LED chip preparation method and LED chip
By immersing the transparent conductive layer of the LED chip in an acidic solution to increase the hole concentration, the problem of insufficient brightness in existing LED chips is solved, and a significant improvement in brightness is achieved.
Patent Information
- Application Number
- CN202311243183.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-09-25
AI Technical Summary
The brightness of existing LED chips is not high enough, which affects their competitiveness.
After growing a transparent conductive layer covering a P-type semiconductor layer and a current blocking layer on the epitaxial layer, an annealing process is performed, and the transparent conductive layer is immersed in an acidic solution to increase the hole concentration by combining hydrogen ions with oxygen, thereby improving conductivity.
It significantly improved the luminous brightness of LED chips, increasing it by 1.5% to 11%, without changing other manufacturing processes.
Smart Images

Figure CN117374173B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and in particular to a method for preparing an LED chip and an LED chip. Background Technology
[0002] LEDs (Light-Emitting Diodes) are solid-state active light sources with advantages such as energy saving and environmental protection, high efficiency, long lifespan, high brightness, high color purity, low energy consumption, and fast response time. They can typically achieve higher durability, more compact size, and greater design flexibility, and are widely used in lighting, display, backlighting, automotive, and other fields.
[0003] In recent years, with significant progress in p-type gallium nitride doping technology, gallium nitride-based LEDs, possessing excellent characteristics such as fast response, long lifespan, low power consumption, small size, and high brightness, have been widely used in backlights for LCD displays, full-color displays, and traffic displays. Since the brightness of LED chips is a crucial performance indicator for LED products, improving chip brightness on the existing basis has become an urgent problem to be solved in order to enhance the competitiveness of LED chips. Summary of the Invention
[0004] Therefore, the purpose of this invention is to provide an LED chip manufacturing method and an LED chip, thereby solving the problem of insufficient brightness in existing LED chips.
[0005] This invention provides a method for preparing an LED chip, the method comprising:
[0006] Provide a semi-finished LED chip with a pre-fabricated epitaxial layer;
[0007] Etching is performed on the epitaxial layer of the semi-finished LED chip to expose the N-type semiconductor layer of the epitaxial layer, and a current blocking layer is deposited on the corresponding area of the P-type semiconductor layer of the epitaxial layer where the electrode is to be fabricated.
[0008] A transparent conductive layer covering the P-type semiconductor layer and the current blocking layer is grown on the epitaxial layer, and the semi-finished LED chip with the transparent conductive layer deposited is annealed.
[0009] The annealed semi-finished LED chip is immersed in an acidic solution for a preset time.
[0010] After soaking, the semi-finished LED chip is cleaned, and then electrodes are grown on the surface of the semi-finished LED chip in the corresponding areas where electrodes are to be made.
[0011] The LED chip fabrication method of this invention adds a process of immersing in an acidic solution after the steps of growing a transparent conductive layer covering a P-type semiconductor layer and a current blocking layer on an epitaxial layer and annealing the semi-finished LED chip with the transparent conductive layer deposited, so that the hydrogen ions in the acidic solution combine with the oxygen in the transparent conductive layer, thereby increasing the hole concentration in the transparent conductive layer, thus increasing the conductivity of the transparent conductive layer, improving the current density, and consequently significantly increasing the luminous brightness of the LED chip.
[0012] Preferably, the transparent conductive layer is made of either indium tin oxide or indium zinc oxide.
[0013] Preferably, the acidic solution is either a BOE solution composed of HF and NH4F or an aqueous solution of a halogen hydride.
[0014] Preferably, the ratio of HF to NH4F in the BOE solution is 1:5-20.
[0015] Preferably, the preset time is 100S-500S.
[0016] Preferably, the step of cleaning the semi-finished LED chip after soaking and then growing electrodes on the surface of the semi-finished LED chip in the corresponding area where electrodes are to be formed includes:
[0017] Clean and dry the semi-finished LED chips;
[0018] Negative photoresist is applied to the surface of the semi-finished LED chip, and then exposed and developed using photomasks with N-type electrode patterns and P-type electrode patterns, respectively.
[0019] Based on the P-type electrode pattern, a portion of the transparent conductive layer and the current blocking layer on the P-type semiconductor layer are removed using etching technology.
[0020] Based on the N-type electrode pattern and the P-type electrode pattern, N-type electrodes and P-type electrodes are prepared at corresponding positions by electron beam evaporation.
[0021] Preferably, after the step of cleaning the semi-finished LED chip after soaking and then growing electrodes on the surface of the semi-finished LED chip in the corresponding area where electrodes are to be formed, the method further includes:
[0022] A passivation layer covering the epitaxial layer and the electrode is grown on the epitaxial layer;
[0023] The passivation layers on the N-electrode and P-electrode of the electrode are etched to expose at least partially the N-electrode and the P-electrode.
[0024] Preferably, the step of providing a semi-finished LED chip with a fabricated epitaxial layer includes:
[0025] Provide a substrate with a reflective layer at the bottom;
[0026] An N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer are epitaxially grown sequentially on the substrate. The N-type semiconductor layer is an n-GaN layer, the P-type semiconductor layer is a P-GaN layer, and the light-emitting layer is a multi-quantum-well active layer.
[0027] Preferably, the step of sequentially epitaxially growing an N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer on the substrate includes:
[0028] An N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer are sequentially grown on a substrate using high-purity hydrogen as the carrier gas, high-purity ammonia as the nitrogen source, trimethylgallium and triethylgallium as gallium sources, trimethylindium as an indium source, silane as an N-type dopant, trimethylaluminum as an aluminum source, and magnesia-dicenocene as a P-type dopant. The thickness of the N-GaN layer is 1 μm-3 μm, the thickness of the P-GaN layer is 200 nm-300 nm, and the molar proportion of In in the multi-quantum-well active layer is 10%-35%.
[0029] The present invention also provides an LED chip, which is prepared by any of the LED chip preparation methods described above. Attached Figure Description
[0030] Figure 1 This is a flowchart of an LED chip fabrication method according to an embodiment of the present invention;
[0031] Figure 2 This is a schematic diagram of an LED chip according to an embodiment of the present invention;
[0032] The following detailed description, in conjunction with the accompanying drawings, will further illustrate the present invention. Detailed Implementation
[0033] To facilitate understanding of the present invention, a more complete description will be given below with reference to the accompanying drawings. Several embodiments of the invention are illustrated in the drawings. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete.
[0034] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.
[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0036] like Figure 1 As shown, the present invention discloses a flowchart of an LED chip fabrication method, which includes steps S10-S14.
[0037] Step S10: Provide a semi-finished LED chip with a fabricated epitaxial layer.
[0038] Before passing the transparent conductive layer through the acidic solution, the transparent conductive layer needs to be grown on the chip first. Therefore, it is necessary to first obtain a semi-finished LED chip with the epitaxial layer fabricated. Specifically, in the embodiments of the present invention, the preparation of the semi-finished LED chip with the epitaxial layer fabricated can be carried out in the following manner:
[0039] Provide a substrate with a reflective layer at the bottom;
[0040] An N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer are epitaxially grown sequentially on a substrate. The N-type semiconductor layer is an n-GaN layer, the P-type semiconductor layer is a P-GaN layer, and the light-emitting layer is a multi-quantum-well active layer.
[0041] Specifically, the substrate can be selected from one of the following: sapphire substrate, SiO2-sapphire composite substrate, silicon substrate, silicon carbide substrate, gallium nitride substrate, and zinc oxide substrate. In this embodiment, a sapphire substrate is selected. Sapphire is currently the most commonly used GaN-based LED substrate material, and most GaN-based LEDs on the market use sapphire as the substrate material. The biggest advantages of sapphire substrates are mature technology, good stability, and low production cost. Furthermore, in this embodiment, when growing the epitaxial layer on the substrate using metal chemical vapor deposition, high-purity hydrogen is used as the carrier gas, high-purity ammonia as the nitrogen source, trimethylgallium and triethylgallium as gallium sources, trimethylindium as the indium source, silane as the N-type dopant, trimethylaluminum as the aluminum source, and magnesium pyrocene as the P-type dopant. The N-type semiconductor layer is an n-GaN layer, the P-type semiconductor layer is a P-GaN layer, and the light-emitting layer is a multi-quantum-well active layer. The thickness of the N-GaN layer is 1μm-3μm. For example, the thickness of the N-GaN layer is 1 μm, 1.5 μm, 2 μm or 3 μm, but not limited thereto; the thickness of the P-GaN layer is 200 nm-300 nm, for example, the thickness of the P-GaN layer is 200 nm, 230 nm, 280 nm or 300 nm, but not limited thereto; the molar proportion of In component in the multi-quantum-well active layer is 10%-35%, for example, the molar proportion of In component in the multi-quantum-well active layer is 10, 15, 25 or 35, but not limited thereto.
[0042] Step S11: Etch the epitaxial layer of the semi-finished LED chip to expose the N-type semiconductor layer of the epitaxial layer, and deposit a current blocking layer in the corresponding area of the electrode to be fabricated on the P-type semiconductor layer of the epitaxial layer.
[0043] Specifically, ICP (Inductively Coupled Plasma) etching is used to etch the epitaxial layer towards the substrate, removing part of the P-type semiconductor layer and the multi-quantum-well active layer, exposing part of the N-type semiconductor layer. Then, a current-blocking layer is fabricated on the P-type semiconductor layer to reduce the recombination of charge carriers directly below the metal electrodes, and to prevent the absorption and blocking of radiated photons by the metal. In this embodiment, the current-blocking layer is made of SiO2 material with a thickness of 200nm-400nm. Exemplary thicknesses include 200nm, 280nm, 360nm, or 400nm, but are not limited to these.
[0044] Step S12: A transparent conductive layer covering the P-type semiconductor layer and the current blocking layer is grown on the epitaxial layer, and the semi-finished LED chip with the transparent conductive layer deposited is annealed.
[0045] Specifically, a transparent conductive layer is fabricated on a P-type semiconductor using magnetron sputtering to increase the lateral current spread capability. The principle involves ionizing Ar gas and bombarding the target material, causing it to sputter onto the wafer surface and depositing the transparent conductive layer. The material for the transparent conductive layer is typically indium tin oxide (ITO) or indium zinc oxide (IZO). Because ITO or IZO deposits have poor density, an annealing process is usually performed to make the crystal arrangement more orderly, the film denser, and the conductivity more stable. The annealing process involves placing the semi-finished LED chip with the transparent conductive layer in a chamber at 300℃-600℃ for 12-18 minutes.
[0046] Step S13: Immerse the annealed semi-finished LED chip in an acidic solution for a preset time.
[0047] Specifically, the acidic solution can be any one of BOE solution or an aqueous solution of a halogen hydride. The halogen hydride can be HBr or HI. The BOE solution consists of HF and NH4F. The ratio of HF to NH4F in the BOE solution is 1:20; exemplary ratios include 1:5, 1:10, 1:15, or 1:20, but are not limited to these. Furthermore, the preset soaking time is 100-500 seconds; exemplary preset times include 100 seconds, 200 seconds, 300 seconds, or 500 seconds, but are not limited to these.
[0048] Step S14: After soaking, clean the semi-finished LED chip and then grow an electrode on the surface of the semi-finished LED chip in the corresponding area where the electrode is to be made.
[0049] Specifically, after cleaning and drying, negative photoresist is applied to the surface of the semi-finished LED chip. Then, photomasks with N-type and P-type electrode patterns are exposed and developed. Based on the P-type electrode pattern, a portion of the transparent conductive layer and the current blocking layer on the P-type semiconductor layer are removed by etching technology so that the subsequently prepared P electrode can contact the P-type semiconductor layer. Then, based on the N-type and P-type electrode patterns, N-type electrodes and P-type electrodes are prepared at corresponding positions by electron beam evaporation.
[0050] In addition, in some optional embodiments of the present invention, after cleaning the semi-finished LED chip after the soaking process, and then growing electrodes on the surface of the semi-finished LED chip in the corresponding area where electrodes are to be formed, the method further includes:
[0051] A passivation layer is grown on the epitaxial layer, covering both the epitaxial layer and the electrodes; and the passivation layer on the N-electrode and P-electrode is etched to expose at least partially the N-electrode and P-electrode for wire bonding, while the remaining portions of the electrodes are completely covered by the passivation layer to enhance the LED chip's resistance to metal migration. Figure 2 The diagram shows an LED chip prepared by this method.
[0052] On the other hand, the LED chip proposed in the embodiments of the present invention is prepared by any of the LED chip preparation methods described above.
[0053] In summary, the LED chip fabrication method and LED chip proposed in the above embodiments of the present invention, by adding a process of immersion in an acidic solution after growing a transparent conductive layer covering a P-type semiconductor layer and a current blocking layer on an epitaxial layer and annealing the semi-finished LED chip with the transparent conductive layer, allows hydrogen ions in the acidic solution to combine with oxygen in the transparent conductive layer, increasing the hole concentration in the transparent conductive layer, thereby improving the conductivity of the transparent conductive layer, increasing the current density, and thus significantly increasing the luminous brightness of the LED chip. Without changing other fabrication processes, the brightness of the LED chip is improved simply by adding an immersion process, solving the problem of insufficient brightness of LED chips in the prior art.
[0054] The present invention will be further illustrated below with specific embodiments:
[0055] Example 1
[0056] This embodiment provides an LED chip, which further includes a substrate with a reflective layer at the bottom, an N-type semiconductor, a multi-quantum-well active layer, a P-type semiconductor, a current-blocking layer, a transparent conductive layer, electrodes, and a passivation layer; the N-type semiconductor, quantum well layer, P-type semiconductor, transparent conductive layer, current-blocking layer, electrodes, and passivation layer are sequentially stacked on the substrate.
[0057] The substrate is a sapphire substrate. Specifically, the thickness of the N-type semiconductor is 2 μm; the molar ratio of In in the multi-quantum well active layer is 20%; the thickness of the P-type semiconductor is 250 nm; the transparent conductive layer is an ITO transparent conductive layer; both the P-type electrode and the N-type electrode are structures with multiple metal layers stacked on top of each other, wherein the metal layers can be one or more of Cr, Al, Ti, Ni, Pt, Au, and Cu.
[0058] The method for preparing the LED chip in this embodiment includes the following steps:
[0059] S20: Provides a sapphire substrate with a reflective layer at the bottom for growth, and sequentially epitaxially grows an N-type semiconductor, a multi-quantum-well active layer, and a P-type semiconductor on the substrate;
[0060] S21: On the P-type semiconductor, etching is performed towards the substrate to expose a portion of the N-type semiconductor; specifically, ICP technology is used to etch the epitaxial layer, wherein etching is performed from the P-type semiconductor towards the substrate to expose the P-type semiconductor;
[0061] S22: A current blocking layer is deposited on the corresponding region of the electrode to be fabricated on the P-type semiconductor layer of the epitaxial layer using a coating equipment. The material of the current blocking layer is SiO2, and the thickness is 300nm.
[0062] S23: Subsequently, an ITO transparent conductive layer was fabricated by magnetron sputtering and annealed at 550°C for 15 minutes.
[0063] S24: Wafers after immersion annealing in BOE solution for 100 seconds, with a BOE solution composition concentration ratio of HF:NH4F = 1:10;
[0064] S25: Then, using photolithography, part of the current blocking layer and transparent conductive layer on the N-type semiconductor are removed, and N-type electrodes and P-type electrodes are deposited at the corresponding positions using an electron beam evaporation machine.
[0065] Example 2
[0066] This embodiment also provides an LED chip preparation method and an LED chip, the difference from Embodiment 1 is that the soaking time is 200 seconds.
[0067] Example 3
[0068] This embodiment also provides an LED chip preparation method and an LED chip, the difference from Embodiment 1 is that the soaking time is 300 seconds.
[0069] Example 4
[0070] This embodiment also provides an LED chip preparation method and an LED chip, the difference from Embodiment 1 is that the soaking time is 500 seconds.
[0071] Example 5
[0072] This embodiment also provides an LED chip preparation method and an LED chip, the difference from Embodiment 1 is that HF:NH4F = 1:15.
[0073] Example 6
[0074] This embodiment also provides an LED chip preparation method and an LED chip, the difference from embodiment five is that the soaking time is 200 seconds.
[0075] Example 7
[0076] This embodiment also provides an LED chip preparation method and an LED chip, the difference from embodiment five is that the soaking time is 300 seconds.
[0077] Example 8
[0078] This embodiment also provides an LED chip preparation method and an LED chip, the difference from embodiment five is that the soaking time is 500 seconds.
[0079] Example 9
[0080] This embodiment also provides an LED chip preparation method and an LED chip, the difference from Embodiment 1 is that HF:NH4F = 1:20.
[0081] Example 10
[0082] This embodiment also provides an LED chip preparation method and an LED chip, the difference from embodiment five is that the soaking time is 200 seconds.
[0083] Example 11
[0084] This embodiment also provides an LED chip preparation method and an LED chip, the difference from embodiment five is that the soaking time is 300 seconds.
[0085] Example 12
[0086] This embodiment also provides an LED chip preparation method and an LED chip, the difference from embodiment five is that the soaking time is 500 seconds.
[0087] Example 13
[0088] This embodiment also provides an LED chip preparation method and an LED chip. The difference from Embodiment 1 is that the soaking solution used is an HI acidic solution with a pH value of 5, and the soaking time is 300 seconds.
[0089] Example 14
[0090] This embodiment also provides an LED chip preparation method and an LED chip. The difference from Embodiment 1 is that the soaking solution used is an HBr acidic solution with a pH of 5, and the soaking time is 300 seconds.
[0091] Experiments were conducted on the LED chips prepared in each embodiment and LED chips in the prior art. The brightness of the chips under the same voltage was statistically analyzed, and the test results are shown in the table below:
[0092]
[0093]
[0094] As can be seen from the table, the LED chip prepared by this invention, by adding an acidic solution immersion process, improves the brightness of LED chips by 1.5% to 11% compared to existing LED chips. Example 4 shows the highest brightness, with an 11% improvement compared to existing technologies. Furthermore, a comparison of Examples 1, 2, 3, and 4 shows that the longer the immersion time, the greater the brightness improvement of the LED chip. A comparison of Examples 1, 5, and 9 shows that a higher proportion of HF in the BOE solution leads to a greater brightness improvement in the LED chip. A comparison of Examples 3, 7, 11, 13, and 14 shows that the BOE solution has a better effect on improving the brightness of the LED chip compared to HI and HBr solutions.
[0095] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0096] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention. Therefore, the scope of protection of this patent should be determined by the appended claims.
Claims
1. A method for fabricating an LED chip, characterized in that, The method includes: Provide a semi-finished LED chip with a pre-fabricated epitaxial layer; Etching is performed on the epitaxial layer of the semi-finished LED chip to expose the N-type semiconductor layer of the epitaxial layer, and a current blocking layer is deposited on the corresponding area of the P-type semiconductor layer of the epitaxial layer where the electrode is to be fabricated. A transparent conductive layer covering the P-type semiconductor layer and the current blocking layer is grown on the epitaxial layer, and the semi-finished LED chip with the transparent conductive layer deposited is annealed. The annealed semi-finished LED chip is immersed in an acidic solution for a preset time. After soaking, the semi-finished LED chip is cleaned, and then electrodes are grown on the surface of the semi-finished LED chip in the corresponding area where the electrodes are to be made. The step of cleaning the semi-finished LED chip after soaking and then growing electrodes on the surface of the semi-finished LED chip in the corresponding area where electrodes are to be formed includes: Clean and dry the semi-finished LED chips; Negative photoresist is applied to the surface of the semi-finished LED chip, and then exposed and developed using photomasks with N-type electrode patterns and P-type electrode patterns, respectively. Based on the P-type electrode pattern, a portion of the transparent conductive layer and the current blocking layer on the P-type semiconductor layer are removed using etching technology. Based on the N-type electrode pattern and the P-type electrode pattern, N-type electrodes and P-type electrodes are prepared at corresponding positions by electron beam evaporation.
2. The method for preparing an LED chip according to claim 1, characterized in that, The transparent conductive layer is made of either indium tin oxide or indium zinc oxide.
3. The method for preparing an LED chip according to claim 1, characterized in that, The acidic solution is either a BOE solution composed of HF and NH4F or an aqueous solution of a hydride of a halide.
4. The method for preparing an LED chip according to claim 3, characterized in that, The ratio of HF to NH4F in the BOE solution is 1:5-20.
5. The method for preparing an LED chip according to claim 1, characterized in that, The preset time is 100S-500S.
6. The method for preparing an LED chip according to claim 1, characterized in that, After the step of cleaning the semi-finished LED chip after soaking and then growing electrodes on the surface of the semi-finished LED chip in the corresponding area where electrodes are to be formed, the method further includes: A passivation layer covering the epitaxial layer and the electrode is grown on the epitaxial layer; The passivation layers on the N-electrode and P-electrode of the electrode are etched to expose at least partially the N-electrode and the P-electrode.
7. The method for preparing an LED chip according to any one of claims 1-6, characterized in that, The step of providing a semi-finished LED chip with a fabricated epitaxial layer includes: Provide a substrate with a reflective layer at the bottom; An N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer are epitaxially grown sequentially on the substrate. The N-type semiconductor layer is an n-GaN layer, the P-type semiconductor layer is a P-GaN layer, and the light-emitting layer is a multi-quantum-well active layer.
8. The method for preparing an LED chip according to claim 7, characterized in that, The step of sequentially epitaxially growing an N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer on the substrate includes: An N-type semiconductor layer, a light-emitting layer, and a P-type semiconductor layer are sequentially grown on a substrate using high-purity hydrogen as the carrier gas, high-purity ammonia as the nitrogen source, trimethylgallium and triethylgallium as gallium sources, trimethylindium as an indium source, silane as an N-type dopant, trimethylaluminum as an aluminum source, and magnesia-dicenocene as a P-type dopant. The thickness of the n-GaN layer is 1 μm-3 μm, the thickness of the P-GaN layer is 200 nm-300 nm, and the molar proportion of In in the multi-quantum-well active layer is 10%-35%.
9. An LED chip, characterized in that, The LED chip is prepared by the method described in any one of claims 1 to 8.
Citation Information
Patent Citations
Manufacturing method of LED chip
CN108110107A
Supporting substrates for semiconductor light emitting device and high-performance vertical structured semiconductor light emitting devices using supporting substrates