Modified positive electrode material and preparation method and application thereof
By performing hydroxylation pretreatment and ALD coating on high-nickel cathode materials, a continuous and uniform LiZr₂(PO₄)₃ coating layer is formed, which solves the structural failure and humidity sensitivity problems of high-nickel cathode materials during cycling, and significantly improves the cycling stability and rate performance of the materials.
Patent Information
- Application Number
- CN202311355034.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-19
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-10-19
AI Technical Summary
Existing high-nickel cathode materials suffer from structural failure during charge-discharge cycles, are sensitive to environmental humidity, and are prone to moisture absorption, leading to cation mixing and increased residual alkali. Furthermore, the existing coating layer has inconsistent uniformity, affecting material performance.
By performing hydroxylation pretreatment on high-nickel cathode materials and combining it with atomic layer deposition (ALD) technology, a continuous and uniform LiZr₂(PO₄)₃ coating layer is formed, enhancing the protective effect.
It improves the cycle stability and rate performance of high-nickel cathode materials, with a specific capacity of over 168.3 mAh/g after 100 cycles at 1C, a capacity retention rate of over 89.05% after 100 cycles at 1C, an initial specific capacity of over 185.2 mAh/g at 2C, and an initial specific capacity of over 177.5 mAh/g at 5C.
Smart Images

Figure BDA0004501436980000081 
Figure BDA0004501436980000091
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery materials, and relates to a modified cathode material, its preparation method, and its application. Background Technology
[0002] Lithium-ion batteries boast high energy density, long cycle life, and excellent rate performance, making them ideal for widespread applications in 3C electronics, new energy, and large-scale energy storage. As a key material in lithium-ion batteries, the fundamental characteristics of the cathode material directly determine the final capacity and energy density of the battery. Currently commercially available lithium-ion battery cathode materials include LiMn2O4, LiCoO3, LiFePO4, and LiNi. x Co y Mn 1-x-y O2, LiNi x Co y Al 1-x-y O2. With the increasing demands for battery life in the end-user market, cathode materials need to possess higher capacity and voltage characteristics.
[0003] Among the cathode material systems currently available for large-scale application, high-nickel ternary cathode materials can meet the high-capacity requirements, with a discharge specific capacity reaching 200 mAh / g and a corresponding energy density of approximately 800 Wh / kg. However, the application of high-nickel cathode materials also faces some challenges. With increasing nickel content, the Ni content in high-nickel cathode materials decreases during charge-discharge cycles. 4+ Reacting with the electrolyte leads to the gradual failure of the material's surface structure, resulting in internal microcracks. Furthermore, high-nickel cathode materials are sensitive to environmental humidity, readily absorbing moisture, causing cation mixing and increased residual alkali. Reduced cobalt content leads to a decrease in the rate performance of high-nickel cathode materials. These fundamental issues pose challenges to the long-term use of the final battery product.
[0004] CN114229917A discloses a surface modification method for high-nickel cathode materials and the modified high-nickel cathode materials, including: acid washing of high-nickel cathode materials, followed by mixing and sintering with a coating agent; wherein the coating agent contains elements W, Al and B.
[0005] CN105406040A discloses a coated modified high-nickel ternary cathode material and its preparation method. The preparation method includes: first dissolving a soluble aluminum salt in deionized water to obtain an aluminum salt solution; then adding LiNi... x Co (1-x) / 2 Mn (1-x) / 2 O2 material is added to aluminum salt solution and mixed to obtain slurry; then an alkaline solution prepared with alkaline metal compound is added to slurry to make pH value ≥ 7.0; after drying, sintering, natural cooling, crushing and sieving, coated modified high nickel ternary cathode material is obtained.
[0006] The aforementioned methods modify the surface of high-nickel cathode materials through coating, using the coating layer to isolate the bulk material from the electrolyte or air as much as possible, protecting the material from corrosion. However, these methods suffer from inconsistent coating uniformity. Furthermore, the oxides used for coating are typically electrochemically inert, which is detrimental to Li... + Migration can cause a decrease in the specific capacity of materials in the early stages, and it is also difficult to effectively improve rate performance. Summary of the Invention
[0007] The purpose of this invention is to provide a modified cathode material, its preparation method, and its application. This invention enhances the layer-by-layer growth capability of the ALD coating layer through hydroxylation, enabling the LiZr2(PO4)3 coating layer to continuously and uniformly coat the cathode particles, effectively alleviating the problem of insufficient performance improvement caused by island-like or random growth.
[0008] To achieve this objective, the present invention adopts the following technical solution:
[0009] In a first aspect, the present invention provides a method for preparing a modified cathode material, the method comprising the following steps:
[0010] (1) Mix the positive electrode material and the hydroxylation solution, heat and stir, and then dry to obtain a positive electrode material with surface hydroxylation;
[0011] (2) The surface-hydroxylated cathode material is subjected to atomic layer deposition to obtain the modified cathode material.
[0012] This invention pretreats the cathode material with a hydroxylation solution, which increases the number of hydroxyl reaction sites on its surface. This is beneficial for forming a continuous and uniform coating layer during atomic layer deposition (ALD), reducing the island-like or random growth of the coating layer when ALD coats the powder material, and maximizing the protection of the high-nickel cathode material.
[0013] Preferably, the chemical formula of the cathode material in step (1) is LiNi. a Co b A 1-a-b O2, A is any one or at least two of Mn, Mg, Al, Zr, Ti, Ta, Nb or Mo, 0.8≤a<1, 0.03≤b≤0.2.
[0014] Preferably, the solute in the hydroxylation solution in step (1) includes any one or a combination of at least two of sodium hydroxide, lithium hydroxide, potassium hydroxide, or hydrogen peroxide.
[0015] Preferably, the solvent of the hydroxylation solution includes any one or a combination of at least two of anhydrous ethanol, methanol, isopropanol or n-butanol.
[0016] Preferably, the concentration of the hydroxylation solution is 0.1% to 2%.
[0017] Preferably, the mass ratio of the positive electrode material to the hydroxylation solution is 1:(5-10), for example: 1:5, 1:6, 1:7, 1:8 or 1:10, etc.
[0018] Preferably, the heating and stirring temperature is 40-60°C, for example: 40°C, 45°C, 50°C, 55°C or 60°C.
[0019] Preferably, the heating and stirring time is 0.5 to 5 hours, for example: 0.5 hours, 1 hour, 2 hours, 3 hours or 5 hours.
[0020] Preferably, the product is dried after heating and stirring.
[0021] Preferably, the drying includes low-temperature drying or freeze-drying.
[0022] Preferably, the atomic layer deposition process in step (2) includes:
[0023] The surface-hydroxylated cathode material is placed in the reaction chamber of an atomic layer deposition apparatus. After evacuation, a zirconium source is introduced for a first purging, followed by an oxygen source for a second purging, a phosphorus source for a third purging, an oxygen source for a fourth purging, a lithium source for a fifth purging, and an oxygen source for a sixth purging. The above steps are repeated to obtain the modified cathode material.
[0024] The atomic layer deposition method described in this invention can obtain LiZr2(PO4)3 coatings of different thicknesses by adjusting process parameters and the number of repetitions.
[0025] Preferably, the temperature of the atomic layer deposition process is 150 to 400°C, for example: 150°C, 180°C, 200°C, 300°C or 400°C.
[0026] Preferably, the zirconium source includes any one or a combination of at least two of tetra(dimethylamino)zirconium, tert-butoxide zirconium, tetra(ethylmethylamino)zirconium, tetra(ethylamino)zirconium, or tetraethoxyzirconium.
[0027] Preferably, the time for introducing the zirconium source is 0.05 to 0.5 s, for example: 0.05 s, 0.1 s, 0.2 s, 0.3 s or 0.5 s.
[0028] Preferably, the oxygen source includes any one or a combination of at least two of water, ozone, or hydrogen peroxide.
[0029] Preferably, the oxygen source is introduced for 0.05 to 0.5 seconds, for example, 0.05 seconds, 0.1 seconds, 0.2 seconds, 0.3 seconds, or 0.5 seconds.
[0030] Preferably, the phosphorus source includes any one or a combination of at least two of tetramethylmethylene diphosphate, trimethyl phosphate, tri(dimethylamine)phosphine, or trialkylphosphine oxide.
[0031] Preferably, the phosphorus source is introduced for 0.05 to 0.5 seconds, for example, 0.05 seconds, 0.1 seconds, 0.2 seconds, 0.3 seconds, or 0.5 seconds.
[0032] Preferably, the lithium source includes any one or a combination of at least two of lithium tert-butoxide, lithium acetoacetate, lithium tert-butyl, or lithium di(trimethylsilyl)amino.
[0033] Preferably, the lithium source is introduced for 0.05 to 0.5 seconds, for example, 0.05 seconds, 0.1 seconds, 0.2 seconds, 0.3 seconds, or 0.5 seconds.
[0034] Preferably, the gases used in the first, second, third, fourth, fifth, and sixth purging processes include inert gases.
[0035] Preferably, the gas flow rates of the first, second, third, fourth, fifth, and sixth purging processes are 1 to 100 sccm, for example: 1 sccm, 5 sccm, 10 sccm, 50 sccm, or 100 sccm.
[0036] Preferably, the purging time for the first, second, third, fourth, fifth, and sixth purging is 10 to 60 seconds, for example: 10 seconds, 20 seconds, 30 seconds, 50 seconds, or 60 seconds.
[0037] In a second aspect, the present invention provides a modified cathode material, characterized in that the modified cathode material is prepared by the method described in the first aspect, and a LiZr2(PO4)3 coating layer is provided on the surface of the modified cathode material.
[0038] The modified cathode material coated with LiZr2(PO4)3 described in this invention can act as a physical barrier, preventing corrosion and damage to the bulk cathode material from air moisture, electrolyte, and HF, and can also serve as a Li... + Conductor. LiZr2(PO4)3, as a fast ion conductor, improves the cycle stability and rate performance of cathode materials.
[0039] Thirdly, the present invention provides a positive electrode sheet, characterized in that the positive electrode sheet comprises the modified positive electrode material as described in the second aspect.
[0040] Fourthly, the present invention provides a lithium-ion battery, characterized in that the lithium-ion battery comprises a positive electrode as described in the third aspect.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] (1) This invention utilizes a wet chemical method to pretreat high-nickel cathode materials, thereby hydroxylating the material surface and enhancing the layer-by-layer growth capability of the ALD coating layer. This allows the LiZr2(PO4)3 coating layer to continuously and uniformly coat the cathode particles, effectively alleviating the problem of insufficient performance improvement caused by island-like or random growth. The LiZr2(PO4)3 grown by ALD deposition using the method described in this invention can effectively improve the cycle performance and rate performance of high-nickel cathode materials.
[0043] (2) The battery made of the modified cathode material described in this invention can achieve a 1C 100-cycle specific capacity of more than 168.3 mAh / g, a 1C 100-cycle capacity retention rate of more than 89.05%, a 2C initial specific capacity of more than 185.2 mAh / g, and a 5C initial specific capacity of more than 177.5 mAh / g. Detailed Implementation
[0044] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0045] Example 1
[0046] This embodiment provides a modified cathode material, and the preparation method of the modified cathode material is as follows:
[0047] (1) High-nickel cathode material (LiNi) 0.9 Co 0.05 Mn 0.05 O2) was dispersed in an ethanol solution with a concentration of 1% NaOH, the material / solution ratio was 1:8, heated and stirred at 45℃ for 2h, filtered and washed, and freeze-dried to obtain a positive electrode material with surface hydroxylation.
[0048] (2) The surface-hydroxylated cathode material is placed in the reaction chamber of an atomic layer deposition apparatus. The reaction temperature is set to 250°C. The chamber is evacuated to achieve the required reaction vacuum. Zirconium tert-butoxide is introduced into the chamber for 0.2 s, followed by argon purging for 30 s at a flow rate of 20 sccm. Ozone is introduced into the chamber for 0.2 s, followed by argon purging for 30 s at a flow rate of 20 sccm. Trimethyl phosphate is introduced into the chamber for 0.2 s, followed by argon purging for 30 s at a flow rate of 20 sccm. Ozone is introduced into the chamber for 0.2 s, followed by argon purging for 30 s at a flow rate of 20 sccm. Lithium tert-butoxide is introduced into the chamber for 0.2 s, followed by argon purging for 30 s at a flow rate of 20 sccm. Ozone is introduced into the chamber for 0.2 s, followed by argon purging for 30 s at a flow rate of 20 sccm. This process is repeated 8 times to obtain the modified cathode material.
[0049] Example 2
[0050] This embodiment provides a modified cathode material, and the preparation method of the modified cathode material is as follows:
[0051] (1) High-nickel cathode material (LiNi) 0.9 Co 0.05 Mn 0.05 O2) was dispersed in an ethanol solution with a concentration of 0.1% hydrogen peroxide, with a material / solution ratio of 1:10. The mixture was heated and stirred at 40°C for 5 hours, filtered, washed, and freeze-dried to obtain a surface-hydroxylated cathode material.
[0052] (2) The surface-hydroxylated cathode material is placed in the reaction chamber of an atomic layer deposition apparatus. The reaction temperature is set to 150°C. The chamber is evacuated to achieve the required reaction vacuum. Zirconium tert-butoxide is introduced into the chamber for 0.05 s, followed by argon purging for 10 s at a flow rate of 50 sccm. Ozone is introduced into the chamber for 0.05 s, followed by argon purging for 10 s at a flow rate of 50 sccm. Trialkyl phosphorus oxide is introduced into the chamber for 0.05 s, followed by argon purging for 10 s at a flow rate of 50 sccm. Ozone is introduced into the chamber for 0.05 s, followed by argon purging for 10 s at a flow rate of 50 sccm. Lithium acetoacetate is introduced into the chamber for 0.05 s, followed by argon purging for 10 s at a flow rate of 50 sccm. Ozone is introduced into the chamber for 0.05 s, followed by argon purging for 10 s at a flow rate of 50 sccm. This process is repeated 10 times to obtain the modified cathode material.
[0053] Example 3
[0054] This embodiment provides a modified cathode material, and the preparation method of the modified cathode material is as follows:
[0055] (1) High-nickel cathode material (LiNi) 0.9 Co 0.05 Mn 0.05O2) was dispersed in an ethanol solution with a concentration of 2% NaOH, the material / solution ratio was 1:5, the mixture was heated and stirred at 50℃ for 0.5h, filtered and washed, and freeze-dried to obtain a positive electrode material with surface hydroxylation.
[0056] (2) The surface-hydroxylated cathode material is placed in the reaction chamber of an atomic layer deposition apparatus. The reaction temperature is set to 300°C. The chamber is evacuated to achieve the required reaction vacuum. Zirconium tert-butoxide is introduced into the chamber for 0.5 s, followed by argon purging for 60 s at a flow rate of 100 sccm. Hydrogen peroxide is introduced into the chamber for 0.5 s, followed by argon purging for 60 s at a flow rate of 100 sccm. Tetramethylmethylene diphosphate is introduced into the chamber for 0.5 s, followed by argon purging for 60 s at a flow rate of 100 sccm. Hydrogen peroxide is introduced into the chamber for 0.5 s, followed by argon purging for 60 s at a flow rate of 100 sccm. Tert-butyllithium is introduced into the chamber for 0.5 s, followed by argon purging for 60 s at a flow rate of 100 sccm. Hydrogen peroxide is introduced into the chamber for 0.5 s, followed by argon purging for 60 s at a flow rate of 100 sccm. This process is repeated 13 times to obtain the modified cathode material.
[0057] Example 4
[0058] The only difference between this embodiment and Example 1 is that the concentration of the hydroxylation solution is 0.05%, while the other conditions and parameters are exactly the same as in Example 1.
[0059] Example 5
[0060] The only difference between this embodiment and Example 1 is that the concentration of the hydroxylation solution is 5%, while the other conditions and parameters are exactly the same as in Example 1.
[0061] Example 6
[0062] The only difference between this embodiment and embodiment 1 is that the stirring temperature in step (1) is 30°C, while the other conditions and parameters are exactly the same as in embodiment 1.
[0063] Example 7
[0064] The only difference between this embodiment and embodiment 1 is that the stirring temperature in step (1) is 60°C, while the other conditions and parameters are exactly the same as in embodiment 1.
[0065] Comparative Example 1
[0066] The only difference between this comparative example and Example 1 is that step (1) hydroxylation is not performed; all other conditions and parameters are exactly the same as in Example 1.
[0067] Performance testing:
[0068] The positive electrode material, conductive carbon, and PVDF / NMP prepared according to a certain mass ratio in the examples and comparative examples were weighed and placed in a homogenizing tank, with a certain amount of NMP added as a solvent. Vacuum degassing and homogenization were performed using a homogenizer to obtain a mixed slurry. The slurry was then uniformly coated onto aluminum foil, and after drying the solvent and moisture in an oven, it was stamped to obtain the positive electrode sheet. Electrodes with good consistency were selected to assemble coin cells. Using lithium metal sheets as the negative electrode, Celgard 2500 as the separator, and 1M LiPF6 (EC:DMC:EMC=1:1:1Vol%) as the electrolyte, coin cells were assembled in a glove box. The charge-discharge test voltage range was 2.5-4.25V. Activation was performed for 2 cycles at 0.1C, followed by cycle testing and rate testing. The cycle test consisted of 100 cycles at 1C, and the rate test consisted of 5 cycles each at 0.2C, 0.5C, 1C, 2C, and 5C. The test results are shown in Table 1.
[0069] Table 1
[0070]
[0071]
[0072] As can be seen from Table 1, and from Examples 1-3, the battery made of the modified cathode material of the present invention can achieve a 1C 100-cycle specific capacity of over 168.3 mAh / g, a 1C 100-cycle capacity retention rate of over 89.05%, a 2C initial specific capacity of over 185.2 mAh / g, and a 5C initial specific capacity of over 177.5 mAh / g.
[0073] A comparison of Examples 1 and 4-5 shows that the concentration of the hydroxylation solution affects the performance of the modified cathode material described in this invention. Controlling the concentration of the hydroxylation solution between 0.1% and 2% yields a cathode material with better performance. If the concentration is too high, alkaline impurities may remain on the surface of the cathode material, causing an increase in pH and affecting its performance. If the concentration is too low, the hydroxylation time becomes longer and the number of hydroxylation sites decreases, resulting in poor subsequent atomic layer deposition.
[0074] A comparison of Examples 1 and 6-7 shows that the temperature of the hydroxylation reaction affects the performance of the modified cathode material of the present invention during preparation. Controlling the temperature of the hydroxylation reaction at 40-60°C results in a cathode material with better performance. If the temperature is too high, the solvent reacts with the material surface, changing the surface structure of the material. If the temperature is too low, the hydroxylation rate on the material surface is slow, and there are fewer hydroxylation sites.
[0075] As can be seen from the comparison between Example 1 and Comparative Example 1, the present invention pre-treats the cathode material with a hydroxylation solution, which increases the number of hydroxyl reaction sites on its surface. This is beneficial for the formation of a continuous and uniform coating layer during ALD deposition, reduces the island-like or random growth of the coating layer when ALD coats the powder material, and maximizes the protection of the high-nickel cathode material.
[0076] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A method for preparing a modified cathode material, characterized in that, The preparation method includes the following steps: (1) Mix the positive electrode material and the hydroxylation solution, heat and stir, and then dry to obtain a positive electrode material with surface hydroxylation; (2) Perform atomic layer deposition on the surface-hydroxylated cathode material to obtain the modified cathode material; In step (1), the solute of the hydroxylation solution includes any one or a combination of at least two of sodium hydroxide, lithium hydroxide, potassium hydroxide, or hydrogen peroxide; the solvent of the hydroxylation solution includes any one or a combination of at least two of anhydrous ethanol, methanol, isopropanol, or n-butanol; the concentration of the hydroxylation solution is 0.1-2%; the mass ratio of the positive electrode material to the hydroxylation solution is 1:(5-10); the heating and stirring temperature is 40-60°C; and the heating and stirring time is 0.5-5 hours.
2. The preparation method according to claim 1, characterized in that, The chemical formula of the cathode material mentioned in step (1) is LiNi. a Co b A 1-a-b O2, A is any one or at least two of Mn, Mg, Al, Zr, Ti, Ta, Nb or Mo, 0.8≤a<1, 0.03≤b≤0.
2.
3. The preparation method according to claim 1, characterized in that, The mixture is heated and stirred before being dried.
4. The preparation method according to claim 3, characterized in that, The drying process includes low-temperature drying or freeze-drying.
5. The preparation method according to claim 1, characterized in that, Step (2) of the atomic layer deposition process includes: The surface-hydroxylated cathode material is placed in the reaction chamber of an atomic layer deposition apparatus. After evacuation, a zirconium source is introduced for a first purging, followed by an oxygen source for a second purging, a phosphorus source for a third purging, an oxygen source for a fourth purging, a lithium source for a fifth purging, and an oxygen source for a sixth purging. The above steps are repeated to obtain the modified cathode material.
6. The preparation method according to claim 5, characterized in that, The temperature for the atomic layer deposition process is 150~400℃.
7. The preparation method according to claim 5, characterized in that, The zirconium source includes any one or a combination of at least two of tetra(dimethylamino)zirconium, tert-butoxide zirconium, tetra(ethylmethylamino)zirconium, tetra(ethylamino)zirconium, or tetraethoxyzirconium.
8. The preparation method according to claim 5, characterized in that, The time for introducing the zirconium source is 0.05~0.5s.
9. The preparation method according to claim 5, characterized in that, The oxygen source includes any one or a combination of at least two of water, ozone, or hydrogen peroxide.
10. The preparation method according to claim 5, characterized in that, The oxygen source is introduced in 0.05 to 0.5 seconds.
11. The preparation method according to claim 5, characterized in that, The phosphorus source includes any one or a combination of at least two of tetramethylmethylene diphosphate, trimethyl phosphate, tri(dimethylamine)phosphine, or trialkylphosphine oxide.
12. The preparation method according to claim 5, characterized in that, The phosphorus source is introduced for 0.05 to 0.5 seconds.
13. The preparation method according to claim 5, characterized in that, The lithium source includes any one or a combination of at least two of lithium tert-butoxide, lithium acetoacetate, lithium tert-butyl, or lithium di(trimethylsilyl)amino.
14. The preparation method according to claim 5, characterized in that, The lithium source is introduced for 0.05 to 0.5 seconds.
15. The preparation method according to claim 5, characterized in that, The gases used in the first, second, third, fourth, fifth, and sixth purging processes include inert gases.
16. The preparation method according to claim 5, characterized in that, The gas flow rates for the first, second, third, fourth, fifth, and sixth purging processes are 1 to 100 sccm.
17. The preparation method according to claim 5, characterized in that, The purging times for the first, second, third, fourth, fifth, and sixth purging processes are 10 to 60 seconds.
18. A modified cathode material, characterized in that, The modified cathode material is prepared by the method described in any one of claims 1-17, wherein a LiZr2(PO4)3 coating layer is provided on the surface of the modified cathode material.
19. A positive electrode plate, characterized in that, The positive electrode sheet comprises the modified positive electrode material as described in claim 18.
20. A lithium-ion battery, characterized in that, The lithium-ion battery includes the positive electrode as described in claim 19.
Citation Information
Patent Citations
Coated and modified high-nickel ternary cathode material and preparation method thereof
CN105406040A
Phosphorus-doped zinc oxide film preparation method
CN103866264A
Anti-reflection super-hydrophobic film as well as preparation method and application thereof
CN115583804A