Microcapsule, microcapsule preservative coating and preparation method
By using microcapsules with a core of chlorinated rubber solution and a capsule wall of dimethyl diallyl ammonium chloride polymer, the problems of easy rusting and bubble formation in epoxy zinc-rich coatings have been solved, achieving continuous protection of the substrate.
Patent Information
- Application Number
- CN202311403477.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-10-26
AI Technical Summary
Existing epoxy zinc-rich coatings are prone to rusting and blistering, resulting in insufficient protection of the substrate to meet practical requirements.
Microcapsules with a core of chlorinated rubber solution and a wall of dimethyl diallyl ammonium chloride polymer are used. By controlling the wall thickness and component ratio, a stable microcapsule structure is formed. When rust or blistering occurs at the coating markings, the capsule wall slowly breaks down, and the core material is slowly released, providing continuous protection.
It extends the protective time of the coating, improves the protective effect on the substrate, and avoids rapid damage to the coating film.
Smart Images

Figure CN117362690B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of anti-corrosion coating preparation technology, and in particular to a microcapsule, a microcapsule anti-corrosion coating, and a preparation method thereof. Background Technology
[0002] Anti-corrosion coatings, as a type of protective product, provide excellent protection for substrates and are widely used in industries such as steel structures, petrochemicals, and wind power.
[0003] Epoxy zinc-rich coatings can be prepared with different zinc contents, resulting in anti-corrosion coating products of 60%, 70%, and 80%, with corresponding salt spray resistance times of 200 hours, 400 hours, and 600 hours, respectively. During salt spray resistance testing, rust and bubbles gradually form on the scribing areas of the coating. These rust and bubbles gradually increase and extend outward until they exceed 2 mm, reaching the standard limit for coating damage. This seriously affects the protective effect of the anti-corrosion coating on the substrate. Therefore, there is an urgent need for a new anti-corrosion coating additive or anti-corrosion coating to solve the above technical problems. Summary of the Invention
[0004] To address the technical problem that existing epoxy zinc-rich coatings are prone to rusting and blistering, resulting in insufficient protection of the substrate, this invention provides microcapsules, microcapsule anti-corrosion coatings, and a preparation method thereof. Therefore, this invention is achieved through the following technical solution.
[0005] In a first aspect, the present invention provides a microcapsule, wherein the core of the microcapsule is a chlorinated rubber solution, the capsule wall is a dimethyl diallyl ammonium chloride polymer with a wall thickness of 30-80 nm and a particle size of 1-2 μm; wherein the concentration of the chlorinated rubber solution is 35-45 wt%.
[0006] Compared with existing technologies, the microcapsules of this invention have a core made of chlorinated rubber solution and a wall composed of dimethyl diallyl ammonium chloride polymer. These microcapsules possess a relatively rigid outer shell, ensuring stability during use. When used in anti-corrosion coatings, after the coating film is formed, the microcapsules can be distributed relatively evenly within the coating. When rust or blistering at the coating's marked areas causes further damage, the specific thickness of the microcapsule wall material in this invention exhibits a good match between the rate of damage and the destructive force. The capsule wall is slowly damaged, and the core material encapsulated within is slowly released, thus protecting the substrate, preventing further damage, and extending the protection time. In particular, the use of chlorinated rubber solution for the core in this invention gives it excellent corrosion resistance.
[0007] Furthermore, the microcapsule loading rate is 80-90%.
[0008] Secondly, the present invention provides a method for preparing microcapsules, applied to the above-mentioned microcapsules, comprising:
[0009] Under stirring conditions, chlorinated rubber resin is added to the first solvent and mixed evenly to obtain a chlorinated rubber solution; the concentration of the chlorinated rubber solution is 35-45 wt%.
[0010] Under stirring conditions, the chlorinated rubber solution and photoinitiator are added to the second solvent and mixed evenly to obtain an oil phase; the mass ratio of the chlorinated rubber solution, photoinitiator and second solvent added is 50:(1~2):(120~150);
[0011] Under stirring conditions, an aqueous solution of dimethyl diallyl ammonium chloride and the oil phase are added to a third solvent; wherein the mass ratio of the added amount of the third solvent, the aqueous solution of dimethyl diallyl ammonium chloride and the oil phase is 1:(150-120):(35-40). The mixture is stirred until homogeneous, irradiated with ultraviolet light until the reaction is complete, stirring is stopped, and the mixture is filtered, impurities are removed, and dried to obtain microcapsules.
[0012] Compared with existing technologies, the microcapsule preparation method of this invention involves adding chlorinated rubber resin to a first solvent and mixing thoroughly to obtain a chlorinated rubber solution. Controlling the concentration of the chlorinated rubber solution to 35-45 wt% ensures that the viscosity of the resulting microcapsule core material is suitable. This allows the chlorinated rubber solution to flow out quickly upon rupture during use, forming a thicker protective coating. Adding the chlorinated rubber solution and a photoinitiator to a second solvent and stirring thoroughly yields an oil phase. Adding an aqueous solution of dimethyl diallyl ammonium chloride and the oil phase to a third solvent forms an oil-in-water emulsion. Since the oil-in-water emulsion contains a photoinitiator, after ultraviolet light irradiation and the reaction complete, the surface of the oil-in-water emulsion solidifies into a film, forming a microcapsule structure. In the microcapsules prepared by this invention, the core is a chlorinated rubber solution, and the capsule wall is composed of a dimethyl diallyl ammonium chloride polymer. Furthermore, by controlling the mass ratio of each component, optimal synergistic effects can be achieved. In particular, the microcapsule wall material of a specific thickness exhibits a good match between its failure rate under external force and the elongation failure force. As the capsule wall is slowly broken down, the core material encapsulated within the capsule is slowly released, thus providing optimal protection for the coated object. Based on the above description, the microcapsules, when applied to the field of anti-corrosion coatings, solve the technical problems of existing epoxy zinc-rich coatings being prone to rusting and blistering, resulting in poor protection of the substrate and failing to meet practical requirements.
[0013] Furthermore, in the method for preparing the microcapsules of the present invention, the first solvent includes xylene;
[0014] The second solvent includes dichloromethane;
[0015] The third solvent includes an aqueous solution of polyvinyl alcohol with a mass concentration of 0.5–2 wt%;
[0016] The concentration of the aqueous solution of dimethyl diallyl ammonium chloride is 1–5 wt%.
[0017] Furthermore, in the method for preparing microcapsules of the present invention, the filtration, impurity removal, and drying include:
[0018] The product obtained after ultraviolet irradiation was filtered, washed with deionized water to remove impurities, and then dried at a temperature of 15–55°C to obtain the microcapsules.
[0019] Furthermore, in the preparation method of the microcapsules of the present invention, the photoinitiator includes (2,4,6-trimethylbenzoyl)-diphenylphosphine oxide.
[0020] Thirdly, the present invention provides a microcapsule anticorrosive coating, comprising a main agent and a hardener. The main agent comprises 10-20 wt% epoxy resin, 65-70 wt% zinc powder, 5-10 wt% fourth solvent, 8-10 wt% microcapsules, 1-2 wt% anti-settling agent, 0.5-2 wt% dispersant, and 0-0.5 wt% defoamer. In the microcapsule anticorrosive coating, the mass ratio of the main agent to the hardener is 10:(0.8-1).
[0021] Compared with the prior art, the beneficial effects of the microcapsule anticorrosive coating of the present invention are the same as the beneficial effects of the microcapsule preparation method described in the above technical solution, and will not be repeated here.
[0022] Furthermore, in the microcapsule anticorrosive coating of the present invention, the fourth solvent includes xylene and butanol; the anti-settling agent includes any one or two of bentonite and polyamide wax;
[0023] The hardener comprises 30-40 wt% of a curing agent resin and 60-70 wt% of a fifth solvent, wherein the curing agent resin comprises one or two of phenolic amine resin and polyamide resin; the fifth solvent comprises xylene and butanol, and the viscosity of the anti-corrosion coating is 110-130 KU.
[0024] Fourthly, the present invention provides a method for preparing a microcapsule anticorrosive coating, which is applied to the above-mentioned microcapsule anticorrosive coating, comprising:
[0025] According to the content of each component in the main agent, the epoxy resin, fourth solvent, dust suppressant, dispersant and defoamer are mixed and stirred at a stirring speed of 800-1000 rpm until they are uniformly mixed to obtain a mixture.
[0026] The stirring speed of the mixture is controlled at 1200-1450 rpm, and the zinc powder is added to the mixture. Stirring is continued until the particle size in the mixture is ≤50μm to obtain the paint slurry.
[0027] The stirring rate of the paint slurry is controlled at 800-1000 rpm, and the microcapsules are added to the paint slurry and stirred evenly to obtain the main agent;
[0028] The curing agent resin was added to the fifth solvent at a stirring speed of 800-1000 rpm and stirred until homogeneous to obtain the hardener.
[0029] The main agent and the hardener are mixed evenly to obtain the microcapsule anticorrosive coating, wherein the mass ratio of the main agent to the hardener is 10:(0.8-1).
[0030] Compared with the prior art, the beneficial effects of the preparation method of the microcapsule anticorrosive coating of the present invention are the same as those of the preparation method of microcapsules described in the above technical solution, and will not be repeated here.
[0031] Furthermore, in the preparation method of the microcapsule anticorrosive coating of the present invention, the dispersant includes a modified polyurethane dispersant and a modified polyacrylate dispersant.
[0032] The defoaming agents include polysiloxane defoamers and polyether defoamers. Attached Figure Description
[0033] The accompanying drawings, which are included to provide a further understanding of the invention and form part of this invention, illustrate exemplary embodiments of the invention and are used to explain the invention, but do not constitute an undue limitation of the invention. In the drawings:
[0034] Figure 1 This is a schematic flowchart of the microcapsule preparation method provided in Embodiment 1 of the present invention. Detailed Implementation
[0035] To make the technical problems to be solved, the technical solutions, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the present invention and are not intended to limit the present invention.
[0036] Epoxy zinc-rich coatings can be prepared with different zinc contents, such as 60%, 70%, and 80%, to produce anti-corrosion coating products with corresponding salt spray resistance times of 200 hours, 400 hours, and 600 hours, respectively. During salt spray resistance testing, rust and bubbles gradually form on the scratched areas of the coating. These rust and bubbles gradually increase and extend outward until they exceed 2 mm, reaching the standard limit for coating damage and seriously affecting the protective effect of the anti-corrosion coating on the substrate.
[0037] To address the aforementioned technical problems, in a first aspect, the present invention provides a microcapsule, wherein the core of the microcapsule is a chlorinated rubber solution, the capsule wall is a dimethyl diallyl ammonium chloride polymer with a thickness of 30-80 nm, and the particle size is 1-2 μm; wherein the concentration of the chlorinated rubber solution is 35-45 wt%.
[0038] Using the above technical solution, the microcapsules of the present invention have a core of chlorinated rubber solution and a capsule wall composed of dimethyl diallyl ammonium chloride polymer. These microcapsules possess a relatively hard outer shell, ensuring stability during use. When used in anti-corrosion coatings, after the coating film is formed, the microcapsules can be relatively evenly distributed within the coating. When rust or blistering at the coating's marked areas causes further damage, the specific thickness of the microcapsule wall material of the present invention exhibits a good match between the rate of damage and the destructive force. The capsule wall is slowly damaged, and the core material encapsulated within is slowly released, thereby protecting the substrate, preventing further damage, and extending the protection time. In particular, the chlorinated rubber solution used for the core of the present invention provides excellent corrosion resistance.
[0039] It should be understood that in order to effectively control the slow release of the chlorinated rubber solution, prevent the spread of damage, and extend the protection time, it is also necessary to control the loading rate and encapsulation rate of the microcapsules. For example, the loading rate of the microcapsules is 80-90%.
[0040] Secondly, the present invention provides a method for preparing microcapsules, comprising:
[0041] Under stirring conditions, chlorinated rubber resin is added to the first solvent and mixed evenly to obtain a chlorinated rubber solution; the concentration of the chlorinated rubber solution is 35-45 wt%.
[0042] Under stirring conditions, the chlorinated rubber solution and photoinitiator are added to the second solvent and mixed evenly to obtain an oil phase; the mass ratio of the chlorinated rubber solution, photoinitiator and second solvent added is 50:(1~2):(120~150);
[0043] Under stirring conditions, an aqueous solution of dimethyl diallyl ammonium chloride and the oil phase are added to a third solvent; wherein the mass ratio of the added amount of the third solvent, the aqueous solution of dimethyl diallyl ammonium chloride and the oil phase is 1:(150-200):(35-40). The mixture is stirred until homogeneous, irradiated with ultraviolet light until the reaction is complete, stirring is stopped, and the mixture is filtered, impurities are removed, and dried to obtain microcapsules.
[0044] Using the above technical solution, in the preparation method of the microcapsules of the present invention, a chlorinated rubber solution is obtained by adding chlorinated rubber resin to a first solvent and mixing it evenly. Controlling the concentration of the chlorinated rubber solution to 35-45 wt% ensures that the viscosity of the obtained microcapsule core material is suitable. During use, when the microcapsule ruptures, the chlorinated rubber solution can flow out at a relatively fast speed, forming a thicker protective coating. An oil phase is obtained by adding the chlorinated rubber solution and a photoinitiator to a second solvent and stirring evenly. An oil-in-water emulsion is formed by adding an aqueous solution of dimethyl diallyl ammonium chloride and the oil phase to a third solvent. Since the oil-in-water emulsion contains a photoinitiator, after ultraviolet light irradiation and the reaction is complete, the surface of the oil-in-water emulsion solidifies into a film, forming a microcapsule structure. In the microcapsules prepared by the present invention, the core is a chlorinated rubber solution, and the capsule wall is composed of a dimethyl diallyl ammonium chloride polymer. Furthermore, by controlling the mass ratio of each component, the components can achieve the best synergistic effect. In particular, when a microcapsule wall material of a specific thickness is prepared, its destruction rate under external force is well matched with the extension destruction force. After the capsule wall is slowly destroyed, the core material encapsulated in the capsule is slowly released, thereby achieving the best protection for the coated object.
[0045] It should be understood that in the preparation method of the microcapsules of the present invention, in order to improve the solubility of chlorinated rubber resin in the first solvent, it is also necessary to control the type of the first solvent. For example, the first solvent can be xylene. Similarly, in order to improve the solubility of the chlorinated rubber solution and the photoinitiator in the second solvent, thereby obtaining a uniformly mixed oil phase, it is also necessary to control the type of the second solvent. For example, the second solvent can be dichloromethane. It should also be understood that in order to obtain a regular oil-in-water emulsion, it is also necessary to control the type of the third solvent. For example, the third solvent can be a 0.5-2 wt% aqueous solution of polyvinyl alcohol. It should also be understood that in order to obtain microcapsules with regular spherical shape and high loading capacity, it is also necessary to control the concentration of the dimethyl diallyl ammonium chloride aqueous solution and the mass ratio of the added third solvent, the dimethyl diallyl ammonium chloride aqueous solution, and the oil phase. For example, the concentration of the dimethyl diallyl ammonium chloride aqueous solution can be 1-5 wt%, and in another example, the concentration of the dimethyl diallyl ammonium chloride aqueous solution can be 1 wt%, 3 wt%, or 5 wt%.
[0046] In one possible implementation, the filtration, impurity removal, and drying processes in the microcapsule preparation method of the present invention include:
[0047] The product obtained after ultraviolet irradiation was filtered, washed with deionized water to remove impurities, and then dried at a temperature of 15–55°C to obtain the microcapsules.
[0048] Using the above technical solution, the product obtained after ultraviolet light irradiation contains liquid and solid impurities. These impurities can be removed by filtration and washing with deionized water, thus achieving impurity removal. The removed product is then dried to obtain microcapsules. It should be understood that to avoid damaging the microcapsule structure or causing excessive hardening of the capsule wall during the drying process, which would affect the outflow of the core liquid, the present invention also requires control of the drying temperature. For example, the drying temperature can be 15–55°C; in another example, the drying temperature can be 15°C, 20°C, 40°C, or 55°C.
[0049] It should be understood that in the preparation method of the microcapsules of the present invention, the photoinitiator can be further controlled to be (2,4,6-trimethylbenzoyl)-diphenylphosphine oxide. Under specific photoinitiator types and component ratios, the obtained polymer capsule wall thickness is between 30 and 80 nm, ensuring that the hardening degree of the capsule shell is within a reasonable range, thus avoiding affecting the outflow of the core liquid. This allows for the preparation of microcapsules with a loading capacity of 80-90%.
[0050] Thirdly, the present invention provides a microcapsule anticorrosive coating, comprising a main agent and a hardener. The main agent comprises 10-20 wt% epoxy resin, 65-70 wt% zinc powder, 5-10 wt% fourth solvent, 8-10 wt% microcapsules, 1-2 wt% anti-settling agent, 0.5-2 wt% dispersant, and 0-0.5 wt% defoamer. In the microcapsule anticorrosive coating, the mass ratio of the main agent to the hardener is 10:(0.8-1).
[0051] Using the above technical solution, in the microcapsule anticorrosive coating of the present invention, the main agent is used to form the matrix, the addition of the hardener allows the main agent to harden and form in a short time, the addition of the anti-settling agent is used to prevent the coating from forming sediment and affecting the product's storability, the addition of the dispersant to the microcapsule anticorrosive coating can reduce the time and energy required for each component to complete the dispersion process, and stabilize the dispersed body; the addition of the defoamer to the microcapsule anticorrosive coating can effectively inhibit or reduce the formation of bubbles, thereby improving the coating efficiency and coating quality, and enhancing the gloss and smoothness of the coating surface, while also avoiding the problem of pitting in the coating. Adding microcapsules to the main agent allows the microcapsules to be distributed relatively evenly in the coating after film formation. When rust or blistering at the coating's marked points causes the coating to extend and break, the destruction rate of the microcapsule wall material of the present invention has a good matching effect with the extending destructive force. The capsule wall is slowly destroyed, and the core material encapsulated in the capsule is slowly released, thereby protecting the substrate, preventing the extension of damage, and achieving the purpose of extending the protection time. It should be understood that, in order to improve the performance of the microcapsule anticorrosive coating, the mass ratio of the main agent to the hardener is controlled to be 10:(0.8-1). For example, the mass ratio of the main agent to the hardener can be 10:0.8, 10:0.9 or 10:1.
[0052] It should also be understood that, in order to achieve the best synergistic effect among the components in the microcapsule anticorrosive coating, the present invention controls the content of each component in the main agent as follows: epoxy resin 10-20 wt%, zinc powder 65-70 wt%, fourth solvent 5-10 wt%, microcapsules 8-10 wt%, anti-settling agent 1-2 wt%, dispersant 0.5-2 wt%, and defoamer 0-0.5 wt%. For example, the content of epoxy resin can be 10 wt%, 15 wt%, or 20 wt%, the content of zinc powder can be 65 wt%, 68 wt%, or 70 wt%, the content of microcapsules can be 8 wt%, 9 wt%, or 10 wt%, the content of anti-settling agent can be 1 wt%, 1.5 wt%, or 2 wt%, the content of fourth solvent can be 5 wt%, 8 wt%, or 10 wt%, the content of dispersant can be 0.5 wt%, 1 wt%, or 2 wt%, and the content of defoamer can be 0.1 wt%, 0.2 wt%, or 0.4 wt%.
[0053] It should be understood that in order to improve the dispersion or dissolution ability of the fourth solvent on each component and reduce the drying time of the microcapsule anticorrosive coating, it is also necessary to control the type of the fourth solvent. For example, the fourth solvent may be xylene or butanol. At the same time, in order to promote the curing effect of the epoxy resin in the coating, it is also necessary to control the type of curing agent resin and the fifth solvent in the hardener. For example, the curing agent resin includes one or two of phenolic amine resin and polyamide resin, and the fifth solvent includes xylene or butanol.
[0054] Furthermore, under the above-mentioned curing agent resin and fifth solvent types and ratios, the viscosity of the anti-corrosion coating can reach 110-130 KU. At this viscosity, the prepared microcapsule anti-corrosion coating has an ideal coating effect. Of course, in specific examples, the viscosity of the anti-corrosion coating can be 110 KU, 120 KU or 130 KU.
[0055] Fourthly, the present invention provides a method for preparing a microcapsule anticorrosive coating, which is applied to the above-mentioned microcapsule anticorrosive coating, comprising:
[0056] According to the content of each component in the main agent, the epoxy resin, fourth solvent, dust suppressant, dispersant and defoamer are mixed and stirred at a stirring speed of 800-1000 rpm until they are uniformly mixed to obtain a mixture.
[0057] The stirring speed of the mixture is controlled at 1200-1450 rpm, and the zinc powder is added to the mixture. Stirring is continued until the particle size in the mixture is ≤50μm to obtain the paint slurry.
[0058] The stirring rate of the paint slurry is controlled at 800-1000 rpm, and the microcapsules are added to the paint slurry and stirred evenly to obtain the main agent;
[0059] The curing agent resin was added to the fifth solvent at a stirring speed of 800-1000 rpm and stirred until homogeneous to obtain the hardener.
[0060] The main agent and the hardener are mixed evenly to obtain the microcapsule anticorrosive coating, wherein the mass ratio of the main agent to the hardener is 10:(0.8-1).
[0061] Compared with the prior art, the beneficial effects of the preparation method of the microcapsule anti-corrosion coating of the present invention are the same as those of the above-mentioned microcapsule preparation method. Furthermore, during the preparation of the main agent, zinc powder and microcapsules work synergistically, primarily for corrosion prevention. By first adding zinc powder to the mixture and stirring until the particle size is ≤50μm, the structure of the microcapsules is avoided from being damaged due to excessively large zinc powder particles in the paint slurry when the microcapsules are subsequently added.
[0062] It should be understood that, in order to further improve the performance of microcapsule anticorrosive coatings, the types of dispersants and defoamers should also be controlled. For example, the dispersants include modified polyurethane dispersants and modified polyacrylate dispersants; the defoamers include polysiloxane defoamers and polyether defoamers.
[0063] To better understand the present invention, the following specific embodiments further illustrate the content of the present invention, but the content of the present invention is not limited to the following embodiments.
[0064] Unless otherwise specified, all raw materials used in the following examples are commercially available.
[0065] Example 1
[0066] This embodiment provides a microcapsule A, wherein the core of the microcapsule A is a chlorinated rubber solution, the capsule wall is a dimethyl diallyl ammonium chloride polymer, the concentration of the chlorinated rubber solution is 35 wt%, the average particle size of the microcapsule A is 2 μm, and the encapsulation rate of the microcapsule A is 85%.
[0067] The preparation method of microcapsule A described in this embodiment includes the following steps:
[0068] S100, under stirring conditions, chlorinated rubber resin is added to dichloromethane and mixed evenly to obtain a chlorinated rubber solution. The concentration of the chlorinated rubber solution is 35 wt%, the stirring speed is 800 rpm, and the stirring time is 65 min.
[0069] S200, under stirring conditions, the chlorinated rubber solution and photoinitiator are added to dichloromethane and mixed evenly to obtain an oil phase; wherein, the mass ratio of the chlorinated rubber solution, photoinitiator and dichloromethane is 50:1:120, the photoinitiator is (2,4,6-trimethylbenzoyl)-diphenylphosphine oxide, the stirring speed is 800 rpm, and the stirring time is 65 min;
[0070] S300, under stirring conditions, dimethyl diallyl ammonium chloride aqueous solution and the oil phase are added to a 0.5 wt% polyvinyl alcohol aqueous solution; after mixing evenly, the mixture is irradiated with ultraviolet light until the reaction is complete, stirring is stopped, the mixture is filtered, washed with deionized water to remove impurities, and then dried at a temperature of 15°C to obtain the microcapsule A;
[0071] The concentration of the dimethyl diallyl ammonium chloride aqueous solution is 1 wt%, and the mass ratio of the added polyvinyl alcohol aqueous solution, dimethyl diallyl ammonium chloride aqueous solution and oil phase is 1:150:35; the stirring speed is 800 rpm, and the stirring time is 65 min.
[0072] Example 2
[0073] This embodiment provides a microcapsule B, wherein the core of the microcapsule B is a chlorinated rubber solution, the capsule wall is a dimethyl diallyl ammonium chloride polymer, the concentration of the chlorinated rubber solution is 45 wt%, the average particle size of the microcapsule B is 1.5 μm, and the encapsulation rate of the microcapsule B is 88%.
[0074] The preparation method of microcapsule B described in this embodiment includes the following steps:
[0075] S100, under stirring conditions, chlorinated rubber resin is added to dichloromethane and mixed evenly to obtain a chlorinated rubber solution with a concentration of 45 wt%, a stirring rate of 800 rpm, and a stirring time of 65 min.
[0076] S200, under stirring conditions, the chlorinated rubber solution and photoinitiator are added to dichloromethane and mixed evenly to obtain an oil phase; wherein, the mass ratio of the chlorinated rubber solution, photoinitiator and dichloromethane is 50:2:150, the photoinitiator is (2,4,6-trimethylbenzoyl)-diphenylphosphine oxide, the stirring speed is 800 rpm, and the stirring time is 65 min;
[0077] S300, under stirring conditions, dimethyl diallyl ammonium chloride aqueous solution and the oil phase are added to a 2 wt% polyvinyl alcohol aqueous solution; after mixing evenly, the mixture is irradiated with ultraviolet light until the reaction is complete, stirring is stopped, the mixture is filtered, washed with deionized water to remove impurities, and then dried at a temperature of 55°C to obtain the microcapsule B;
[0078] The concentration of the dimethyl diallyl ammonium chloride aqueous solution is 5 wt%, and the mass ratio of the added polyvinyl alcohol aqueous solution, dimethyl diallyl ammonium chloride aqueous solution and oil phase is 1:200:40; the stirring speed is 800 rpm, and the stirring time is 65 min.
[0079] Example 3
[0080] This embodiment provides a microcapsule C, wherein the core of the microcapsule C is a chlorinated rubber solution, the capsule wall is a dimethyl diallyl ammonium chloride polymer, the concentration of the chlorinated rubber solution is 40 wt%, the average particle size of the microcapsule C is 1.5 μm, and the encapsulation loading rate of the microcapsule C is 87%.
[0081] The preparation method of microcapsule C described in this embodiment includes the following steps:
[0082] S100, under stirring conditions, chlorinated rubber resin is added to dichloromethane and mixed evenly to obtain a chlorinated rubber solution. The concentration of the chlorinated rubber solution is 40 wt%, the stirring speed is 800 rpm, and the stirring time is 65 min.
[0083] S200, under stirring conditions, the chlorinated rubber solution and photoinitiator are added to dichloromethane and mixed evenly to obtain an oil phase; wherein, the mass ratio of the chlorinated rubber solution, photoinitiator and dichloromethane is 50:1.5:140, the photoinitiator is (2,4,6-trimethylbenzoyl)-diphenylphosphine oxide, the stirring rate is 800 rpm, and the stirring time is 65 min;
[0084] S300, under stirring conditions, dimethyl diallyl ammonium chloride aqueous solution and the oil phase are added to a 1 wt% polyvinyl alcohol aqueous solution; after mixing evenly, the mixture is irradiated with ultraviolet light until the reaction is complete, stirring is stopped, the mixture is filtered, washed with deionized water to remove impurities, and then dried at a temperature of 35°C to obtain the microcapsule C;
[0085] The concentration of the dimethyl diallyl ammonium chloride aqueous solution is 3 wt%, and the mass ratio of the added polyvinyl alcohol aqueous solution, dimethyl diallyl ammonium chloride aqueous solution and oil phase is 1:170:38; the stirring speed is 800 rpm, and the stirring time is 65 min.
[0086] Example 4
[0087] This embodiment provides a microcapsule D, wherein the core of the microcapsule D is a chlorinated rubber solution, the capsule wall is a dimethyl diallyl ammonium chloride polymer, the concentration of the chlorinated rubber solution is 42 wt%, the average particle size of the microcapsule D is 1 μm, and the encapsulation loading rate of the microcapsule D is 86.5%.
[0088] The preparation method of microcapsule D described in this embodiment includes the following steps:
[0089] S100, under stirring conditions, chlorinated rubber resin is added to dichloromethane and mixed evenly to obtain a chlorinated rubber solution. The concentration of the chlorinated rubber solution is 42 wt%, the stirring rate is 800 rpm, and the stirring time is 65 min.
[0090] S200, under stirring conditions, the chlorinated rubber solution and photoinitiator are added to dichloromethane and mixed evenly to obtain an oil phase; wherein, the mass ratio of the chlorinated rubber solution, photoinitiator and dichloromethane is 50:2:130, the photoinitiator is (2,4,6-trimethylbenzoyl)-diphenylphosphine oxide, the stirring speed is 800 rpm, and the stirring time is 65 min;
[0091] S300, under stirring conditions, dimethyl diallyl ammonium chloride aqueous solution and the oil phase are added to a 1 wt% polyvinyl alcohol aqueous solution; after mixing evenly, the mixture is irradiated with ultraviolet light until the reaction is complete, stirring is stopped, the mixture is filtered, washed with deionized water to remove impurities, and then dried at a temperature of 40°C to obtain the microcapsules D;
[0092] The concentration of the dimethyl diallyl ammonium chloride aqueous solution is 3 wt%, and the mass ratio of the added polyvinyl alcohol aqueous solution, dimethyl diallyl ammonium chloride aqueous solution and oil phase is 1:180:39; the stirring speed is 800 rpm, and the stirring time is 65 min.
[0093] The following examples use microcapsule anticorrosive coatings and their preparation methods as examples for illustration. The microcapsule anticorrosive coatings include the microcapsules listed in Examples 1 to 4. Specific examples are as follows.
[0094] Example 5
[0095] This embodiment provides a microcapsule anticorrosive coating, comprising a main agent and a hardener. The mixing mass ratio of the main agent to the hardener in the microcapsule anticorrosive coating is 10:0.8. The main agent comprises 10 wt% epoxy resin, 65 wt% zinc powder, 8 wt% xylene, 2 wt% butanol, 10 wt% microcapsule A, 1 wt% bentonite, 1.8 wt% polyamide wax, 2 wt% modified polyurethane dispersant, and 0.2 wt% polysiloxane defoamer. The hardener consists of 30 wt% phenolic amine resin, 50 wt% xylene, and 20 wt% butanol. The viscosity of the anticorrosive coating is 110 KU.
[0096] The preparation method of the microcapsule anticorrosive coating described in this embodiment includes the following steps:
[0097] S100, according to the content of each component in the main agent, the epoxy resin, xylene, butanol, bentonite, modified polyurethane dispersant and polysiloxane defoamer are stirred at a stirring speed of 800 rpm until they are mixed evenly to obtain a mixture.
[0098] S200, control the stirring speed of the mixture to 1200 rpm, add the zinc powder to the mixture, and continue stirring until the particle size in the mixture is ≤50μm to obtain the paint slurry;
[0099] S300, control the stirring speed of the paint slurry to 800 rpm, and add the polyamide wax and microcapsule A to the paint slurry, stir evenly, and obtain the main agent;
[0100] S400, under a stirring speed of 800 rpm, the phenolic amine resin is added to the xylene and butanol, and stirred evenly to obtain the hardener;
[0101] S500, the main agent and the hardener are mixed evenly to obtain the microcapsule anti-corrosion coating, wherein the mixing mass ratio of the main agent and the hardener is 10:0.8.
[0102] Example 6
[0103] This embodiment provides a microcapsule anticorrosive coating, comprising a main agent and a hardener. The mixing mass ratio of the main agent to the hardener in the microcapsule anticorrosive coating is 10:1. The main agent comprises 15 wt% epoxy resin, 70 wt% zinc powder, 4.3 wt% xylene, 1 wt% butanol, 8 wt% microcapsule B, 1 wt% polyamide wax, 0.5 wt% modified polyurethane dispersant, and 0.2 wt% polysiloxane defoamer. The hardener consists of 40 wt% polyamide resin, 40 wt% xylene, and 20 wt% butanol. The viscosity of the anticorrosive coating is 116 KU.
[0104] The preparation method of the microcapsule anticorrosive coating described in this embodiment includes the following steps:
[0105] S100, according to the content of each component in the main agent, the epoxy resin, xylene, butanol, modified polyurethane dispersant and polysiloxane defoamer are mixed and stirred at a stirring speed of 1000 rpm until they are uniformly mixed to obtain a mixture.
[0106] S200, control the stirring speed of the mixture to 1450 rpm, add the zinc powder to the mixture, and continue stirring until the particle size in the mixture is ≤50μm to obtain the paint slurry;
[0107] S300, control the stirring speed of the paint slurry to 1000 rpm, and add the polyamide wax and microcapsule B to the paint slurry, stir evenly, and obtain the main agent;
[0108] S400, under a stirring speed of 1000 rpm, the polyamide resin is added to xylene and butanol, and stirred evenly to obtain the hardener;
[0109] S500, the main agent and the hardener are mixed evenly to obtain the microcapsule anti-corrosion coating, wherein the mixing mass ratio of the main agent and the hardener is 10:1.
[0110] Example 7
[0111] This embodiment provides a microcapsule anticorrosive coating, comprising a main agent and a hardener. The mixing mass ratio of the main agent to the hardener in the microcapsule anticorrosive coating is 10:1. The main agent comprises 10 wt% epoxy resin, 70 wt% zinc powder, 5.6 wt% xylene, 2 wt% butanol, 9 wt% microcapsule C, 1 wt% bentonite, 2 wt% modified polyurethane dispersant, and 0.4 wt% polysiloxane defoamer. The hardener consists of 35 wt% polyamide resin, 45 wt% xylene, and 20 wt% butanol. The viscosity of the anticorrosive coating is 130 KU.
[0112] The preparation method of the microcapsule anticorrosive coating described in this embodiment includes the following steps:
[0113] S100, according to the content of each component in the main agent, the epoxy resin, xylene, butanol, bentonite, modified polyurethane dispersant and polysiloxane defoamer are mixed and stirred at a stirring speed of 850 rpm until they are uniformly mixed to obtain a mixture.
[0114] S200, control the stirring speed of the mixture to 1300 rpm, add the zinc powder to the mixture, and continue stirring until the particle size in the mixture is ≤50μm to obtain the paint slurry;
[0115] S300, control the stirring speed of the paint slurry to 900 rpm, and add the microcapsule C to the paint slurry, stir evenly, and obtain the main agent;
[0116] S400, under a stirring speed of 900 rpm, the phenolic amine resin is added to the xylene and butanol, and stirred evenly to obtain the hardener;
[0117] S500, the main agent and the hardener are mixed evenly to obtain the microcapsule anti-corrosion coating, wherein the mixing mass ratio of the main agent and the hardener is 10:1.
[0118] Example 8
[0119] This embodiment provides a microcapsule anticorrosive coating, comprising a main agent and a hardener. The mixing mass ratio of the main agent to the hardener in the microcapsule anticorrosive coating is 9:1. The main agent comprises 19 wt% epoxy resin, 65 wt% zinc powder, 4 wt% xylene, 1 wt% butanol, 8 wt% microcapsule D, 1.5 wt% bentonite, 1 wt% modified polyurethane dispersant, and 0.5 wt% polysiloxane defoamer. The hardener consists of 38 wt% polyamide resin, 43 wt% xylene, and 19 wt% butanol. The viscosity of the anticorrosive coating is 128 KU.
[0120] The preparation method of the microcapsule anticorrosive coating described in this embodiment includes the following steps:
[0121] S100, according to the content of each component in the main agent, the epoxy resin, xylene, butanol, bentonite, modified polyurethane dispersant and polysiloxane defoamer are mixed and stirred at a stirring speed of 900 rpm until they are uniformly mixed to obtain a mixture.
[0122] S200, control the stirring speed of the mixture to 1250 rpm, add the zinc powder to the mixture, and continue stirring until the particle size in the mixture is ≤50μm to obtain the paint slurry;
[0123] S300, control the stirring speed of the paint slurry to 850 rpm, and add the microcapsules D to the paint slurry, stir evenly, and obtain the main agent;
[0124] S400, under a stirring speed of 900 rpm, the phenolic amine resin is added to the xylene and butanol, and stirred evenly to obtain the hardener;
[0125] S500, the main agent and the hardener are mixed evenly to obtain the microcapsule anti-corrosion coating, wherein the mixing mass ratio of the main agent and the hardener is 10:1.
[0126] The microcapsule anticorrosive coatings prepared in Examples 5 to 8 were subjected to performance testing, and the test results are shown in Table 1 below.
[0127] Table 1. Performance test results of the microcapsule anticorrosive coatings prepared in Examples 5-8:
[0128]
[0129]
[0130] Comparative Example 1
[0131] The anti-corrosion coating provided in this comparative example differs from that in Example 5 only in that the microcapsule A is replaced with an equal amount of polyurethane microcapsules, while other components and preparation processes remain unchanged.
[0132] Comparative Example 2
[0133] The anti-corrosion coating provided in this comparative example differs from that in Example 5 in that microcapsule A is replaced with an anti-rust agent in equal amounts, while other components and preparation processes remain unchanged.
[0134] Comparative Example 3
[0135] The anti-corrosion coating provided in this comparative example differs from that in Example 5 only in that the microcapsule A is replaced with an equal amount of zinc powder, while other components and preparation processes remain unchanged.
[0136] The anti-corrosion coatings prepared in Comparative Examples 1 to 3 were tested for salt spray resistance and adhesion. The test results are shown in Table 2 below.
[0137] Table 2 shows the performance test results of the anti-corrosion coatings prepared in Comparative Examples 1-3:
[0138] Comparison / Project Salt spray resistance h Adhesion / MPa Comparative Example 1 600h 8.3 Comparative Example 2 480h 8.5 Comparative Example 3 552h 8.1
[0139] Through the above embodiments of the present invention and the test results of the microcapsule anticorrosive coating, it can be seen that the microcapsule anticorrosive coating prepared under the conditions of the embodiments of the present invention has excellent adhesion and a non-volatile matter content higher than the index requirements, meeting national environmental protection and VOC emission requirements. In the microcapsule anticorrosive coating of the present invention, the proportion of zinc-rich coating is greatly reduced, the coating coverage rate is increased, the amount of coating used is reduced, and the coating cost is effectively reduced. The microcapsules of the present invention crack due to the damage of the coating film during the salt spray test, thereby allowing the anticorrosive material to flow out and play a role in timely repairing the substrate. The microcapsules have outstanding performance in the microcapsule anticorrosive coating, and the self-healing of the substrate can greatly save existing coating and repair costs.
[0140] In the description of the above embodiments, specific features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments or examples.
[0141] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A microcapsule, characterized in that, The core of the microcapsule is a chlorinated rubber solution, and the capsule wall is a dimethyl diallyl ammonium chloride polymer with a thickness of 30-80 nm and a particle size of 1-2 μm; wherein, the concentration of the chlorinated rubber solution is 35-45 wt%; and the microcapsule loading rate is 80-90%.
2. A method for the preparation of microcapsules, applied to the microcapsules of claim 1, characterized by, include: Under stirring conditions, chlorinated rubber resin is added to the first solvent and mixed evenly to obtain a chlorinated rubber solution; The concentration of the chlorinated rubber solution is 35-45 wt%, and the first solvent includes xylene; Under stirring conditions, the chlorinated rubber solution and photoinitiator are added to the second solvent and mixed evenly to obtain an oil phase; the mass ratio of the chlorinated rubber solution, photoinitiator and second solvent added is 50:(1~2):(120~150), and the second solvent includes dichloromethane; Under stirring conditions, an aqueous solution of dimethyl diallyl ammonium chloride and the oil phase are added to a third solvent; wherein the mass ratio of the added third solvent, the aqueous solution of dimethyl diallyl ammonium chloride, and the oil phase is 1:(150~200):(35~40), the mixture is stirred until homogeneous, irradiated with ultraviolet light until the reaction is complete, stirring is stopped, and the mixture is filtered, impurities are removed, and dried to obtain microcapsules; wherein the third solvent comprises an aqueous solution of polyvinyl alcohol with a mass concentration of 0.5~2wt%, and the aqueous solution of dimethyl diallyl ammonium chloride has a concentration of 1~5wt%.
3. The method of claim 2, wherein the microcapsules are prepared by The filtration, impurity removal, and drying processes include: The product obtained after ultraviolet irradiation was filtered, washed with deionized water to remove impurities, and then dried at a temperature of 15~55℃ to obtain the microcapsules.
4. The method of claim 2, wherein the microcapsules are prepared by a method comprising: The photoinitiator includes (2,4,6-trimethylbenzoyl)-diphenylphosphine oxide.
5. A microcapsule corrosion protective coating characterized in that, The coating comprises a main agent and a hardener. The main agent includes 10-20 wt% epoxy resin, 65-70 wt% zinc powder, 5-10 wt% fourth solvent, 8-10 wt% microcapsules as described in claim 1, 1-2 wt% anti-settling agent, 0.5-2 wt% dispersant, and 0-0.5 wt% defoamer. In the microcapsule anticorrosive coating, the mass ratio of the main agent to the hardener is 10:(0.8-1). The fourth solvent includes xylene and butanol, and the anti-settling agent includes any one or two of bentonite and polyamide wax. The hardener comprises 30-40 wt% of a curing agent resin and 60-70 wt% of a fifth solvent, wherein the curing agent resin comprises one or two of phenolic amine resin and polyamide resin; the fifth solvent comprises xylene and butanol; and the viscosity of the anti-corrosion coating is 110-130 KU. The dispersant includes modified polyurethane and modified acrylate dispersant; The defoaming agents include polysiloxane defoamers and polyether defoamers.
6. A method for the preparation of a microcapsule anticorrosive coating characterized in that, The microcapsule anticorrosive coating applied to the microcapsule anticorrosive coating of claim 5 comprises: According to the content of each component in the main agent, the epoxy resin, fourth solvent, dust suppressant, dispersant and defoamer are mixed and stirred at a stirring speed of 800~1000 rpm until the mixture is uniform to obtain a mixture. The stirring speed of the mixture is controlled at 1200~1450 rpm, and the zinc powder is added to the mixture. Stirring is continued until the particle size in the mixture is ≤50μm to obtain the paint slurry. The stirring rate of the paint slurry is controlled at 800~1000 rpm, and the microcapsules are added to the paint slurry and stirred evenly to obtain the main agent; The curing agent resin was added to the fifth solvent at a stirring speed of 800-1000 rpm and stirred until homogeneous to obtain the hardener. The main agent and the hardener are mixed evenly to obtain the microcapsule anticorrosive coating, wherein the mass ratio of the main agent to the hardener is 10:(0.8~1).
Citation Information
Patent Citations
Electrostatic spraying type chlorinated rubber anticorrosive paint and preparation method thereof
CN102796425A
Chlorinated rubber anti-corrosive paint
CN109627982A