A citric acid chelated titanium, its preparation method and application
By reacting citric acid with ammonium carbonate to generate a mixed solution of ammonium citrate, which is then neutralized and complexed with titanium hydroxide, the problem of complex preparation process and insufficient chelation strength of existing titanium fertilizers is solved. This achieves high chelation strength and good water solubility, making it suitable for water-soluble micronutrient fertilizers for agricultural color change.
Patent Information
- Application Number
- CN202311302245.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-10
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-10-10
AI Technical Summary
Existing titanium fertilizer preparation processes are complex and have weak chelation strength, making them incompatible with major fertilizers such as potassium dihydrogen phosphate, which leads to inconvenience in agricultural use.
A mixed solution of ammonium citrate is generated by reacting citric acid with ammonium carbonate. This solution is then neutralized and complexed with freshly prepared titanium hydroxide to form citric acid chelated titanium, which enhances the chelation strength and improves the compatibility with potassium dihydrogen phosphate.
The prepared citric acid chelated titanium has high chelation strength and is compatible with potassium dihydrogen phosphate in aqueous solution for a long time. It has good water solubility, which simplifies the preparation process and improves the convenience of agricultural application.
Smart Images

Figure BDA0004484965020000101 
Figure BDA0004484965020000111 
Figure BDA0004484965020000112
Abstract
Description
Technical Field
[0001] This invention relates to the field of chemical synthesis technology, and more specifically, to a citrate chelated titanium, its preparation method, and its application. Background Technology
[0002] During plant growth and development, titanium can not only promote crop growth and development, enhance the plant's ability to produce nutrients through photosynthesis, increase the activity of nitrogenase, peroxidase, nitrate reductase, and 2-6 phosphatase in the plant, mobilize endogenous hormones to transport to the growth center, promote differentiation and induce callus tissue, but also greatly improve the internal quality of crop fruits, increasing color and sweetness.
[0003] Patent document CN109824506A discloses a method for preparing the plant growth regulator titanium ammonium citrate. The titanium source is titanium tetrachloride, titanium sulfate, tetrabutyl titanate, and titanium nitrate. These react with an alkaline solution below 5°C to form an acid-soluble titanium precipitate, which is then reacted with citric acid until a clear state is achieved. Finally, the pH is adjusted to slightly alkaline using ammonia. This method has harsh and complex process conditions, and according to its reaction mechanism, it only utilizes acid-base neutralization to generate a simple inorganic salt, which releases titanium ions in water, making it unsuitable for simultaneous use with high-phosphorus fertilizers. Patent document CN112250478A discloses a method for preparing a fully water-soluble titanium fertilizer. The titanium raw material used is a refined titanium solution, an intermediate product of titanium dioxide. One or more of the following are selected as small-molecule chelating agents: citric acid, mannitol, sorbitol, glucose, amino acids, ascorbic acid, and tartaric acid, to chelate and complex the refined titanium solution. Although the titanium fertilizer prepared by this method has good water solubility, it also suffers from poor compatibility with major fertilizers such as potassium dihydrogen phosphate due to weak chelation strength. Patent document CN108456016A discloses a method for preparing water-soluble organic titanium fertilizer, which uses the hydrolysis of orthotitanate ester and chelation complexation reaction with gluconic acid ligands; patent document CN112961000A discloses a water-soluble titanium fertilizer containing tranexamic acid, which is prepared by uniformly mixing adjuvants, water-soluble titanium compounds and tranexamic acid raw materials. The above-mentioned existing titanium fertilizer preparation technologies are not only complex in preparation process, but also suffer from weak chelation strength with titanium, making them unable to be mixed with major fertilizers such as potassium dihydrogen phosphate, causing inconvenience in agricultural use.
[0004] In view of this, the present invention is proposed. Summary of the Invention
[0005] The purpose of this invention is to provide a citrate chelated titanium, its preparation method, and its application.
[0006] This invention is implemented as follows:
[0007] In a first aspect, the present invention provides a method for preparing citrate chelated titanium, comprising reacting freshly prepared titanium hydroxide with a mixed solution of citric acid and ammonium citrate to obtain citrate chelated titanium.
[0008] A mixed solution of citric acid and ammonium citrate is prepared by reacting citric acid with ammonium carbonate.
[0009] In an optional embodiment, the mass ratio of citric acid to ammonium carbonate is 0.8–1.2:0.2–0.3.
[0010] Preferably, the concentration of citric acid is 400-600 g / L, and the ammonium carbonate is a block solid.
[0011] Preferably, the reaction time between citric acid and ammonium carbonate is 3 to 60 minutes.
[0012] In an optional embodiment, the preparation of the newly prepared titanium hydroxide includes reacting titanium oxysulfate with an alkaline solution, wherein the solute in the alkaline solution includes any one of sodium carbonate, sodium hydroxide, potassium carbonate, potassium hydroxide, ammonium carbonate, or ammonia water.
[0013] Preferably, the mass ratio of titanium oxysulfate to alkaline solution is 0.8-1.2:0.6-1.
[0014] Preferably, the concentration of titanium oxysulfate is 300-400 g / L, and the concentration of solute in the alkaline solution is 200-300 g / L.
[0015] In an optional embodiment, the reaction temperature of titanium oxysulfate with alkaline solution is 20–35°C, and the reaction time is 40–80 min.
[0016] Preferably, titanium hydroxide is obtained by precipitation at 10–50°C after the reaction is completed.
[0017] In an optional embodiment, the reaction temperature of titanium hydroxide with the mixed solution of citric acid and ammonium citrate is 80–100°C, and the reaction time is 60–120 min.
[0018] In an optional embodiment, the reaction solution is further concentrated after the reaction is complete.
[0019] Preferably, the thermal specific gravity of the concentrated reaction solution is 1.25 to 1.30.
[0020] In an optional embodiment, the concentrated solution is further dried.
[0021] In an optional implementation, the drying method is spray drying.
[0022] Preferably, the inlet air temperature of the spray dryer is 200-220°C, and the outlet air temperature is 105-110°C.
[0023] Secondly, the present invention provides a citrate chelated titanium, which is prepared by any of the preparation methods described in the foregoing embodiments.
[0024] Thirdly, the present invention provides an application of citric acid chelated titanium prepared by any of the foregoing embodiments as a water-soluble micronutrient fertilizer for color change in agriculture.
[0025] The present invention has the following beneficial effects:
[0026] This invention provides a citric acid chelated titanium, its preparation method, and its application. In particular, ammonium carbonate is selected as an enhancer for citric acid chelation. First, it reacts with citric acid to prepare a mixed solution of citric acid and ammonium citrate. This mixed solution and freshly prepared titanium hydroxide achieve simultaneous neutralization and complexation reactions. The two reactions promote each other, and the final citric acid chelated titanium has high chelation strength, is compatible with potassium dihydrogen phosphate in aqueous solution for a long time, and has good water solubility. Detailed Implementation
[0027] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0028] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0029] In a first aspect, the present invention provides a method for preparing citrate chelated titanium, comprising reacting freshly prepared titanium hydroxide with a mixed solution of citric acid and ammonium citrate to obtain citrate chelated titanium.
[0030] A mixed solution of citric acid and ammonium citrate is prepared by reacting citric acid with ammonium carbonate.
[0031] Citric acid is a ternary organic acid with a hydroxyl group. Under acidic conditions, its overall chelating ability is weak. When it reacts with metal ions, it is difficult to form stable cyclic complexes. This results in poor compatibility between citric acid chelated titanium and potassium dihydrogen phosphate, which are prepared by directly reacting citric acid with titanium compounds. They are difficult to be miscible with potassium dihydrogen phosphate for a long time. Therefore, they need to be prepared on the spot, which increases the operation in the actual application process. The inventors specifically selected ammonium carbonate as an enhancer for citric acid chelation. First, it reacts with citric acid monohydrate to prepare a mixed solution of citric acid and ammonium citrate. This mixed solution, along with freshly prepared titanium hydroxide, allows for simultaneous neutralization and complexation reactions. Specifically, citric acid partially neutralizes ammonium carbonate, generating some ammonium citrate, thus forming a mixed solution of citric acid and ammonium citrate. Then, the ammonium citrate generated from the neutralization reaction undergoes a complexation reaction with the freshly prepared titanium hydroxide, promoting the forward reaction between citric acid and ammonium carbonate. The two reactions mutually promote each other, ultimately producing citric acid chelated titanium. This chelation has high strength, is readily soluble in potassium dihydrogen phosphate in aqueous solution for an extended period, exhibits good water solubility (solid product solubility ≥80g), and the titanium content in the citric acid chelated titanium solution is ≥60g / L.
[0032] In an optional embodiment, to improve reaction efficiency, the mass ratio of citric acid to ammonium carbonate is 0.8–1.2:0.2–0.3.
[0033] Preferably, the concentration of citric acid is 400-600 g / L, and the ammonium carbonate is a block solid.
[0034] Preferably, the reaction time between citric acid and ammonium carbonate is 3 to 60 minutes.
[0035] In an optional embodiment, the preparation of the newly prepared titanium hydroxide includes reacting titanium oxysulfate with an alkaline solution, wherein the solute in the alkaline solution includes any one of sodium carbonate, sodium hydroxide, potassium carbonate, potassium hydroxide, ammonium carbonate, or ammonia water, preferably sodium carbonate.
[0036] When the solute in the alkaline solution is sodium carbonate, preferably, the mass ratio of titanium oxysulfate to sodium carbonate is 0.8-1.2:0.6-1.
[0037] Preferably, the concentration of titanium oxysulfate is 300-400 g / L and the concentration of sodium carbonate is 200-300 g / L.
[0038] In an optional embodiment, the reaction temperature of titanium oxysulfate with sodium carbonate is 20–35°C, and the reaction time is 40–80 min.
[0039] Preferably, the process of dissolving titanium oxysulfate in water to prepare a titanium oxysulfate solution includes heating the solution at a temperature of 50–60°C to ensure a clear solution is obtained.
[0040] Preferably, titanium hydroxide is precipitated at 10–50°C after the reaction. Currently, the preparation of titanium hydroxide using titanium sulfate requires strict control of the precipitation temperature to ensure successful precipitation; generally, the reaction temperature needs to be controlled at 5°C or below, increasing the complexity of the preparation process. However, this application uses titanium oxysulfate as a raw material to react with sodium carbonate, eliminating the need for strict temperature control. The reaction can proceed at room temperature or slightly above room temperature, precipitating titanium hydroxide and simplifying the preparation process.
[0041] In an optional embodiment, the reaction temperature of titanium hydroxide with the mixed solution of citric acid and ammonium citrate is 80–100°C, and the reaction time is 60–120 min.
[0042] In an optional embodiment, in order to prepare solid citrate chelated titanium, the citrate chelated titanium solution needs to be dried. To further improve the drying efficiency, the reaction solution is also concentrated after the reaction is completed.
[0043] Preferably, the thermal specific gravity of the concentrated reaction solution is 1.25 to 1.30, for example, it can be 1.25, 1.26, 1.27, 1.28, 1.29 or 1.30.
[0044] In an optional embodiment, the concentrated solution is further dried.
[0045] In an optional embodiment, spray drying is used to obtain citric acid chelated titanium solids with uniform particle size.
[0046] Preferably, the inlet air temperature for spray drying is 200–220°C, for example, 200°C, 205°C, 210°C, 215°C, or 220°C. The outlet air temperature is 105–110°C, for example, 105°C, 106°C, 107°C, 108°C, 109°C, or 110°C.
[0047] In some embodiments, the method for preparing citrate-chelated titanium provided by the present invention includes the following steps:
[0048] S01. Dissolve titanium oxysulfate in pure water and heat until clear to obtain titanium oxysulfate solution. Dissolve sodium carbonate in pure water to obtain sodium carbonate solution, add sodium carbonate solution to titanium oxysulfate solution and react at room temperature to form titanium hydroxide precipitate. After filtration, wash the solid with pure water and filter a second time to obtain titanium hydroxide solid.
[0049] S02. Dissolve citric acid in pure water, add ammonium carbonate to neutralize it, and prepare a mixed solution of citric acid and ammonium citrate.
[0050] S03. After adding solid titanium hydroxide to a mixed solution of citric acid and ammonium citrate, a citric acid chelated titanium solution is obtained.
[0051] S04. Concentrate the citric acid chelated titanium solution until the solution is clear and the thermal specific gravity is 1.25-1.30. Then spray dry the concentrated solution to obtain solid citric acid chelated titanium.
[0052] Secondly, the present invention provides a citrate chelated titanium, which is prepared by any of the preparation methods described in the foregoing embodiments.
[0053] Thirdly, the present invention provides an application of citric acid chelated titanium prepared by any of the foregoing embodiments as a water-soluble micronutrient fertilizer for color change in agriculture.
[0054] Example 1
[0055] This embodiment provides a method for preparing citrate-chelated titanium, comprising the following steps:
[0056] S01. Dissolve 1 part of titanium oxysulfate in 3 parts of pure water and accelerate the dissolution at 50-60℃ to obtain a titanium oxysulfate solution. Dissolve 0.8 parts of sodium carbonate in 3 parts of pure water to obtain a sodium carbonate solution. Add the sodium carbonate solution to the titanium oxysulfate solution and react at room temperature (25℃) for 1 hour to form titanium hydroxide precipitate. After filtration, wash the solid with pure water and filter a second time to obtain solid titanium hydroxide.
[0057] S02. Dissolve 1 part citric acid in 2 parts pure water, add 0.25 parts ammonium carbonate to neutralize, and a mixed solution of citric acid and ammonium citrate is generated.
[0058] S03. Add titanium hydroxide precipitate to a mixed solution of citric acid and ammonium citrate, and react at 95°C for 80 min to obtain a citric acid chelated titanium solution.
[0059] S04. The citric acid chelated titanium solution was placed in a beaker and concentrated by stirring and heating until the specific gravity of the concentrated solution was 1.275. The concentrated solution was then spray-dried at an inlet air temperature of 220°C and an outlet air temperature of 110°C.
[0060] Example 2
[0061] This embodiment provides a method for preparing citrate-chelated titanium, comprising the following steps:
[0062] S01. Dissolve 1 part of titanium oxysulfate in 3 parts of pure water, accelerate the dissolution and clarify at 50-60℃ to obtain a titanium oxysulfate solution. Dissolve 0.8 parts of ammonium carbonate in 3 parts of pure water to obtain an ammonium carbonate solution. Add the ammonium carbonate solution to the titanium oxysulfate solution and react at room temperature (25℃) for 1 hour to generate titanium hydroxide precipitate. After filtration, wash the solid with pure water and filter a second time to obtain solid titanium hydroxide.
[0063] S02. Dissolve 1 part citric acid in 2 parts pure water, add 0.25 parts ammonium carbonate to neutralize, and a mixed solution of citric acid and ammonium citrate is generated.
[0064] S03. Add titanium hydroxide precipitate to a mixed solution of citric acid and ammonium citrate, and react at 95°C for 80 min to obtain a citric acid chelated titanium solution.
[0065] S04. The citric acid chelated titanium solution is placed in a beaker and heated and stirred to concentrate it until the specific gravity of the solution is 1.275. The concentrate is then spray-dried at an inlet air temperature of 220℃ and an outlet air temperature of 110℃.
[0066] Example 3
[0067] This embodiment provides a method for preparing citrate chelated titanium, which is the same as that in Example 1, except that the reaction raw material sodium carbonate is replaced with potassium carbonate.
[0068] Example 4
[0069] This embodiment provides a method for preparing citrate chelated titanium, which is the same as that in Example 1, except that the amount of titanium oxysulfate is reduced from one part to 0.8 parts.
[0070] Example 5
[0071] This embodiment provides a method for preparing citric acid chelated titanium, which is the same as that in Example 2, except that in step S01, the raw material ammonium carbonate for precipitating titanium hydroxide is replaced with ammonia.
[0072] Example 6
[0073] This embodiment provides a method for preparing citrate chelated titanium, which is the same as that in Example 2, except that the amount of titanium oxysulfate is reduced from one part to 0.8 parts.
[0074] Comparative Example 1
[0075] S01. Dissolve 1 part of titanium oxysulfate in 3 parts of pure water and accelerate the dissolution at 50-60℃ to obtain a titanium oxysulfate solution. Dissolve 0.8 parts of sodium carbonate in 3 parts of pure water to obtain a sodium carbonate solution. Add the sodium carbonate solution to the titanium oxysulfate solution and react at room temperature (25℃) for 1 hour to form titanium hydroxide precipitate. After filtration, wash the solid with pure water and filter a second time to obtain solid titanium hydroxide.
[0076] S02. Dissolve 1 part citric acid in 2 parts pure water, stir until dissolved and clear.
[0077] S03. Add titanium hydroxide precipitate to an aqueous citric acid solution and react at 95°C for 80 min to obtain a titanium citrate solution.
[0078] S04. The titanium citrate solution is placed in a beaker and concentrated by stirring and heating. The specific gravity of the concentrated solution is 1.275. The concentrated solution is then spray-dried at an inlet air temperature of 220°C and an outlet air temperature of 110°C.
[0079] Comparative Example 2
[0080] S01. Dissolve 1 part of titanium oxysulfate in 3 parts of pure water and accelerate the dissolution at 50-60℃ to obtain a titanium oxysulfate solution. Dissolve 0.8 parts of sodium carbonate in 3 parts of pure water to obtain a sodium carbonate solution. Add the sodium carbonate solution to the titanium oxysulfate solution and react at room temperature (25℃) for 1 hour to form titanium hydroxide precipitate. After filtration, wash the solid with pure water and filter a second time to obtain solid titanium hydroxide.
[0081] S02. Dissolve 1 part citric acid in 2 parts pure water, stir until dissolved and clear.
[0082] S03. Add titanium hydroxide precipitate to an aqueous citric acid solution and react at 95°C for 80 min to obtain a titanium citrate solution.
[0083] S04. Add an appropriate amount of ammonia to the titanium citrate aqueous solution cooled to room temperature (25°C) to carry out a neutralization reaction.
[0084] S05. The titanium ammonium citrate solution is placed in a beaker and concentrated by stirring and heating. The specific gravity of the concentrated solution is 1.275. The concentrated solution is then spray-dried at an inlet air temperature of 220°C and an outlet air temperature of 110°C.
[0085] Experimental Example 1
[0086] The citrate chelated titanium prepared in Examples 1-6 were tested, and the results are shown in Table 1.
[0087] The testing method is as follows: GB5009.268-2016 Method I.
[0088] Table 1. Titanium content of citric acid chelated titanium
[0089]
[0090]
[0091] As shown in Table 1, the method provided by this invention can stably synthesize citrate chelated titanium, and the process route is reasonable. Raw materials such as sodium carbonate, potassium carbonate, sodium hydroxide, potassium hydroxide, ammonium carbonate, and ammonia can all be used to precipitate titanium hydroxide and achieve the same precipitation effect. Adjusting the amount of titanium oxysulfate raw material has a stable effect on the titanium content and pH value of titanium ammonium citrate.
[0092] Experimental Example 2
[0093] A 50 g / L potassium dihydrogen phosphate solution was prepared using distilled water. 1 g of titanium citrate prepared in Example 1, Comparative Example 1, and Comparative Example 2 was taken and mixed with 100 ml of the 50 g / L potassium dihydrogen phosphate solution, respectively. The results are as follows:
[0094]
[0095]
[0096] As shown in Table 2, by first neutralizing citric acid and ammonium carbonate, some ammonium citrate is generated in the solution. The mixture of ammonium citrate and citric acid is then neutralized and complexed with freshly prepared titanium hydroxide, which can significantly enhance its chelation strength. The citric acid chelated titanium prepared by this method can be co-soluble with potassium dihydrogen phosphate for a long time.
[0097] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for the preparation of citrate chelated titanium, characterized by, This includes reacting freshly prepared titanium hydroxide with a mixed solution of citric acid and ammonium citrate to prepare citric acid chelated titanium; The mixed solution of citric acid and ammonium citrate is prepared by reacting citric acid with ammonium carbonate.
2. The production method according to claim 1, characterized by, The mass ratio of citric acid to ammonium carbonate is 0.8~1.2:0.2~0.
3.
3. The preparation method according to claim 1, characterized in that, The concentration of citric acid is 400~600g / L, and the ammonium carbonate is a blocky solid.
4. The preparation method according to claim 1, characterized in that, The reaction time between citric acid and ammonium carbonate is 3 to 60 minutes.
5. The preparation method according to claim 1, characterized in that, The preparation of the newly prepared titanium hydroxide involves reacting titanium oxysulfate with an alkaline solution, wherein the solute in the alkaline solution includes any one of sodium carbonate, sodium hydroxide, potassium carbonate, potassium hydroxide, ammonium carbonate, or ammonia water.
6. The preparation method according to claim 5, characterized in that, The mass ratio of titanium oxysulfate to alkaline solution is 0.8~1.2:0.6~1.
7. The preparation method according to claim 5, characterized in that, The concentration of the titanium oxysulfate is 300~400g / L, and the concentration of the solute in the alkaline solution is 200~300g / L.
8. The preparation method according to any one of claims 5 to 7, characterized in that, The reaction temperature of the titanium oxysulfate with the alkaline solution is 20~35℃, and the reaction time is 40~80min; after the reaction is completed, titanium hydroxide is obtained by precipitation at 10~50℃.
9. The preparation method according to claim 1, characterized in that, The reaction temperature of the titanium hydroxide with the mixed solution of citric acid and ammonium citrate is 80~100℃, and the reaction time is 60~100min.
10. The preparation method according to claim 9, characterized in that, After the reaction is complete, the reaction solution is concentrated, and the thermal specific gravity of the concentrated reaction solution is 1.25~1.
30.
11. The preparation method according to claim 10, characterized in that, It also includes drying the concentrated solution.
12. The preparation method according to claim 11, characterized in that, The drying method is spray drying; The inlet air temperature for spray drying is 200~220℃, and the outlet air temperature is 105~110℃.
Citation Information
Patent Citations
Water-soluble organic titanium fertilizer and preparation method thereof
CN108456016A
Preparation method of plant growth regulator ammonium titanate citrate
CN109824506A
Full water-soluble titanium fertilizer and preparation method thereof
CN112250478A
Tranexamic acid-containing water-soluble titanium fertilizer and application method thereof
CN112961000A
Titanium compounds
CA825704A