A tin-lead perovskite photodetector based on n'n-carbonyldiimidazole as a passivation layer and a preparation method thereof

By using N′N-carbonyldiimidazole as a passivation layer in a tin-lead perovskite photodetector, the problems of easy oxidation and surface roughness of the thin film were solved, the stability and photoelectric conversion efficiency of the device were improved, and high-sensitivity near-infrared photodetection was achieved.

CN117377359BActive Publication Date: 2026-11-24JILIN UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311396426.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-26
Publication Date
2026-11-24
Estimated Expiration
2043-10-26

AI Technical Summary

Technical Problem

Tin-lead perovskite photodetector films are prone to oxidation, have rough surfaces and low coverage, resulting in poor stability, large dark current, and difficulty in achieving high-sensitivity near-infrared photodetection.

Method used

Using N′N-carbonyldiimidazole as a passivation layer, deep-level defects are eliminated and photogenerated carrier trapping is reduced through contact with the perovskite layer interface and surface, thereby improving device performance.

Benefits of technology

This enhances the stability and photoelectric conversion efficiency of the photodetector, optimizes the open-circuit voltage and external quantum efficiency, and improves the electrical signal quality and detection sensitivity of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117377359B_ABST
    Figure CN117377359B_ABST
Patent Text Reader

Abstract

A tin-lead perovskite photodetector based on N'N-carbonyldiimidazole as a passivation layer and its fabrication method are disclosed, belonging to the field of perovskite optoelectronic device technology. The detector consists of an ITO conductive glass anode, a PTAA anode buffer layer, and a Cs... 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 I3 tin-lead perovskite polycrystalline thin film, N'N-carbonyl diimidazole passivation layer, C 60 The cathode consists of a BCP cathode buffer layer and a Cu cathode. This invention utilizes the lone pair electrons provided by N and O in the N'N-carbonyldiimidazole passivation layer and the uncoordinated Pb in the perovskite layer. 2+ Ion bonding effectively eliminates deep-level defects in perovskites, reduces ion migration during device operation, and significantly improves device performance. The optimization effect is mainly reflected in V. oc By improving open-circuit voltage and external quantum efficiency (EQE), defects are passivated, traps are reduced, and photoelectric conversion efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of perovskite optoelectronic device technology, specifically relating to a tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as a passivation layer and its preparation method. Background Technology

[0002] Photodetectors, as photoelectric conversion devices, play a crucial role in both military and civilian applications. Organic-inorganic hybrid perovskite materials, due to their advantages such as high mobility, low defect density, long carrier lifetime, and tunable optical performance, have been widely used in various optoelectronic devices. Currently, tin-lead perovskite, with its narrower bandgap, higher charge mobility, and lower toxicity, has been used to replace some lead, extending the perovskite absorption spectrum into the near-infrared region, and has broad application prospects in the near-infrared detection field. However, although tin-lead perovskite possesses a narrow bandgap and broad spectrum, its thin films are prone to oxidation, have rough surfaces, and low coverage, resulting in poor stability, high dark current, and susceptibility to short circuits, making it difficult to achieve high-sensitivity and high-stability near-infrared photodetectors. Therefore, selecting suitable passivation materials, developing effective processes, and improving the fundamental performance and operational stability of tin-lead perovskite polycrystalline thin films through methods such as adding defect passivation layers, doping in the active layer, and using anti-solvents to improve the crystallization process are of great significance to the development of near-infrared perovskite photodetectors. Summary of the Invention

[0003] The purpose of this invention is to provide a tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as a passivation layer and its preparation method.

[0004] The photodetector designed in this invention comprises, from bottom to top, an ITO conductive glass anode, a PTAA (poly(bis(4-phenyl)(2,4,6-trimethylphenyl)amine)) anode buffer layer, a tin-lead perovskite polycrystalline thin film prepared by the anti-solvent method, an N′N-carbonyl diimidazole passivation layer, and a C 60 The device consists of a (fμllerene) / BCP (bathocμproine) cathode buffer layer and a Cu cathode. The tin-lead perovskite material used in the device is Cs. 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 I3.

[0005] The light signal is incident from the ITO side. Due to the photoelectric effect, electron-hole pairs are generated in the tin-lead perovskite material. The PTAA anode buffer layer blocks the electrons. 60 C in the BCP cathode buffer layer 60The layer blocks holes, and the continuous accumulation of electrons and holes creates a built-in electric field. Due to this built-in electric field, electrons and holes will move towards C. 60 Moving in the direction of PTAA, it ultimately converts the optical signal into an electrical signal. However, due to the presence of a large amount of uncoordinated Pb in the perovskite... 2+ It will trap photogenerated carriers, thereby reducing device performance; and Sn 2+ Due to its susceptibility to oxidation, the stability of the device needs improvement. This invention proposes a strategy using N′N-carbonyldiimidazole as a passivation layer. N′N-carbonyldiimidazole can effectively fill the interface and surface of the perovskite layer, mitigating the contact between the perovskite layer and water / oxygen. Furthermore, the lone pair electrons provided by the N and O atoms in N′N-carbonyldiimidazole interact with the uncoordinated Pb atoms in the perovskite layer. 2+ Ion bonding effectively eliminates deep-level defects in perovskites, reducing ion migration during device operation and thus minimizing lattice damage caused by ion migration, significantly improving device performance. Ultimately, it passivates defects, reduces trapping of photogenerated electrons, and improves photoelectric conversion efficiency. The optimization effect is mainly reflected in V... oc On (open circuit voltage) and EQE (external quantum efficiency).

[0006] The method for fabricating a tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as a passivation layer, as described in this invention, comprises the following steps:

[0007] 1. Place ITO conductive glass (260-300mm) 2 The ITO conductive glass is ultrasonically cleaned with acetone, ethanol and deionized water for 15-20 minutes in sequence, and then dried with nitrogen to obtain a dry and clean ITO conductive glass. It is then treated with ultraviolet ozone for 20-30 minutes to serve as the anode of the device.

[0008] 2. Dissolve 2-4 mg of PTAA in 1-2 mL of chlorobenzene, stir at room temperature for 8-12 h, and then spin coat it onto ITO conductive glass in a nitrogen-filled glove box at a spin coating speed of 3000-4000 rpm for 30-40 s. Then place it on a preheated hot plate and anneal at 90-110 °C for 10-20 min to obtain a PTAA anode buffer layer with a thickness of 30-40 nm.

[0009] 3. Mix DMF and DMSO at a volume ratio of 5:1 to obtain a DMF-DMSO mixed solvent; mix the raw materials MAI, FAI, PbI2, SnI2 and CsI according to the tin-lead perovskite Cs 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5I3 was added to the mixed solvent in a stoichiometric ratio, and the mixture was stirred in a nitrogen-filled glove box for 6–8 h to obtain a perovskite precursor solution with a concentration of 1–1.5 mol / L. Then, in a nitrogen-filled glove box at 4000–5000 rpm, 50–70 μL of DMF was dropped onto the PTAA anode buffer layer for wetting. After wetting for 10–15 s, 50–80 μL of the perovskite precursor solution was dropped onto the PTAA anode buffer layer and spin-coated for 20–40 s. With 15–20 s remaining in the spin-coating time, 300–350 μL of the anti-solvent chlorobenzene was added. After spin-coating, the device was transferred to a preheated stage and annealed at 90–110 °C for 10–20 min to obtain high-quality Cs. 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 I3 tin-lead perovskite thin film with a thickness of 500–700 nm;

[0010] 4. Using isopropanol as a solvent, prepare an N′N-carbonyldiimidazole passivation solution with a concentration of 0.5–2 mg / mL. In a nitrogen-filled glove box, spin-coat the prepared passivation solution onto the perovskite layer at a speed of 3000–4000 rpm for 30–40 s. Then, place it on a preheated hot plate and anneal at 90–110 °C for 30–50 s to obtain an N′N-carbonyldiimidazole passivation layer with a thickness of 10–15 nm.

[0011] 5. In 6×10 -5 ~9×10 -4 Under Pa conditions, using a multi-source organic vapor deposition system, CN-carbonyldiimidazole passivation layers with a thickness of 20–40 nm were prepared on the N′N-carbonyldiimidazole passivation layer by vacuum evaporation. 60 Layer, then in C 60 A BCP layer with a thickness of 5-10 nm is then vacuum-deposited on the top layer to obtain C. 60 / BCP cathode buffer layer;

[0012] 6. In 6×10 -5 ~9×10 -4 Under the condition of Pa, a Cu cathode with a thickness of 80-90 nm was prepared on the cathode buffer layer by vacuum evaporation using a multi-source organic vapor deposition system, thereby preparing the tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as the passivation layer of the present invention. Attached Figure Description

[0013] Figure 1 : A schematic diagram of the tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as a passivation layer according to the present invention; the names of the parts from bottom to top are: ITO conductive glass 1, PTAA anode buffer layer 2, Cs0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 3. I3 tin-lead perovskite thin film; 4. N′N-carbonyl diimidazole passivation layer; 5. C 60 / BCP cathode buffer layer 5, Cu cathode 6;

[0014] Figure 2 Photoluminescence (PL) spectra of the perovskite layers prepared in Examples 1 and 3, with and without N′N-carbonyldiimidazole passivation layers, were measured under 325 nm laser irradiation. The figures show that Cs... 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 The I3 perovskite film exhibited a PL peak at 964 nm. After adding the passivation layer N′N-carbonyldiimidazole, we observed a slight blue shift from 964 nm to 955 nm, along with a slight increase in the intensity of the PL peak. We attribute this 9 nm blue shift to the successful passivation of the perovskite by N′N-carbonyldiimidazole. This provides valid evidence that N′N-carbonyldiimidazole can effectively passivate perovskite defects.

[0015] Figure 3 The results of light and dark current tests on the tin-lead perovskite photodetectors prepared in Examples 1-3 are shown. The voltage scan range is -200mV to 1200mV, and the voltage is provided by a digital source meter. Logarithmic curves were used to obtain clearer images. Curves a, b, and c represent the dark current of the devices prepared in Examples 1-3 under dark conditions. The devices exhibit obvious rectification characteristics. The dark current density of curve a at -100mV is 6.08 × 10⁻⁶. -5 mA cm -2 The dark current density of curves b and c after adding the passivation layer is 8.51 × 10⁻⁶ at -100 mV. -5 mA cm -2 7.57×10 -5 mA cm -2 There was no significant change. Curves d, e, and f represent the results of devices prepared in Examples 1-3 at 100mW cm⁻¹. -2 The photocurrent under AM1.5G standard sunlight is approximately 4 to 5 orders of magnitude greater than the dark current. As shown in the figure, the open-circuit voltages displayed by curves b and c are significantly higher than those of curve a, indicating that the device passivated with N′N-carbonyldiimidazole significantly reduces voltage loss, increases the open-circuit voltage, and results in a photodetector with superior performance.

[0016] Figure 4Cs prepared in Examples 1 and 3 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 The external quantum efficiency (EQE) test curves of the I3 tin-lead perovskite thin film photodetector (incident light wavelength range of 400–110 nm, with curves a and b corresponding to Examples 1 and 3 respectively) show that the device exhibits good photoelectric conversion capability in the visible and near-infrared light ranges. Example 3, with the addition of an N′N-carbonyldiimidazole passivation layer, exhibits even higher EQE, mainly improved in the 500–750 nm and near 900 nm ranges. Its conversion efficiency exceeds 80% around 530 nm and exceeds 60% around 900 nm, with a cutoff at approximately 1000 nm, consistent with perovskite absorption. Therefore, the tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as a passivation layer prepared by the method described in this invention has good photoelectric conversion capability, and N′N-carbonyldiimidazole effectively passivates defects.

[0017] Figure 5 The responsivity (R) of the tin-lead perovskite photodetector prepared in Example 3, based on N′N-carbonyldiimidazole as a passivation layer, was calculated using the external quantum efficiency. The specific calculation formula is as follows:

[0018]

[0019] q is the electron charge, λ is the incident light wavelength, h is Planck's constant, c is the speed of light, and EQE is the external quantum efficiency.

[0020] The device fabricated using this method achieved a response of 0.45AW at 745nm and 925nm. -1 Therefore, the tin-lead perovskite photodetector prepared by this method, based on N′N-carbonyldiimidazole as a passivation layer, can produce a good current response to incident light within the operating wavelength range.

[0021] Figure 6 Example 3 shows the noise current test curve of the tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as the passivation layer (the noise current was measured using a Fast Fourier Transform (FFT) signal analyzer and a current preamplifier). The horizontal line in the figure represents the noise margin of the device, calculated from the device's dark current. As shown in the figure, the noise current of the device fabricated using this method at 70Hz is 4.16 × 10⁻⁶. -13A, this is related to the low defect density of the device, further demonstrating that the presence of the N′N-carbonyldiimidazole passivation layer reduces the defects in the perovskite layer. This proves that the active layer of the tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as the passivation layer has a low defect density, resulting in low complexity of the electrical signals obtained during device operation.

[0022] Figure 7 Example 3 shows the calculated detection sensitivity curve of the tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as a passivation layer. Detection sensitivity is an important parameter representing the strength of the device's detection capability. The specific detection sensitivity (D*) of the photodetector described in this invention can be obtained through the following equation:

[0023]

[0024] In the formula, A is the active layer area, Δf is the bandwidth, and NEP is the noise equivalent power, which can be measured using experimental instruments. The unit for specific detection sensitivity is cm Hz. -1 / 2 W -1 (Jones). The device fabricated using this method achieved a detection sensitivity (D*) of 2.2 × 10⁻⁶ nm in the 700–950 nm range. 11 Jones demonstrated that tin-lead perovskite photodetectors based on N′N-carbonyldiimidazole as a passivation layer have good detection capabilities for weak light. Detailed Implementation

[0025] Example 1:

[0026] 1. ITO conductive glass (19.7*14.7mm, area 289.59mm²) 2 The ITO conductive glass was ultrasonically cleaned with acetone, ethanol and deionized water for 20 minutes in sequence, and then dried with nitrogen to obtain a dry and clean ITO conductive glass. After being treated with ultraviolet ozone for 20 minutes, it was used as the anode of the device.

[0027] 2. Dissolve 2 mg of PTAA in 1 mL of chlorobenzene, stir at room temperature for 8 hours, and then spin-coat the solution onto a surface with an area of ​​289.59 mm² in a nitrogen-filled glove box. 2 On the ITO conductive glass, the spin coating speed was 4000 rpm and the spin coating time was 40 s. Then, it was placed on a preheated hot plate and annealed at 110°C for 20 min to obtain a PTAA anode buffer layer with a thickness of 30 nm.

[0028] 3. First, a tin-lead perovskite precursor solution was prepared by mixing DMF and DMSO at a volume ratio of 5:1 to obtain a DMF-DMSO mixed solvent. The raw materials MAI, FAI, PbI2, SnI2, and CsI were then mixed according to the Cs... 0.05 MA0.45 FA 0.5 Pb 0.5 Sn 0.5 I3 was added to the mixed solvent in a stoichiometric ratio, and the mixture was stirred for 8 hours in a nitrogen-filled glove box to obtain a perovskite precursor solution with a concentration of 1.5 mol / L. The precursor solution was then spin-coated onto the prepared PTAA device in the glove box. Using an anti-solvent method, spin-coating was performed at 4000 rpm for 40 seconds. 70 μL of DMF was added dropwise before spin-coating to wet the device. With 30 seconds remaining in the spin-coating time, 80 μL of the perovskite precursor solution was added dropwise, and with 15 seconds remaining, 300 μL of the anti-solvent chlorobenzene was added dropwise. After spin-coating, the device was transferred to a preheated hot plate and annealed at 110 °C for 10 minutes to obtain high-quality Cs. 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 I3 tin-lead perovskite thin film with a thickness of 600 nm;

[0029] 4. In 7×10 -4 Under Pa conditions, using a multi-source organic vapor deposition system, C20 nm thick films were prepared on tin-lead perovskite films via vacuum evaporation to achieve a C20 nm thickness. 60 Layer, then in C 60 A BCP layer with a thickness of 8 nm is then deposited on top of the layer to obtain C. 60 / BCP cathode buffer layer;

[0030] 5. In 7×10 -4 Under the condition of Pa, a Cu with a thickness of 80 nm was prepared on the cathode buffer layer by vacuum evaporation using a multi-source organic vapor phase molecular deposition system, thereby preparing a tin-lead perovskite photodetector.

[0031] Example 2:

[0032] 1. ITO conductive glass (19.7*14.7mm, area 289.59mm²) 2 The ITO conductive glass was ultrasonically cleaned with acetone, ethanol and deionized water for 20 minutes in sequence, and then dried with nitrogen to obtain a dry and clean ITO conductive glass. After being treated with ultraviolet ozone for 20 minutes, it was used as the anode of the device.

[0033] 2. Dissolve 2 mg of PTAA in 1 mL of chlorobenzene, stir at room temperature for 8 hours, and then spin-coat the solution onto a surface with an area of ​​289.59 mm² in a nitrogen-filled glove box. 2 On the ITO conductive glass, the spin coating speed was 4000 rpm and the spin coating time was 40 s. Then, it was placed on a preheated hot plate and annealed at 110°C for 20 min to obtain a PTAA anode buffer layer with a thickness of 30 nm.

[0034] 3. First, a tin-lead perovskite precursor solution was prepared by mixing DMF and DMSO at a volume ratio of 5:1 to obtain a DMF-DMSO mixed solvent. The raw materials MAI, FAI, PbI2, SnI2, and CsI were then mixed according to the Cs... 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 I3 was added to the mixed solvent in a stoichiometric ratio, and the mixture was stirred for 8 hours in a nitrogen-filled glove box to obtain a perovskite precursor solution with a concentration of 1.5 mol / L. Then, in a nitrogen-filled glove box at 4000 rpm, 70 μL of DMF was dropped onto the PTAA anode buffer layer for wetting. After wetting for 10 seconds, 80 μL of the perovskite precursor solution was added to the PTAA anode buffer layer and spin-coated for 30 seconds. With 15 seconds remaining in the spin-coating time, 300 μL of the anti-solvent chlorobenzene was added. After spin-coating, the device was transferred to a preheated stage and annealed at 110 °C for 10 minutes to obtain high-quality Cs. 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 I3 tin-lead perovskite thin film with a thickness of 600 nm;

[0035] 4. An N′N-carbonyldiimidazole passivation layer was prepared on the perovskite layer. Using isopropanol as a solvent, a passivation solution with a concentration of 0.5 mg / mL was prepared. The prepared solution was spin-coated on the tin-lead perovskite film at a speed of 4000 rpm for 30 s in a glove box filled with nitrogen. Then, it was placed on a preheated hot plate and annealed at 90°C for 30 s to obtain an N′N-carbonyldiimidazole passivation layer with a thickness of 10 nm.

[0036] 5. In 7×10 -4 Under Pa conditions, a 20 nm thick C layer was prepared on an N′N-carbonyldiimidazole passivation layer using a multi-source organic vapor deposition system via vacuum evaporation. 60 Layer, then in C 60 A BCP layer with a thickness of 8 nm is then deposited on top of the layer to obtain C. 60 / BCP cathode buffer layer;

[0037] 6. In 7×10 -4 Under the condition of Pa, a Cu with a thickness of 80 nm was prepared on the cathode buffer layer by vacuum evaporation using a multi-source organic vapor phase molecular deposition system, thereby preparing the tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as the passivation layer as described in this invention.

[0038] Example 3:

[0039] 1. ITO conductive glass (19.7*14.7mm, area 289.59mm²) 2 The ITO conductive glass was ultrasonically cleaned with acetone, ethanol and deionized water for 20 minutes in sequence, and then dried with nitrogen to obtain a dry and clean ITO conductive glass. After being treated with ultraviolet ozone for 20 minutes, it was used as the anode of the device.

[0040] 2. Dissolve 2 mg of PTAA in 1 mL of chlorobenzene, stir at room temperature for 8 hours, and then spin-coat the solution onto a surface with an area of ​​289.59 mm² in a nitrogen-filled glove box. 2 On the ITO conductive glass, the spin coating speed was 4000 rpm and the spin coating time was 40 s. Then, it was placed on a preheated hot plate and annealed at 110°C for 20 min to obtain a PTAA anode buffer layer with a thickness of 30 nm.

[0041] 3. First, a tin-lead perovskite precursor solution was prepared by mixing DMF and DMSO at a volume ratio of 5:1 to obtain a DMF-DMSO mixed solvent. The raw materials MAI, FAI, PbI2, SnI2, and CsI were then mixed according to the Cs... 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 I3 was added to the mixed solvent in a stoichiometric ratio, and the mixture was stirred for 8 hours in a nitrogen-filled glove box to obtain a perovskite precursor solution with a concentration of 1.5 mol / L. Then, in a nitrogen-filled glove box at 4000 rpm, 70 μL of DMF was dropped onto the PTAA anode buffer layer for wetting. After wetting for 10 seconds, 80 μL of the perovskite precursor solution was added to the PTAA anode buffer layer and spin-coated for 30 seconds. With 15 seconds remaining in the spin-coating time, 300 μL of the anti-solvent chlorobenzene was added. After spin-coating, the device was transferred to a preheated stage and annealed at 110 °C for 10 minutes to obtain high-quality Cs. 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 I3 tin-lead perovskite thin film with a thickness of 600 nm;

[0042] 4. An N′N-carbonyldiimidazole passivation layer was prepared on the perovskite layer. Using isopropanol as a solvent, a passivation solution with a concentration of 1 mg / mL was prepared. The prepared solution was spin-coated on the tin-lead perovskite film at a speed of 4000 rpm for 30 s in a nitrogen-filled glove box. Then, it was placed on a preheated hot plate and annealed at 90°C for 30 s to obtain an N′N-carbonyldiimidazole passivation layer with a thickness of 10 nm.

[0043] 5. In 7×10 -4Under Pa conditions, a 20 nm thick C layer was prepared on an N′N-carbonyldiimidazole passivation layer using a multi-source organic vapor deposition system via vacuum evaporation. 60 Layer, then in C 60 A BCP layer with a thickness of 8 nm is then deposited on top of the layer to obtain C. 60 / BCP cathode buffer layer;

[0044] 6. In 7×10 -4 Under the condition of Pa, a Cu with a thickness of 80 nm was prepared on the cathode buffer layer by vacuum evaporation using a multi-source organic vapor phase molecular deposition system, thereby preparing the tin-lead perovskite photodetector based on N′N-carbonyldiimidazole as the passivation layer as described in this invention.

Claims

1. A method for fabricating a tin-lead perovskite photodetector based on N'N-carbonyldiimidazole as a passivation layer, comprising the following steps: (1) The ITO conductive glass is ultrasonically cleaned with acetone, ethanol and deionized water for 15-20 minutes in sequence, and then dried with nitrogen to obtain a dry and clean ITO conductive glass. Then it is treated with ultraviolet ozone for 20-30 minutes to be used as the anode of the device. (2) Dissolve 2-4 mg of PTAA in 1-2 mL of chlorobenzene, stir at room temperature for 8-12 h, spin coat it onto ITO conductive glass in a glove box filled with nitrogen, and then place it on a preheated hot plate for annealing to obtain a PTAA anode buffer layer with a thickness of 30-40 nm. (3) Mix DMF and DMSO at a volume ratio of 5:1 to obtain a DMF-DMSO mixed solvent; mix raw materials MAI, FAI, PbI2, SnI2 and CsI according to the tin-lead perovskite Cs 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 I3 was added to the mixed solvent in a stoichiometric ratio, and the mixture was stirred in a nitrogen-filled glove box for 6–8 h to obtain a perovskite precursor solution with a concentration of 1–1.5 mol / L. Then, in a nitrogen-filled glove box at 4000–5000 rpm, DMF was dropped onto the PTAA anode buffer layer for wetting. After wetting for 10–15 s, the perovskite precursor solution was dropped onto the PTAA anode buffer layer and spin-coated for 20–40 s. With 15–20 s remaining in the spin-coating time, the anti-solvent chlorobenzene was added. After spin-coating, the device was transferred to a preheated hot plate for annealing to obtain Cs. 0.05 MA 0.45 FA 0.5 Pb 0.5 Sn 0.5 I3 tin-lead perovskite thin film with a thickness of 500–700 nm; (4) Using isopropanol as a solvent, prepare an N'N-carbonyldiimidazole passivation solution with a concentration of 0.5-2 mg / mL. Spin-coat the prepared passivation solution onto the perovskite layer in a glove box filled with nitrogen. Then place it on a preheated hot plate for annealing to obtain an N'N-carbonyldiimidazole passivation layer with a thickness of 10-15 nm. (5) Vacuum evaporation of C with a thickness of 20-40 nm on the N'N-carbonyldiimidazole passivation layer. 60 Layer, then in C 60 A BCP layer with a thickness of 5-10 nm is then vacuum-deposited on the top layer to obtain C. 60 / BCP cathode buffer layer; (6) A Cu cathode with a thickness of 80-90 nm is vacuum-deposited on the cathode buffer layer to prepare the tin-lead perovskite photodetector based on N'N-carbonyldiimidazole as a passivation layer.

2. The method for fabricating a tin-lead perovskite photodetector based on N'N-carbonyldiimidazole as a passivation layer as described in claim 1, characterized in that: Step (1) The area of ​​the ITO conductive glass is 260-300 mm². 2 In step (3), the volume of DMF added to the PTAA anode buffer layer is 50-70 μL, the volume of the perovskite precursor solution added is 50-80 μL, and the volume of the antisolvent chlorobenzene added is 300-350 μL.

3. The method for fabricating a tin-lead perovskite photodetector based on N'N-carbonyldiimidazole as a passivation layer as described in claim 1, characterized in that: The spin coating speed in step (2) is 3000-4000 rpm and the spin coating time is 30-40 s; the annealing temperature in steps (2) and (3) is 90-110℃ and the annealing time is 15-20 min.

4. The method for fabricating a tin-lead perovskite photodetector based on N'N-carbonyldiimidazole as a passivation layer as described in claim 1, characterized in that: Step (4) involves spin-coating the passivation solution onto the perovskite layer at a rotation speed of 3000-4000 rpm for 30-40 seconds, with an annealing temperature of 90-110℃ and an annealing time of 30-50 seconds.

5. The method for fabricating a tin-lead perovskite photodetector based on N'N-carbonyldiimidazole as a passivation layer as described in claim 1, characterized in that: The vacuum conditions in steps (5) and (6) are 6 × 10⁻⁶. -5 ~9×10 -4 Pa.

6. A tin-lead perovskite photodetector based on N'N-carbonyldiimidazole as a passivation layer, characterized in that: It is prepared by the method described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Detection layer comprising perovskite crystals

    CN107076864A

  • Preparation method of 4-pyridine methylamine bromide optimized tin-lead mixed perovskite solar cell

    CN113437226A