after KCl elution of drug-loaded microspheres

[0226]

[0227]

[0228] The microspheres prepared by this invention maintained a purity of over 95% after 7 days of drug loading, and remained above 88% after 14 days. This is significantly superior to the commercially available microsphere product HepaSphere, which has a purity of 81.47% after 7 days of drug loading.

[0229] Test Example 6: Exudate Limit Test

[0230] Take about 0.5g of blank microspheres into a vial, accurately add 3.5mL of ultrapure water, sterilize and dispense, take the supernatant and centrifuge at 10000rpm for 10 minutes, filter through a 0.45μm microporous membrane, and determine by high performance liquid chromatography.

[0231] Chromatographic conditions: Using size-exclusion columns (such as BioBasic) TM The mobile phase was 0.1% TFA:water:acetonitrile (1:700:300). Flow rate: 0.6 mL / min; detector: RID 35℃; column temperature: 30℃; injection volume: 50 μL.

[0232] Table 6. Determination of leachate content under different media conditions.

[0233]

[0234] After being placed at 40°C for 6 months, the polyvinyl alcohol content of the prepared embolization microspheres remained below 0.05%, meeting the requirements. No sodium polyacrylate precipitation was detected.

[0235] The foregoing description of specific exemplary embodiments of the invention is for illustrative and explanatory purposes. These descriptions are not intended to limit the invention to the precise forms disclosed, and it will be apparent that many changes and variations can be made in accordance with the foregoing teachings. The exemplary embodiments were chosen and described in order to explain the specific principles of the invention and its practical application, thereby enabling those skilled in the art to implement and utilize various different exemplary embodiments of the invention, as well as various different choices and variations. The scope of the invention is intended to be defined by the claims and their equivalents.

Claims

1. Polymer microspheres, characterized in that, The polymer microspheres comprise cross-linked polymeric compounds containing hydroxyl groups, as well as polymeric compounds containing ionic groups; The polymer microspheres are formed by cross-linking a polymer compound containing hydroxyl groups with a cross-linking agent to form a spherical skeleton, and the spherical skeleton encapsulates a polymer compound containing ionic groups; The raw materials for preparing the polymer microspheres include polymeric compounds containing hydroxyl groups, polymeric compounds containing ionic groups, crosslinking agents, and dispersants; The hydroxyl-containing polymer compound is polyvinyl alcohol; The polymeric compound containing ionic groups is sodium polyacrylate; The crosslinking agent is glutaraldehyde; The dispersant is cellulose acetate butyrate; The mass ratio of the polymer containing hydroxyl groups to the polymer containing ionic groups is (0.5-5):1; The mass ratio of the dispersant to the hydroxyl-containing polymer compound is (4-5):(1-4); The mass ratio of the crosslinking agent to the hydroxyl-containing polymer compound is (0.1-0.6):1; The polymer microspheres are prepared by a method comprising the following steps: forming a cross-linked aqueous solution by combining a polymer compound containing hydroxyl groups and a polymer compound containing ionic groups; the pH of the cross-linked aqueous solution is less than or equal to 5; adding the cross-linked aqueous solution to an organic solvent containing a dispersant, adding a cross-linking agent to carry out a cross-linking reaction, thereby obtaining the polymer microspheres; the cross-linking reaction is a one-step cross-linking reaction; and washing the polymer microspheres obtained by the cross-linking reaction with alkali. The volume ratio of the cross-linked aqueous solution to the organic solvent is 1:(4-8); The organic solvents mentioned do not include hydrocarbon solvents.

2. The microspheres according to claim 1, wherein, The viscosity of the hydroxyl-containing polymer compound is 1 mPa·s-50 mPa·s.

3. The microspheres according to claim 1, wherein, The organic solvent is ethyl acetate and / or butyl acetate.

4. The microspheres according to claim 1, wherein, The reaction temperature for the crosslinking reaction is 30-50℃.

5. The microspheres according to claim 1, wherein, The cross-linking reaction takes 2-6 hours.

6. The microspheres according to claim 1, wherein, The average particle size of the microspheres after swelling is greater than or equal to 100 μm.

7. The microspheres according to claim 1, wherein, The microspheres have a water content greater than 80% after swelling.

8. A method for preparing polymer microspheres, comprising the following steps: A cross-linked aqueous solution is formed by combining a polymer containing hydroxyl groups and a polymer containing ionic groups. The pH of the cross-linked aqueous solution is less than or equal to 5; The crosslinking aqueous solution is added to an organic solvent containing a dispersant, and a crosslinking agent is added to carry out a crosslinking reaction to obtain the polymer microspheres; The crosslinking reaction is a one-step crosslinking reaction; The polymer microspheres were subjected to alkaline washing; The hydroxyl-containing polymer compound is polyvinyl alcohol; The polymeric compound containing ionic groups is sodium polyacrylate; The crosslinking agent is glutaraldehyde; The dispersant is cellulose acetate butyrate; The mass ratio of the polymer containing hydroxyl groups to the polymer containing ionic groups is (0.5-5):1; The mass ratio of the dispersant to the hydroxyl-containing polymer compound is (4-5):(1-4); The mass ratio of the crosslinking agent to the hydroxyl-containing polymer compound is (0.1-0.6):1; The volume ratio of the cross-linked aqueous solution to the organic solvent is 1:(4-8); The organic solvents mentioned do not include hydrocarbon solvents.

9. The preparation method according to claim 8, wherein, The organic solvent is ethyl acetate and / or butyl acetate.

10. The preparation method according to claim 8, wherein, The reaction temperature for the crosslinking reaction is 30-50℃.

11. The preparation method according to claim 8, wherein, The cross-linking reaction takes 2-6 hours.

12. Drug-loaded polymeric microspheres, which are obtained by loading antitumor drugs onto polymeric microspheres prepared by any one of claims 1-7 or by any one of claims 8-11.

13. The drug-loaded polymer microspheres according to claim 12, wherein, The antitumor drug is a charged antitumor drug.

14. The drug-loaded polymer microspheres according to claim 12, wherein, The antitumor drug is doxorubicin or pirarubicin.

15. The drug-loaded polymer microspheres according to claim 12, wherein, The drug-loaded polymer microspheres are obtained by contacting the polymer microspheres with the antitumor drug, wherein the contact is achieved by dissolving the polymer microspheres and the antitumor drug together in an aqueous solution so that the polymer microspheres adsorb the antitumor drug.

16. The use of the polymer microspheres according to any one of claims 1-7, the polymer microspheres prepared by the preparation method according to any one of claims 8-11, or the drug-loaded polymer microspheres according to any one of claims 12-15 in the preparation of embolic agents.

17. The application according to claim 16, wherein, The embolic agent is a transcatheter arterial chemoembolization agent.

Citation Information

Patent Citations

  • Three polymer microspheres as well as preparation method and application thereof

    CN114917399A

  • Developable polyvinyl alcohol microballoon / particle embolic agent and preparation process thereof

    CN102139128A

  • Drug-loaded embolism microsphere with developing function and preparation method thereof

    CN111569144A