Coal-based graphite negative electrode material, preparation method, use and lithium ion battery

By developing a method for preparing coal-based graphite anode materials, the problems of poor rate performance and high raw material cost of graphite anode materials have been solved, achieving high rate performance and low cost graphite materials suitable for lithium-ion batteries.

CN117374278BActive Publication Date: 2026-11-20CHINA ENERGY INVESTMENT CORP LTD +3
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210766444.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-01
Publication Date
2026-11-20
Estimated Expiration
2042-07-01

AI Technical Summary

Technical Problem

Existing graphite anode materials have poor rate performance and complex preparation processes with high raw material costs.

Method used

A graphite anode material with excellent rate performance was prepared by using coal-based graphite anode material, which was coked and graphitized by mixing coking coal, coking coal, 1/3 coking coal and lean coal in a specific ratio, controlling the peak intensity ratio between (110) crystal plane and (004) crystal plane and between (110) crystal plane and (101) crystal plane, as well as the interlayer spacing and graphitization degree.

Benefits of technology

The graphite material achieves high rate performance with low raw material cost, multiple lithium-ion insertion and extraction channels, fast diffusion rate, high coulombic efficiency and capacity, and a capacity retention rate of over 60% at 2C/0.1C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The application discloses a coal-based graphite negative electrode material, a preparation method, application and a lithium ion battery. The peak intensity I110 of a (110) crystal face of the coal-based graphite negative electrode material and the peak intensity I004 of a (004) crystal face satisfy the following condition: I110 / I004 >= 1.0. The peak intensity I110 of the (110) crystal face of the graphite negative electrode material and the peak intensity I101 of a (101) crystal face satisfy the following condition: I110 / I101 >= 1.5. The graphite negative electrode material has good rate capability and low raw material cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of carbon materials, specifically to a coal-based graphite anode material, its preparation method and uses, and lithium-ion batteries. Background Technology

[0002] Lithium-ion battery anodes are broadly classified into carbon materials and non-carbon materials. Carbon materials mainly include amorphous carbon, natural graphite, and artificial graphite. Graphite has a regular layered structure, a theoretical specific capacity of 372 mA·h / g, and high efficiency, making it the mainstream anode material. However, graphite has poor rate performance. Therefore, developing graphite with excellent rate performance is essential to improve material performance. Currently, the industry mostly uses a secondary granulation process to improve the rate performance of graphite, but this process is costly.

[0003] In addition, CN109768217A discloses a method for preparing graphite materials, which includes mixing needle coke raw materials with aromatic heterocyclic compounds to form coke, and then preparing graphite materials through graphitization and other treatments. Due to the removal of S / N from the heterocyclic compounds in the subsequent treatment, leaving channels, and the subsequent coating treatment with modifiers, it is convenient for subsequent lithium-ion diffusion and improves the rate performance of graphite materials. However, its process is relatively complex and the raw material cost is high. Summary of the Invention

[0004] The purpose of this invention is to provide a coal-based graphite anode material, its preparation method, its uses, and a lithium-ion battery, wherein the graphite anode material has good rate performance and low raw material cost.

[0005] To achieve the first aspect of the aforementioned objective, the coal-based graphite anode material provided by this invention adopts the following technical solution:

[0006] A coal-based graphite anode material, wherein the peak intensity I110 of the (110) crystal plane and the peak intensity I004 of the (004) crystal plane of the graphite anode material satisfy the following condition: I110 / I004≥1.0; the peak intensity I110 of the (110) crystal plane and the peak intensity I101 of the (101) crystal plane of the graphite anode material satisfy the following condition: I110 / I101≥1.5.

[0007] In a preferred embodiment of the coal-based graphite anode material according to the present invention, 1.0≤I110 / I004≤2.0, such as 1.2, 1.5, 1.6, 1.7 or 1.9, preferably 1.4≤I110 / I004≤1.8; 1.5≤I110 / I101≤3.0, such as 1.6, 1.8, 2.0, 2.3 or 2.8, preferably 1.7≤I110 / I101≤2.5.

[0008] In a preferred embodiment of the coal-based graphite anode material according to the present invention, the interlayer spacing d of the graphite anode material is ≤0.34nm, preferably 0.336nm≤d≤0.337nm, and more preferably 0.3364nm≤d≤0.3369nm.

[0009] In a preferred embodiment of the coal-based graphite anode material according to the present invention, the degree of graphitization G of the graphite anode material satisfies 80% ≤ G ≤ 90%, such as 82%, 84%, 86% or 87%; preferably, 81% ≤ G ≤ 89%; more preferably, 85% ≤ G ≤ 88%.

[0010] To achieve the second aspect of the aforementioned objective, the present invention also provides a method for preparing the aforementioned coal-based graphite anode material, employing the following technical solution: A method for preparing a coal-based graphite anode material, comprising the following steps:

[0011] 1) Based on the total dry ash-free weight of raw coal, blend 18-25% fat coal, 49-55% coking coal, 14-21% 1 / 3 coking coal and 7-15% lean coal.

[0012] 2) The obtained mixed coal is added to a coking oven for coking treatment to obtain coke;

[0013] 3) The obtained coke is crushed and shaped.

[0014] 4) The coke particles crushed in step 3) are graphitized to obtain graphitized material;

[0015] 5) The obtained graphitized material is sieved and demagnetized to obtain the coal-based graphite anode material.

[0016] In step 1) of this invention, coking coal, 1 / 3 coking coal, and lean coal, used as raw coal, are blended and mixed, wherein the proportion of each coal type is based on dry weight. In a preferred embodiment, the raw coal comprises 20-23% coking coal (e.g., 22%), 50-55% coking coal (e.g., 52% or 53%), 15-20% 1 / 3 coking coal (e.g., 16% or 18%), and 8-12% lean coal (e.g., 9% or 10%) to achieve better results. Studies have found that the above-mentioned coal blending is beneficial to improving the subsequent graphite ratio.

[0017] In step 2) of the present invention, the obtained coal is subjected to coking treatment to obtain coke; the coal coking process is well known in the art. For example, in the present invention, the coking conditions can be: coking temperature 1000-1200℃, coking time 8-20 hours, such as 10 or 16 hours.

[0018] In step 3) of this invention, the coke is pulverized and shaped to obtain coke particles. The pulverization can be performed using mechanical pulverization, air jet milling, or grinding, without particular limitation. For example, a high-speed mechanical impact mill, hammer mill, toothed mill, milling mill, air jet mill, ball mill, Raymond mill, etc., can be used. The equipment used for shaping is not particularly limited; equipment known in the art can be selected, such as a mechanical shaping machine or an air jet shaping machine. Preferably, the average particle size D50 of the obtained coke particles is 5-20 micrometers, for example, 10 micrometers, 12 micrometers, or 15 micrometers.

[0019] In step 4) of the present invention, preferably, the graphitization temperature is 2800-3400℃, such as 2900℃, 3000℃, or 3200℃; further, the graphitization time can be 4-12 hours, such as 5-10 hours, or for example, 6 hours or 8 hours. The graphitization can be performed using methods known in the art, such as an internal series graphitization furnace, an Atchison graphitization furnace, or a box-type graphitization furnace.

[0020] In step 5) of the present invention, the obtained graphitized material is sieved and demagnetized. This process is a common process in the field of graphite preparation and is well known in the art, so it will not be described in detail here.

[0021] To achieve the third aspect of the above-mentioned objective, the present invention also provides the application of the above-mentioned coal-based graphite anode material or the coal-based graphite anode material prepared according to the above-mentioned method in lithium-ion batteries.

[0022] To achieve the third aspect of the above-mentioned objective, the present invention also provides a lithium-ion battery, wherein the negative electrode of the lithium-ion battery contains the above-mentioned coal-based graphite negative electrode material or the coal-based graphite negative electrode material prepared according to the above-mentioned method.

[0023] In this invention, unless otherwise specified, all percentages appearing in the text are mass percentages.

[0024] Those skilled in the art will understand that the ash content of the coal-based graphite anode material should not be high, for example, not exceeding 10%, such as 3%, 5%, or 7%. This requirement can be met by washing and deashing the raw coal, which is well known in the art and will not be elaborated here.

[0025] In this invention, unless otherwise specified, all percentage contents refer to mass percentage contents.

[0026] Compared with the prior art, the present invention has the following advantages

[0027] This invention uses coal as raw material, blends various types of coal, then cokes and graphitizes it. This process facilitates the preferential orientation growth of graphite along the 110 facets during graphitization, resulting in more 110 facets, good rate performance, and low raw material cost. The graphite material of this invention has multiple lithium-ion insertion and extraction channels and a fast diffusion rate, achieving high power output while maintaining high coulombic efficiency and high capacity. Furthermore, it exhibits excellent rate performance with a 2C / 0.1C capacity retention rate of ≥60%. Detailed Implementation

[0028] The present invention will be further described below with reference to the embodiments, but the present invention is not limited to the listed embodiments.

[0029] In the following examples / comparative examples, the coking coal came from Zhenchengdi Mine; the coking coal came from Kailuan Coal Mine; 1 / 3 of the coking coal came from Xiaoquan Mine; and the lean coal came from Shigejie Mine.

[0030] XRD test conditions:

[0031] Interlayer spacing d, graphitization degree G, and I110 / I004 and I110 / I101 were all obtained by testing and analysis using a D8 Advance X-ray diffractometer from Bruker AXS GmbH, Germany. XRD was calibrated using the silicon internal standard method. 002 Values ​​obtained through Bragg's formula The degree of graphitization was calculated using the formula G = (0.344 - d). 002 The result is calculated as (0.344 - 0.3354).

[0032] Particle size D 50

[0033] D 50 The particle size distribution was obtained through testing using a MalvernMastersizer 2000 laser particle size analyzer from Malvern Instruments Ltd., UK.

[0034] Electrochemical performance (battery charge / discharge capacity, initial coulombic efficiency, and 2C / 0.2C capacity retention) testing: The negative electrode material was first prepared into an aqueous coin cell, and lithium metal was used as the reference electrode. Then, charge / discharge tests were performed using the CT2001A battery tester from Wuhan Landian Electronics Co., Ltd., with a current of 0.1C (1C = 350mAh / g) and a voltage of 0.05-1.5V.

[0035] Example 1

[0036] (1) Based on the total dry basis of raw coal, 20% fat coal, 50% coking coal, 20% 1 / 3 coking coal and 10% lean coal are blended together;

[0037] (2) The blended coal obtained from coal blending is added to a coking oven for coking treatment at a coking temperature of 1050℃ and a coking time of 18 hours.

[0038] (3) The obtained coke is crushed by a mechanical pulverizer and then shaped by a shaping machine to obtain D. 50 =10μm powdered coke particles;

[0039] (4) The coke particles were graphitized at 2900℃ for 25h to obtain graphitized materials.

[0040] (5) The graphitized sample is sieved and demagnetized to obtain the product.

[0041] Example 2

[0042] (1) Based on the total dry basis of raw coal, 23% fat coal, 52% coking coal, 16% 1 / 3 coking coal and 9% lean coal are blended together;

[0043] (2) Add the mixed coal into the coking oven for coking treatment at a coking temperature of 1100℃ and a coking time of 16 hours.

[0044] (3) The coke is crushed by a mechanical crusher and then shaped by a shaping machine to obtain D. 50 =12μm powdered coke particles;

[0045] (4) The coke particles were graphitized at 3000℃ for 16h to obtain graphitized materials.

[0046] (5) The graphitized sample is sieved and demagnetized to obtain the product.

[0047] Example 3

[0048] (1) Based on the total dry basis of raw coal, 19% fat coal, 54% coking coal, 15% 1 / 3 coking coal and 12% lean coal are blended together;

[0049] (2) Add the mixed coal into the coking oven for coking treatment at a coking temperature of 1150℃ and a coking time of 12 hours.

[0050] (3) The coke is crushed by a mechanical crusher and then shaped by a shaping machine to obtain D. 50 =15μm powdered coke particles;

[0051] (4) The coke particles were graphitized at 3100℃ for 10h to obtain graphitized materials.

[0052] (5) The graphitized sample is sieved and demagnetized to obtain the product.

[0053] Comparative Example 1

[0054] (1) The anthracite is crushed by a mechanical crusher and then shaped by a shaping machine to obtain D. 50 =12μm powdered coal particles;

[0055] (2) Coal particles were graphitized at 3000℃ for 16 hours to obtain graphitized materials;

[0056] (3) The graphitized sample is sieved and demagnetized to obtain the product.

[0057] Comparative Example 2

[0058] (1) The lean coal is crushed by a mechanical crusher and then shaped by a shaping machine to obtain D. 50 =12μm powdered coal particles;

[0059] (2) Coal particles were graphitized at 3000℃ for 16 hours to obtain graphitized materials;

[0060] (3) The graphitized sample is sieved and demagnetized to obtain the product.

[0061] Comparative Example 3

[0062] (1) The asphalt coke is crushed by a mechanical crusher and then shaped by a shaping machine to obtain D. 50 =12μm powder particles;

[0063] (2) The particles were graphitized at 3000℃ for 16h to obtain graphitized materials;

[0064] (3) The graphitized sample is sieved and demagnetized to obtain the product.

[0065] Table 1

[0066]

[0067]

[0068] Table 2

[0069]

Claims

1. A coal-based graphite anode material, characterized in that, The peak intensities I110 of the (110) crystal plane and I004 of the (004) crystal plane of the coal-based graphite anode material satisfy the following conditions: I110 / I004≥1.0; the peak intensities I110 of the (110) crystal plane and I101 of the (101) crystal plane of the graphite anode material satisfy the following conditions: 1.5≤I110 / I101≤3.

0.

2. The coal-based graphite anode material according to claim 1, characterized in that, 1.0≤I110 / I004≤2.

0.

3. The coal-based graphite anode material according to claim 1, characterized in that, 1.4≤I110 / I004≤1.8, 1.7≤I110 / I101≤2.

5.

4. The coal-based graphite anode material according to any one of claims 1-3, characterized in that, The interlayer spacing d of the graphite anode material is ≤0.34nm; The degree of graphitization G of the graphite anode material satisfies 80% ≤ G ≤ 90%.

5. The coal-based graphite anode material according to claim 4, characterized in that, 0.336nm≤d≤0.337nm; 81%≤G≤89%.

6. The coal-based graphite anode material according to claim 5, characterized in that, 0.3364nm≤d≤0.3369nm; 85%≤G≤88%.

7. A method for preparing a coal-based graphite anode material according to any one of claims 1-6, comprising the following steps: 1) Based on the total weight of the raw coal on a dry, ash-free basis, blend 18-25% of fat coal, 49-55% of coking coal, 14-21% of 1 / 3 coking coal and 7-15% of lean coal. 2) The obtained mixed coal is added to a coking oven for coking treatment to obtain coke; 3) The obtained coke is crushed and shaped; 4) The coke particles crushed in step 3) are graphitized to obtain graphitized material; 5) The obtained graphitized material is sieved and demagnetized to obtain the coal-based graphite anode material.

8. The preparation method according to claim 7, characterized in that, In step 1), the raw coal comprises 20-23% fat coal, 50-55% coking coal, 15-20% 1 / 3 coking coal, and 8-12% lean coal.

9. The preparation method according to claim 7 or 8, characterized in that, In step 2), the coking conditions are: coking temperature 1000-1200℃, coking time 8-20 hours.

10. The preparation method according to claim 9, characterized in that, In step 3), the average particle size D50 of the obtained coke particles is 5-20 micrometers.

11. The preparation method according to claim 7, characterized in that, In step 4), the graphitization temperature is 2800-3400℃.

12. Use of the coal-based graphite anode material according to any one of claims 1-6 or the coal-based graphite anode material prepared by the preparation method according to any one of claims 7-11 in lithium-ion batteries.

13. A lithium-ion battery, characterized in that, The negative electrode of the lithium-ion battery contains the coal-based graphite negative electrode material according to any one of claims 1-6 or the coal-based graphite negative electrode material prepared by the preparation method according to any one of claims 7-11.

Citation Information

Patent Citations

  • Graphite material and preparation method thereof, negative electrode and lithium ion battery

    CN109768217A

  • Top-mounting coke oven mixed coal and formulation method

    CN109266368A

  • Crystalline carbon precursor coal blending method

    CN111029576A

  • Non-aqueous electrolyte secondary cell with high output power

    CN1744370A