An aqueous zinc-ion battery in-situ SEI film and a preparation method thereof

By constructing an in-situ SEI film of diethylene glycolamine and basic zinc sulfate on the surface of the zinc electrode, the problems of zinc anode corrosion and dendrite formation were solved, and the electrochemical performance and cycle stability of aqueous zinc-ion batteries were improved.

CN117374287BActive Publication Date: 2026-11-24SICHUAN UNIVERSITY OF SCIENCE AND ENGINEERING
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311400758.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-26
Publication Date
2026-11-24
Estimated Expiration
2043-10-26

AI Technical Summary

Technical Problem

Aqueous zinc-ion batteries lack a stable solid electrolyte interphase (SEI) at the zinc anode, leading to zinc anode corrosion and dendrite growth, which affects the battery's coulombic efficiency and cycle life.

Method used

Diethylene glycolamine was adsorbed onto the surface of a zinc electrode using an dip-coating method and then cured at high temperature to form an in-situ SEI film composed of diethylene glycolamine and basic zinc sulfate. This film blocks the direct contact between the zinc electrode and the electrolyte and regulates the nucleation and growth behavior of zinc ions.

Benefits of technology

It improves the electrochemical performance of aqueous zinc-ion batteries, enhances coulombic efficiency and cycle life, and inhibits the formation of zinc dendrites.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117374287B_ABST
    Figure CN117374287B_ABST
Patent Text Reader

Abstract

This invention discloses an in-situ SEI film for an aqueous zinc-ion battery and its preparation method. The preparation method includes: adsorbing diethylene glycolamine onto the surface of a zinc electrode using a dip-coating method, drying, and then performing a high-temperature curing treatment; finally, assembling an aqueous zinc-ion battery using zinc sulfate as the electrolyte, thereby constructing the SEI film in situ on the surface of the zinc electrode. The SEI film is composed of diethylene glycolamine and basic zinc sulfate. The SEI film obtained by this preparation method can not only block water-related side reactions but also regulate the nucleation and growth behavior of zinc ions, thereby improving the electrochemical performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of aqueous zinc-ion battery anode materials, and specifically relates to an in-situ SEI film for aqueous zinc-ion batteries and its preparation method. Background Technology

[0002] In recent years, aqueous zinc-ion batteries have gained popularity due to their low cost, abundant resources, and high theoretical capacity (820 mAh g). -1 The aqueous zinc-ion battery has attracted widespread attention due to its environmental friendliness and other characteristics. Compared to current secondary batteries based on organic electrolytes, aqueous electrolytes offer faster ion transport rates and inherent safety features. Because of these advantages, aqueous zinc-ion batteries are among the most promising candidates for the construction of large-scale energy storage grids in the future.

[0003] However, unlike lithium-ion batteries, aqueous zinc-ion batteries lack a stable solid electrolyte interphase (SEI) on the anode side. Therefore, the zinc anode is constantly exposed to water erosion (hydrogen evolution and corrosion), resulting in low coulombic efficiency and short cycle life. Due to the variability in the surface state of the zinc anode, during the zinc plating process, Zn... 2+ It tends to accumulate nuclei at low interface energies and grow rapidly into dendrites. The continuously growing zinc dendrites will pierce the separator, causing the positive and negative electrodes to be directly connected, resulting in a short circuit in the battery.

[0004] Currently, the main modification strategies for addressing dendrite formation and corrosion issues in zinc anodes include: (1) constructing 3D host materials; (2) modifying the electrolyte; and (3) coating with an artificial protective layer. However, the design of 3D host materials is often complex and costly, and while increasing the specific surface area, it also exacerbates side reactions, resulting in low coulombic efficiency of the battery. Although electrolyte additives can regulate the electrochemical environment at the electrode interface, they can also disrupt the rapid ion migration characteristics in aqueous electrolytes, and additives may alter the Zn content. 2+ The solvent sheath structure places higher demands on the structural stability of the matching cathode material; the artificial protective layer can isolate the electrode from direct contact with water, thereby blocking side reactions; however, the artificial interface layer applied by physical coating in Zn... 2+ Repeated electroplating / stripping processes can easily cause the zinc anode to peel off from the substrate, thus losing its protective effect. Therefore, how to firmly and permanently protect the zinc anode from corrosion and dendrite formation is a technical problem that those skilled in the art hope to solve. Summary of the Invention

[0005] In view of the above-mentioned shortcomings of the existing technology, the purpose of this invention is to provide an in-situ SEI film for aqueous zinc-ion batteries and a method for preparing the same. The SEI film obtained by this method can not only block water-related side reactions, but also regulate the nucleation and growth behavior of zinc ions, thereby improving the electrochemical performance of the battery.

[0006] The technical solution of this invention is implemented as follows: A method for preparing an in-situ SEI film for an aqueous zinc-ion battery involves using a dip-coating method to adsorb diethylene glycol amine onto the surface of a zinc electrode sheet, followed by drying and high-temperature curing. Finally, an aqueous zinc-ion battery is assembled using zinc sulfate as the electrolyte, thereby constructing the SEI film in situ on the surface of the zinc electrode sheet.

[0007] Furthermore, the specific steps include: (1) Mix diethylene glycolamine with an organic solvent to obtain a diethylene glycolamine mixed solution; (2) The zinc electrode sheet is immersed in a diethylene glycolamine mixed solution once or multiple times. After each immersion, the zinc electrode sheet is taken out and dried to obtain a pretreated zinc sheet. (3) The pretreated zinc sheet is cured at 90~150℃ for 0.5~2 h to obtain cured zinc sheet; (4) Using zinc sulfate as electrolyte, solidified zinc sheet is assembled into an aqueous zinc-ion battery as an electrode sheet, thereby constructing an SEI film in situ on the surface of the zinc electrode sheet.

[0008] Furthermore, in step (1), the content of diethylene glycolamine in the diethylene glycolamine mixed solution is 1%~10%.

[0009] Furthermore, the organic solvent is anhydrous ethanol, xylene-type alcohols, and aromatic solvents.

[0010] Further, in step (1), after mixing diethylene glycolamine and organic solvent, the mixture is ultrasonically treated for 30-40 min and then left to stand for 4-6 h to obtain a uniformly mixed diethylene glycolamine solution.

[0011] Furthermore, in step (2), the soaking time is 1~10 min each time, the drying temperature is 30~70℃, and the drying time is 30~40 min.

[0012] Furthermore, the concentration of zinc sulfate is 1~5 mol / L.

[0013] Furthermore, in step (3), the curing temperature is 100~130 ℃.

[0014] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention constructs an SEI film in situ on the surface of a zinc electrode substrate. The SEI film is composed of basic zinc sulfate and diethylene glycolamine. The SEI film prevents direct contact between the zinc electrode and the electrolyte, thereby blocking continuous hydrogen evolution and corrosion side reactions, ensuring a stable electrochemical environment at the electrode / electrolyte interface, and thus improving the electrochemical performance of the aqueous zinc-ion battery. This allows the battery to maintain high coulombic efficiency, long cycle life, and considerable rate performance during cycling.

[0015] Furthermore, when the SEI film contains diethylene glycolamine, its abundant polar functional groups (amino and hydroxyl groups) help induce uniform deposition of zinc ions and inhibit the formation of zinc dendrites.

[0016] 2. The multiple immersion method employed in this invention effectively ensures that diethylene glycolamine is uniformly adsorbed onto the surface of the zinc electrode substrate. Due to the affinity of amino and hydroxyl groups for zinc electrode sheets, diethylene glycolamine is easily adsorbed onto the surface of the zinc electrode sheet. Subsequent high-temperature curing further fixes it onto the zinc electrode sheet, thereby ensuring that the subsequently formed SEI film has a high bonding strength with the zinc electrode sheet. Attached Figure Description

[0017] Figure 1 - XRD pattern and Raman diagram of the in-situ SEI film prepared in Example 2.

[0018] Figure 2 -SEM image of the in-situ SEI film prepared in Example 2.

[0019] Figure 3 - Cyclic performance of SEI films prepared in Examples 1 to 3 and Comparative Example 2 assembled into symmetrical cells.

[0020] Figure 4 - SEM images of the zinc electrode surfaces after pretreatment in Examples 2, 4, 5, and Comparative Examples 1, 4, and 5.

[0021] Figure 5 - Rate performance of the SEI film prepared in Example 2 assembled into a Zn||Zn symmetric cell.

[0022] Figure 6 - Comparison of coulombic efficiencies of Zn||Cu batteries assembled in Example 6 and Comparative Example 3. Detailed Implementation

[0023] A method for preparing an in-situ SEI film for an aqueous zinc-ion battery involves adsorbing diethylene glycolamine onto the surface of a zinc electrode using a dip-coating method, followed by drying and high-temperature curing. Finally, an aqueous zinc-ion battery is assembled using zinc sulfate as the electrolyte, thereby constructing the SEI film in situ on the surface of the zinc electrode. Furthermore, the SEI film is composed of both diethylene glycolamine and basic zinc sulfate.

[0024] In practice, the specific steps include: (1) Mix diethylene glycolamine with an organic solvent to obtain a diethylene glycolamine mixed solution, wherein the content of diethylene glycolamine in the diethylene glycolamine mixed solution is 1%~10%; (2) The zinc electrode sheet is immersed in a diethylene glycolamine mixed solution once or multiple times. After each immersion, the zinc electrode sheet is taken out and dried to obtain a pretreated zinc sheet. (3) The pretreated zinc sheet is cured at 90~150℃ for 0.5~2 h to obtain cured zinc sheet; (4) Using zinc sulfate as electrolyte, solidified zinc sheet is assembled into an aqueous zinc-ion battery as an electrode sheet, thereby generating an SEI film in situ on the surface of the zinc electrode sheet.

[0025] When constructing an SEI film on the surface of a zinc electrode, the number of immersions and the immersion time must be controlled according to the content of diethylene glycolamine in the mixed solution. If the content of diethylene glycolamine in the mixed solution is too low, the surface of the zinc electrode will not be completely covered by diethylene glycolamine, which is not conducive to the subsequent formation of a dense and uniform SEI film. If the content of diethylene glycolamine in the mixed solution is too high, it is easy for diethylene glycolamine to form aggregates on the surface of the zinc electrode, resulting in a thicker SEI film, which hinders the transfer of zinc ions and affects the electrochemical performance of the aqueous zinc-ion battery.

[0026] Because of the high affinity of diethylene glycolamine for zinc due to its abundant polar functional groups (amino and hydroxyl groups), it is easy for diethylene glycolamine to be adsorbed onto the zinc electrode surface. High-temperature curing can further improve the bonding force between diethylene glycolamine and zinc sheet, thereby ensuring that the SEI film formed subsequently can be stably bonded to the zinc electrode sheet.

[0027] Finally, a Zn||Zn symmetric battery was assembled using zinc sulfate as the electrolyte and cured zinc sheets as electrodes. During the charge and discharge process, diethylene glycolamine on the surface of the zinc electrode reacts rapidly with zinc ions to generate basic zinc sulfate, thereby forming a dense and uniform SEI film at the electrode / electrolyte interface. Once the SEI film stabilizes, it isolates water from the zinc electrode, thus blocking continuous hydrogen evolution and corrosion side reactions, ensuring a stable electrochemical environment at the electrode / electrolyte interface. This improves the electrochemical performance of the aqueous zinc-ion battery, enabling it to maintain high coulombic efficiency, long cycle life, and considerable rate performance during cycling. Furthermore, the diethylene glycolamine in the SEI film can effectively regulate the nucleation and growth behavior of zinc ions, thereby inhibiting the formation of zinc dendrites.

[0028] The organic solvents used here should be miscible with diethylene glycol amine, volatile, and non-reactive with the zinc substrate material. Examples include anhydrous ethanol, xylene alcohols, and aromatic solvents.

[0029] In specific implementation, the curing temperature in step (3) is preferably 100~130 ℃. At this temperature, it is beneficial for the uniform dispersion of diethylene glycolamine on the zinc electrode, while also preventing the diethylene glycolamine organic film from breaking or even decomposing.

[0030] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.

[0031] Example 1 Diethylene glycolamine and anhydrous ethanol were mixed evenly at a volume ratio of 1:19 to obtain mixed solution A. Zinc electrode sheets were immersed in mixed solution A for 5 min by dip coating, then removed and dried at 60 °C for 30 min to obtain pretreated zinc sheet A. Pretreated zinc sheet A was immersed in mixed solution A again for 2 min, then removed, dried and cured at 120 °C for 1 h to obtain pretreated zinc sheet B. Pretreated zinc sheet B was assembled into a Zn||Zn symmetric cell, using 2M ZnSO4 as the electrolyte and glass fiber filter paper as the separator.

[0032] Example 2 This embodiment is the same as Embodiment 1, except that the first soaking time is 3 minutes and the second soaking time is 1 minute.

[0033] Example 3 This embodiment is the same as Embodiment 1, except that the first soaking time is 1 minute and the second soaking time is 30 seconds.

[0034] Example 4 This embodiment is the same as Embodiment 2, except that the curing temperature is 90 ℃.

[0035] Example 5 This embodiment is the same as Embodiment 2, except that the curing temperature is 150 ℃.

[0036] Example 6 This embodiment is the same as Embodiment 2, except that the pretreated zinc sheet B is assembled into a Zn||Cu battery.

[0037] Comparative Example 1 This embodiment is the same as Embodiment 2, except that the curing temperature is 60 ℃.

[0038] Comparative Example 2 In this embodiment, untreated zinc electrode sheets are used to assemble a Zn||Zn symmetric cell. The electrolyte used is 2MZnSO4, and the separator is glass fiber filter paper.

[0039] Comparative Example 3 In this embodiment, an untreated zinc electrode sheet is used to assemble a Zn||Cu battery. The electrolyte used is 2MZnSO4, and the separator is glass fiber filter paper.

[0040] Comparative Example 4 This embodiment is the same as Embodiment 2, except that in the mixed solution A, diethylene glycolamine and anhydrous ethanol are mixed at a volume ratio of 1:999.

[0041] Comparative Example 5 This embodiment is the same as Embodiment 2, except that the diethylene glycolamine and anhydrous ethanol in mixed solution A are in a volume ratio of 1:4.

[0042] 1. The XRD pattern, Raman spectroscopy pattern, and SEM image of the in-situ SEI film formed by immersing the treated zinc electrode sheet obtained in Example 2 in ZnSO4 electrolytic electrolyte are shown below. Figure 1 (a) Figure 1 (b) and Figure 2 As shown.

[0043] Depend on Figure 1 (a) It can be seen that the characteristic peaks appearing at 8.093°, 21.328°, and 33.007° belong to the characteristic peaks of (Zn(OH)2)3(ZnSO4)(H2O)5, indicating that the SEI membrane contains basic zinc sulfate ZHS generated in situ by DGA and electrolyte. Figure 1 (b) The functional groups of the SEI membrane are the same as those of diethylene glycolamine, indicating that diethylene glycolamine is still present in the formed SEI membrane, that is, the formed SEI membrane is a composite membrane of diethylene glycolamine and basic zinc sulfate.

[0044] Depend on Figure 2 It can be seen that the in-situ generated SEI film is formed by a dense arrangement of lamellar ZHS layers. The dense ZHS layers help to isolate the zinc electrode from direct contact with water, while simultaneously regulating the Zn content. 2+ The migration path induces uniform deposition of zinc ions, which helps to avoid the formation of zinc dendrites.

[0045] 2. Constant current charge-discharge tests were conducted on the Zn||Zn symmetric batteries assembled in Examples 1, 2, 3, and Comparative Example 2. The cycle performance results are as follows: Figure 3 As shown in (a), 3(b), 3(c) and 3(d).

[0046] Depend on Figure 3 (d) It can be seen that, due to Zn 2+ During the deposition process, the "point effect" causes zinc dendrites to grow rapidly and pierce the separator, leading to a short circuit in the battery. Furthermore, severe side reactions cause Zn... 2+ As the battery is continuously consumed, its cycle reversibility decreases. Figure 3 (a) ~ Figure 3 (d) As can be seen, compared with Comparative Example 2, the zinc electrode sheet prepared by the present invention can effectively improve the cycle life of the Zn||Zn symmetric cell, and maintains an almost single cycle curve during charge and discharge. This indicates that the SEI film constructed in situ on the surface of the zinc electrode sheet has a positive effect on corrosion side reactions and Zn 2+ Deposition behavior has a regulatory role.

[0047] 3. The surface morphology of the zinc electrodes after treatment in Examples 2, 1, 4, and 5 are as follows: Figure 4 As shown in (a), 4(b), 4(c), and 4(d), the surface morphology of the zinc electrodes after treatment in Comparative Examples 4 and 5 is as follows. Figure 4 (e) and Figure 4 As shown in (f).

[0048] Depend on Figure 4 (a) ~ Figure 4 (d) It is evident that when the curing temperature is low, the diethylene glycolamine on the zinc electrode surface tends to aggregate into clumps. As the temperature increases, it facilitates the uniform dispersion of diethylene glycolamine on the zinc electrode. However, excessively high temperatures will cause the diethylene glycolamine organic film to rupture or even decompose, thus affecting the subsequent formation of a stable SEI film. Furthermore, as... Figure 4 As shown in (e) and (f), if the DGA content in the mixed solution is low, a continuous SEI cannot be formed on the zinc electrode surface. If the DGA content is high, an organic insulating layer will accumulate on the zinc electrode surface, which is not conducive to the migration of zinc ions.

[0049] 4. The rate performance of the Zn||Zn symmetric cell assembled in Example 2 was tested, and the rate performance was as follows: Figure 5 As shown, even with the continuous increase in surface current density and areal capacity density of the zinc electrode, the time-voltage curve of the cell remains very stable, indicating the positive effect of the SEI film on stabilizing the zinc anode.

[0050] 5. The coulombic efficiency curves of the Zn||Cu batteries assembled in Example 6 and Comparative Example 3 are shown below. Figure 6 As shown, the battery assembled with untreated zinc electrode sheets fails rapidly in a short period of time, which is attributed to severe side reactions that promote dendrite growth; in contrast, the battery assembled with treated electrode sheets exhibits excellent stability and reversibility, thanks to the favorable regulation of zinc ion diffusion and deposition behavior by the SEI film.

[0051] Finally, it should be noted that the above embodiments of the present invention are merely illustrative examples and not intended to limit the implementation of the invention. Those skilled in the art can make other variations and modifications based on the above description. It is impossible to exhaustively list all possible implementations here. All obvious variations or modifications derived from the technical solutions of this invention are still within the scope of protection of this invention.

Claims

1. A method for preparing an in-situ SEI film for an aqueous zinc-ion battery, characterized in that, Diethylene glycolamine was applied to the surface of a zinc electrode sheet using a dip-coating method. After drying, the electrode sheet was cured at high temperature. Finally, an aqueous zinc-ion battery was assembled using zinc sulfate as the electrolyte, thereby constructing the SEI film in situ on the surface of the zinc electrode sheet.

2. The method for preparing an in-situ SEI film for an aqueous zinc-ion battery according to claim 1, characterized in that, Specifically, the following steps are included: (1) Mix diethylene glycolamine with an organic solvent to obtain a diethylene glycolamine mixed solution; (2) The zinc electrode sheet is immersed in a diethylene glycolamine mixed solution once or multiple times. After each immersion, the zinc electrode sheet is taken out and dried to obtain a pretreated zinc sheet. (3) The pretreated zinc sheet is cured at 90~150℃ for 0.5~2 h to obtain cured zinc sheet; (4) Using zinc sulfate as electrolyte, solidified zinc sheet is assembled into an aqueous zinc-ion battery as an electrode sheet, thereby generating an SEI film in situ on the surface of the zinc electrode sheet.

3. The method for preparing an in-situ SEI film for an aqueous zinc-ion battery according to claim 2, characterized in that, In step (1), the content of diethylene glycolamine in the diethylene glycolamine mixed solution is 1%~10%.

4. A method for preparing an in-situ SEI film for an aqueous zinc-ion battery according to claim 2 or 3, characterized in that, The organic solvent is anhydrous ethanol, xylene-type alcohols, and aromatic solvents.

5. The method for preparing an in-situ SEI film for an aqueous zinc-ion battery according to claim 4, characterized in that, Step (1): After mixing diethylene glycolamine and organic solvent, the mixture is ultrasonically treated for 30-40 min and then left to stand for 4-6 h to obtain a uniformly mixed diethylene glycolamine solution.

6. The method for preparing an in-situ SEI film for an aqueous zinc-ion battery according to claim 2, characterized in that, In step (2), the soaking time is 1~10 min each time, the drying temperature is 30~70℃, and the drying time is 30~40 min.

7. The method for preparing an in-situ SEI film for an aqueous zinc-ion battery according to claim 2, characterized in that, The concentration of zinc sulfate is 1~5 mol / L.

8. The method for preparing an in-situ SEI film for an aqueous zinc-ion battery according to claim 2, characterized in that, In step (3), the curing temperature is 100~130 ℃.

9. An in-situ SEI membrane for an aqueous zinc-ion battery, characterized in that, The in-situ SEI membrane for an aqueous zinc-ion battery was prepared using any one of the preparation methods described in claims 1 to 8.

Citation Information

Patent Citations

  • Zinc negative electrode and preparation method and application thereof

    CN114597407A

  • Preparation method of modified zinc negative electrode and application of modified zinc negative electrode in aqueous zinc ion battery

    CN116759522A