Disordered high current stirring pin for high load and high stability friction stir welding
By designing a high-flow stirring needle with a disordered pattern, the material is promoted to flow randomly during the friction stir welding process, which solves the problem of unstable lap joint structure and realizes a high-load-bearing and high-stability friction stir welding head, thus improving the welding quality.
Patent Information
- Application Number
- CN202311578317.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-24
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-24
AI Technical Summary
In the existing friction stir welding joints, the lap interface structure is unstable during the welding process, making it difficult to achieve high load-bearing capacity and high stability. In particular, the morphological changes of the hook-shaped structure and cold lap have a negative impact on the welding quality, and the joints are sensitive to changes in process parameters.
Design a high-flow stirring pin with and without disorder, comprising an upper part, a middle part, and a lower part of the stirring pin, each part having threaded grooves and symmetrical grooves with opposite rotation directions, to promote relatively disordered flow of materials during welding, avoid the formation of material agglomeration zones, and enhance interfacial mixing and metallurgical bonding.
This method improves the stability and strength of the lap joint morphology during welding, expands the weld nugget width, enhances the load-bearing capacity and overall mechanical properties of the joint, and reduces the impact of the adhesive layer on the weld nugget.
Smart Images

Figure CN117381137B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of friction stir welding technology, specifically relating to a disordered high-current stirring needle for high load-bearing and high-stability friction stir welding. Background Technology
[0002] Friction stir welding (FSW) is a solid-state welding technology with important applications in manufacturing fields such as aerospace, shipbuilding, automotive, and trains. During the welding process, a stirring head, consisting of a shoulder and a stirring pin, generates heat through friction with the materials to be welded, plasticizing the materials and driving their flow and mixing. This, combined with the upsetting action of the shoulder, achieves the joining of the materials. Therefore, the stirring head is the core of friction stir welding technology, and its structural design is a key factor affecting weld quality.
[0003] In traditional friction stir lap welding, a tapered threaded stirring pin is typically used to promote the downward flow of material, thereby achieving the connection of the materials to be welded and avoiding the formation of voids in the weld. During friction stir lap welding, a single-threaded stirring pin inserted into the lower plate causes a large amount of material to flow downward in a "relatively orderly" manner, accumulating at the tip of the stirring pin to form a "material accumulation zone." This "material accumulation zone" compresses the material in the thermodynamically affected zone of the lower plate, causing the lap interface (composed of the lower surface of the upper plate and the upper surface of the lower plate) outside the weld nugget area to bend upward. Simultaneously, during welding, the material within the weld nugget migrates from the advancing side to the retreating side under the action of the shoulder, and then flows from the retreating side to the advancing side, filling the momentary cavity left by the stirring pin. The material filling the momentary cavity flows downward under the action of the shoulder and compresses the lap interface, causing the interface within the weld nugget to form a downwardly bent morphology. Therefore, on the advancing side, the lap interface that bends upwards only outside the weld nugget area is called a hook-like structure; on the retreating side, the lap interface partially existing within the weld nugget exhibits a shape that first bends upwards and extends into the weld nugget before bending downwards, which is called a cold lap. The hook-like structure and cold lap determine the effective lap thickness and effective lap width of the joint. The upward bending of the lap interface and its extension into the weld nugget are not conducive to obtaining a large effective lap thickness and effective lap width, thus making it difficult to obtain a high-load-bearing friction stir lap weld joint. Since changing welding process parameters (rotation speed, welding speed, etc.) cannot alter the bending characteristics of the lap interface, the optimized design based on the geometry of the stirring head is key to improving the lap interface structure and obtaining a high-load-bearing joint.
[0004] CN108838510A relates to a stirring pin with an improved hook-shaped structure for friction stir lap welded joints. It consists of a large-diameter primary stirring pin and a small-diameter secondary stirring pin, which can achieve a hook-shaped structure that is horizontal or even slightly bent downwards.
[0005] CN111906432B discloses a stirring friction lap method based on impact flow, which designs a concave opposing thread stirring needle, causing the hook-shaped structure to bend downward and significantly shortening the cold lap within the weld nugget.
[0006] Although the two patents mentioned above can achieve a downward-curving hook-like structure or significantly shorten the cold overlap length, these two types of stirring heads are very sensitive to changes in process parameters. When used in actual engineering applications, the joint interface morphology is not stable enough.
[0007] Existing reports indicate that the heat input during welding and the location of the "material accumulation zone" have a significant impact on the control of the lap joint interface. However, due to factors such as thickness errors and differences in thermal conductivity of the structures to be welded, it is difficult to ensure consistency in the heat input and the location of the "material accumulation zone" formed by the "relatively ordered" flow during welding in actual engineering. This results in differences in the structural characteristics of the lap joint interface along the weld direction, which in turn affects the stability of the strength of the friction stir lap weld joint along the weld direction. Summary of the Invention
[0008] To address the shortcomings of existing technologies, this invention provides a high-current stirring pin with and without disorder for high-load, high-stability friction stir welding, improving the interface structure inside the lap joint. The stirring pin designed in this invention enhances the intense mixing of materials near the original lap interface without forming a "material agglomeration zone," improving the structural characteristics of the lap interface inside and outside the weld nugget zone. In particular, the straight state of the hook-shaped structure outside the weld nugget zone does not change significantly due to variations in welding process parameters such as rotation speed, welding speed, and pressure, thereby achieving high-strength, high-stability welding.
[0009] A high-current stirring pin with and without disorder is provided for high-load and high-stability friction stir welding. The stirring pin includes an upper part, a middle part, and a lower part, which are connected sequentially. The upper part of the stirring pin has a frustum-shaped structure that is narrow at the top and wide at the bottom, while the lower part has an inverted frustum-shaped structure that is wide at the top and narrow at the bottom. The outer surfaces of both the upper and lower parts of the stirring pin are provided with threaded grooves with opposite directions of rotation. The outer surface of the middle part of the stirring pin is symmetrically provided with grooves of the same inclination angle along the central axis.
[0010] The diameter of the top of the middle part of the stirring needle is the same as that of the bottom of the upper part of the stirring needle, and the diameter of the bottom of the middle part of the stirring needle is the same as that of the top of the lower part of the stirring needle.
[0011] The upper outer surface threaded groove I of the stirring pin has a depth that decreases from deep to shallow and a width that decreases from wide to narrow from top to bottom. The lower outer surface threaded groove II of the stirring pin has a depth that decreases from deep to shallow and a width that decreases from wide to narrow from bottom to top, which can promote the downward and upward flow of materials, respectively.
[0012] The maximum depth of the threaded groove I, threaded groove II, and groove is not less than 0.01 mm, and the pitch is not less than 0.1 mm. The maximum depth and pitch can be adjusted according to the diameter of the stirring needle and other requirements.
[0013] The middle part of the stirring needle is cylindrical, elliptical, or drum-shaped, with the same or different diameters at the top and bottom; the groove on the outer surface of the middle part of the stirring needle can be a straight groove or other symmetrical grooves.
[0014] The length of the stirring needle is determined by the thickness of the first plate and the second plate. The length of the stirring needle is less than the sum of the thicknesses of the first plate and the second plate. The upper part of the stirring needle is less than the sum of the thickness of the first plate and the downward pressure of the shoulder. The middle part of the stirring needle always penetrates the original overlapping interface.
[0015] The first and second plates are made of the same or different materials, such as metals or thermoplastic polymers, and the thickness of the first and second plates is 1-20mm.
[0016] The beneficial effects of this invention are:
[0017] 1. The positive and negative threaded grooves on the disordered high-flow stirring needle proposed in this invention cause the upper and lower plate materials to flow downward and upward respectively during the friction stir lap welding process. They converge near the lap interface and form strong material interaction and mixing, which strengthens the metallurgical bond between the materials near the interface. The converged material flows upward and downward in a reciprocating "relatively disordered" manner under the drive of the symmetrical groove in the middle of the stirring needle, avoiding the formation of a "material agglomeration zone" near the lap interface. This greatly weakens the upward thrust on the material in the thermodynamic affected zone, so that the outer lap interface of the weld nugget is always flat and distributed during long weld welding, and the inner lap interface (cold lap) structure of the weld nugget is complicated, thus achieving high-strength and high-stability welding.
[0018] 2. The parabolic rotating body structure with outward protrusion of disordered strong flow stirring needle designed in this invention can enhance the outward pushing effect on the surrounding material (overlapping interface) after the material converges near the lap interface, expand the weld nugget width, increase the effective lap width of the joint, and further enhance the load-bearing capacity of the joint.
[0019] 3. During friction stir welding, the outward convex profile of the disordered strong flow stirring pin is beneficial for pushing the material near the middle section of the stirring pin (overlapping interface), which can effectively reduce or even prevent the adhesive layer from entering the weld nugget area; the strong reciprocating up and down flow of the stirring pin can expand the dispersion of the discontinuous distribution of adhesive entering the weld nugget, thereby improving the overall mechanical properties of the joint.
[0020] 4. The disordered high-flow stirring needle designed in this invention, during the friction stir lap welding of dissimilar metals, allows the material to flow strongly back and forth near the lap interface, which can increase the degree of fragmentation of intermetallic compounds or make the boundaries of continuously distributed intermetallic compounds more complex, thus increasing the crack propagation path and slowing down the crack propagation speed, thereby helping to improve the joint strength. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of the structure of the stirring needle of the present invention;
[0022] Figure 2 This is a schematic diagram showing the orientation of the threaded groove I, threaded groove II, and groove of the stirring needle of the present invention.
[0023] Figure 3 This is a schematic diagram of material flow during the frictional overlap of the stirring pins in this invention;
[0024] Figure 4 This is a schematic diagram of the shoulder structure in an embodiment of the present invention;
[0025] Figure 5 This is a schematic diagram of the welding process of friction stir lap welding using the stirring head of the stirring needle of the present invention in Embodiment 1 of the present invention.
[0026] Among them, 1. Upper part of stirring needle; 2. Middle part of stirring needle; 3. Lower part of stirring needle; 4. Thread groove I; 5. Groove; 6. Thread groove II; 7. Original overlapping interface; 8. First plate; 9. Second plate; 10. Shoulder end face. Detailed Implementation
[0027] To better explain and facilitate understanding of the present invention, the morphology of the stirring pin and the welding process of the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0028] like Figure 1-4As shown, a high-load, high-stability friction stir welding device with and without disordered high-current stirring pin is presented. The stirring pin includes an upper part 1, a middle part 2, and a lower part 3, which are connected sequentially. The upper part 1 has a frustum-shaped structure that is narrower at the top and wider at the bottom, while the lower part 3 has an inverted frustum-shaped structure that is wider at the top and narrower at the bottom. Both the upper part 1 and the lower part 3 have threaded grooves on their outer surfaces, with opposite directions of rotation. When the outer surface of the upper part 1... When the upper part 1 of the stirring needle has a left-hand thread and the lower part 3 of the stirring needle has a right-hand thread, the stirring head using the stirring needle of the present invention rotates clockwise; when the upper part 1 of the stirring needle has a right-hand thread and the lower part 3 of the stirring needle has a left-hand thread, the stirring head using the stirring needle of the present invention rotates counterclockwise; both of the above methods can make the thread grooves I4 and II6 of the upper part 1 and the lower part 3 of the stirring needle promote the material of the first plate 8 and the second plate 9 to flow towards the middle part 2 of the stirring needle.
[0029] The top of the middle part 2 of the stirring needle has the same diameter as the bottom of the upper part 1 of the stirring needle, and the bottom of the middle part 2 of the stirring needle has the same diameter as the top of the lower part 3 of the stirring needle.
[0030] The outer surface of the middle part 2 of the stirring pin is symmetrically provided with grooves 5 of the same inclination angle along the central axis. The height of the groove 5 in the middle part of the stirring pin along the plate thickness direction is sufficient to ensure that the original lap interface 7 is always penetrated when the shoulder pressing amount fluctuates slightly during the welding process.
[0031] The threaded groove I4 on the outer surface of the upper part 1 of the stirring pin has a depth that decreases from deep to shallow and a width that decreases from wide to narrow from top to bottom. The threaded groove II6 on the outer surface of the lower part 3 of the stirring pin has a depth that decreases from deep to shallow and a width that decreases from wide to narrow from bottom to top, which can promote the downward and upward flow of materials respectively.
[0032] The maximum depth of the threaded groove I4, threaded groove II6, and groove 5 is not less than 0.01mm, and the pitch is not less than 0.1mm. The maximum depth and pitch can be adjusted according to the diameter of the stirring needle and other requirements.
[0033] The middle part 2 of the stirring needle has a cylindrical, elliptical drum-shaped or other structure with the same or different upper and lower diameters.
[0034] The groove 5 on the outer surface of the middle part 2 of the stirring needle can be a straight groove or other symmetrical grooves.
[0035] A shoulder is connected above the upper part 1 of the stirring needle. The ratio of the diameter of the shoulder to the upper diameter of the upper part 1 of the stirring needle is 2:1-10:1. A multi-directional groove is provided on the end face 10 of the shoulder. The number of multi-directional grooves is 0-8, and the rotation angle of the multi-directional grooves is 0-360°. When the rotation angle is 360°, the multi-directional grooves are concentric circles. The multi-directional grooves on the end face 10 of the shoulder are from deep to shallow and from wide to narrow from the outside to the inside of the shoulder.
[0036] The length of the stirring needle is determined by the thickness of the first plate 8 and the second plate 9. The length of the stirring needle is less than the sum of the thicknesses of the first plate 8 and the second plate 9. The upper part 1 of the stirring needle is less than the sum of the thickness of the first plate 8 and the downward pressure of the shoulder. The middle part 2 of the stirring needle always penetrates the original overlapping interface 7.
[0037] The first plate 8 and the second plate 9 are made of the same or different materials, such as metal, thermoplastic polymer, etc. The thickness of the first plate 8 and the second plate 9 is 1-20mm.
[0038] During the welding process, the positive and negative threaded grooves of the upper part 1 and the lower part 3 of the stirring pin cause the materials of the first plate 8 and the second plate 9 to flow downward and upward respectively during the friction stir lap welding process. They converge in the middle part 2 of the stirring pin and form strong material interaction and mixing, which strengthens the metallurgical bond between materials near the interface. The converged material flows upward and downward in a reciprocating "relatively disordered" manner under the drive of the symmetrical groove 5 in the middle part 2 of the stirring pin, avoiding the formation of a "material agglomeration zone" near the lap interface. This greatly weakens the upward thrust on the material in the thermodynamic affected zone, making the outer lap interface of the weld nugget always flat and distributed during long weld welding, and making the inner lap interface (cold lap) structure of the weld nugget more complex, thus achieving high strength and high stability welding. At the same time, the outward convex feature of the stirring pin enhances the outward pushing effect after the material converges near the lap interface, expands the weld nugget width, increases the effective lap width of the joint, and helps to further enhance the load-bearing capacity of the joint.
[0039] When performing friction stir welding, the outward convex shape and positive and negative threads of the stirring pin can more effectively prevent the adhesive layer from entering the weld nugget or weaken the influence of the adhesive inside the weld nugget on its strength.
[0040] The working mechanism of the stirring head using the stirring pin of this invention is as follows: The shoulder end face 10 is provided with multi-directional grooves that decrease in depth and width from the outer side to the inner side of the shoulder, allowing the material to converge more quickly at the root of the stirring pin. During the welding process, the plasticizing material itself is a fluid, and the multi-directional grooves that decrease in depth act as fluid channels. The flow area of the fluid along the channels gradually decreases, and the speed gradually increases, enhancing the "relatively ordered" aggregation effect of the material. Taking the counterclockwise rotation of the stirring pin of this invention with disordered high-flow stirring head as an example, the threaded groove I4 of the upper part 1 of the stirring pin, which decreases in depth and width from wide to narrow, promotes the accelerated downward flow of the material; the threaded groove II6 of the lower part 3 of the stirring pin promotes the accelerated upward flow of the material; and the material in the middle part 2 of the stirring pin flows up and down in a disordered manner under the action of the symmetrical grooves 5.
[0041] like Figure 3As shown, in order to enhance the strong, relatively disordered upward and downward flow mixing of the first plate 8 and the second plate 9 near the original overlap interface 7 without forming a "material agglomeration area", when the stirring head stops sinking after reaching the predetermined sinking depth, the upper part 1 of the stirring needle should be located on the first plate 8, the lower part 3 of the stirring needle should be located on the second plate 9, and the middle part 2 of the stirring needle should just penetrate the original overlap interface 7.
[0042] Example 1
[0043] like Figure 5 As shown, the method for welding thin aluminum alloy plates using the stirring needle of the present invention is as follows:
[0044] Step 1: Clamp the first plate 8 and the second plate 9 to be welded on the tooling of the friction stir welding machine. The first plate 8 and the second plate 9 are the same aluminum alloy with a thickness of 1.5mm and a length of 1000mm.
[0045] Step 2: In this embodiment, the lengths of the upper part 1, the lower part 3, and the middle part 2 of the stirring needle are 0.8mm, 1.0mm, and 0.6mm, respectively; the top diameter of the upper part 1 and the bottom diameter of the lower part 3 are 3mm, and the bottom diameters of the upper part 1, the lower part 3, and the middle part 2 are all 5mm. The upper part 1 has a right-hand thread, the lower part 3 has a left-hand thread, and the groove 5 on the outer surface of the middle part 2 is a straight groove.
[0046] Step 3: Install the stirring needle of the present invention from Step 2 on the shoulder of the shaft. The diameter of the shoulder is 10mm. Install the stirring head of the stirring needle of the present invention on the main shaft of the welding machine. The stirring head rotates counterclockwise at a speed of 800rpm and plunges down to the welding start position at a speed of 2mm / min. When the plunging depth reaches 2.6mm, the center line of the middle part 2 of the stirring needle is exactly located at the original overlapping interface 7 of the first plate 8 and the second plate 9. The stirring head stops plunging down and stays for 1 minute to allow the surrounding material to be fully plasticized.
[0047] Step 4: Weld with the stirring head at a welding speed of 300 mm / min until the end of the weld;
[0048] Step 5: The stirring head is pulled back at the end of the weld, and the entire welding process is completed.
[0049] In this embodiment, thin aluminum alloy plates are used for welding. The gradually changing depth and width of the threaded grooves on the upper part 1 and lower part 3 of the stirring pin enhance the "relatively ordered" downward and upward flow of the first plate 8 and the second plate 9, and enhance the mixing effect of the material gathered in the middle part 2 of the stirring pin. At the same time, due to the thickness error of the structure to be welded, the relative positional relationship between the material accumulation area formed by the "relatively ordered" flow and the lap interface is difficult to control during the welding process, which greatly affects the final interface morphology of the joint. The symmetrical straight groove design in the middle of the stirring pin with disordered strong flow adopted in this embodiment can realize the reciprocating up and down flow of the material, which is equivalent to avoiding the formation of material accumulation area, making the outer interface of the weld nugget have a flat morphology, thereby ensuring the stability of the strength of the friction stir lap weld joint along the weld direction.
[0050] Example 2
[0051] The method for welding dissimilar metals, aluminum alloy and pure copper, using the stirring pin of this invention is as follows:
[0052] Step 1: Clamp the first plate 8 and the second plate 9 to be welded on the tooling of the friction stir welding machine, wherein the first plate 8 and the second plate 9 are 6061-T6 aluminum alloy with a thickness of 3mm and T2 pure copper with a thickness of 3mm, respectively.
[0053] Step 2: In this embodiment, the stirring head with disordered high-flow has an upper part 1 with a length of 2.1 mm, a lower part 3 with a length of 2.1 mm, a middle part with a length of 0.8 mm, a top diameter of the upper part 1 and a bottom diameter of the lower part 3 with a diameter of 3 mm, a bottom diameter of the upper part 1, a top diameter of the lower part 3, a top diameter of the middle part 2, and a bottom diameter of 5 mm. The upper part 1 has a right-hand thread, the lower part 3 has a left-hand thread, and the groove 5 on the outer surface of the middle part 2 is a straight groove.
[0054] Step 3: Install the stirring needle of the present invention from Step 2 on the shoulder of the shaft. The diameter of the shoulder is 13mm. Install the stirring head of the stirring needle of the present invention on the main shaft of the welding machine. The stirring head rotates counterclockwise at a speed of 1200rpm and plunges into the plate to be welded at a speed of 2mm / min at the welding start position. When the stirring needle 4 plunges to a depth of 5.2mm, the center line of the middle part 2 of the stirring needle is located 0.3mm above the original overlapping interface 5. The stirring head stops plunging and stays for 1 minute to allow the surrounding material to be fully plasticized.
[0055] Step 4: Weld with the stirring head at a welding speed of 150 mm / min until the end of the weld;
[0056] Step 5: Complete the welding of dissimilar metals.
[0057] In this embodiment, aluminum alloy and pure copper are used for dissimilar metal welding. During the dissimilar metal friction stir welding process, the high-current stirring needle with and without disorder can make the dissimilar materials at the original overlapping interface 7 flow upward and downward in a reciprocating "relatively disordered" manner under the action of the symmetrical straight groove in the middle 2 of the stirring needle, forming strong material interaction and mixing, strengthening the metallurgical bond between materials near the interface, and dispersing the hard and brittle intermetallic compounds, which is conducive to improving the joint strength.
[0058] Example 3
[0059] The method for using the stirring pin of this invention to perform friction stir composite adhesive welding on thin aluminum alloy plates is as follows:
[0060] Step 1: Clamp the first plate 8 and the second plate 9 to be welded onto the fixture of the friction stir welding machine, wherein the first plate 8 and the second plate 9 are 6061-T6 aluminum alloy with a thickness of 1.5mm.
[0061] Step 2: In this embodiment, the lengths of the upper part 1, the lower part 3, and the middle part 2 of the stirring needle are 1.0mm, 1.0mm, and 0.4mm, respectively; the top diameter of the upper part 1 and the bottom diameter of the lower part 3 are both 3mm, and the bottom diameters of the upper part 1, the lower part 3, the middle part 2, and the middle part 2 are all 5mm. The upper part 1 has a right-hand thread, the lower part 3 has a left-hand thread, and the groove 5 on the outer surface of the middle part 2 is a straight groove.
[0062] Step 3: On the original lap interface 7 of the first plate 8 and the second plate 9, a 6mm wide area is reserved for welding in the direction of the weld seam without applying adhesive, and adhesive is applied evenly to the remaining area.
[0063] Step 4: The stirring head of the stirring needle of the present invention is installed on the main shaft of the welding machine and rotated clockwise at a speed of 800 rpm. It is then driven down to the welding start position at a speed of 2 mm / min. When the driving depth reaches 2.6 mm, the center line of the middle part 2 of the stirring needle is located 0.1 mm above the original overlap interface 7 of the first plate 8 and the second plate 9. The stirring head stops driving down and stays for 1 minute to allow the surrounding material to be fully plasticized.
[0064] Step 5: Weld with the stirring head at a welding speed of 300 mm / min until the end of the weld;
[0065] Step Six: The stirring head is pulled back at the end of the weld, and the entire welding process is completed.
[0066] In this embodiment, thin aluminum alloy is used for friction stir composite adhesive welding. The outer contour of the disordered high-current stirring needle of the present invention is convex, which can enhance the outward pushing effect on the surrounding material (overlapping interface) after the material gathers near the overlap interface, expand the weld nugget width, significantly reduce or even effectively prevent the adhesive from entering the weld nugget area, and ensure that the adhesive effectively fills the overlap interface outside the weld nugget, which is beneficial to improving the overall mechanical properties of the joint.
Claims
1. A high-current stirring pin with or without disorder for high-load, high-stability friction stir welding, characterized in that, It includes an upper part (1), a middle part (2), and a lower part (3) of a stirring needle, which are connected in sequence. The upper part (1) of the stirring needle is a frustum-shaped structure that is narrow at the top and wide at the bottom, and the lower part (3) of the stirring needle is an inverted frustum-shaped structure that is wide at the top and narrow at the bottom. The top of the middle part (2) of the stirring needle has the same diameter as the bottom of the upper part (1), and the bottom of the middle part (2) of the stirring needle has the same diameter as the top of the lower part (3). The outer surface of the upper part (1) and the outer surface of the lower part (3) of the stirring needle are both provided with threaded grooves, and the rotation direction of the threaded grooves is opposite. The outer surface of the middle part (2) of the stirring needle is symmetrically provided with grooves (5) with the same inclination angle along the central axis. The middle part (2) of the stirring needle is cylindrical or elliptical long drum-shaped, and the groove (5) on the outer surface of the middle part (2) of the stirring needle is a straight groove; The upper part (1) of the stirring needle has a threaded groove I (4) on the outer surface that is deeper and narrower from top to bottom, and the lower part (3) of the stirring needle has a threaded groove II (6) on the outer surface that is deeper and narrower from bottom to top. The middle part of the stirring needle (2) always penetrates the original overlapping interface (7); During the friction stir lap welding process, the positive and negative thread grooves of the upper part (1) and lower part (3) of the stirring needle cause the materials of the first plate (8) and the second plate (9) to flow downward and upward respectively, and converge in the middle part (2) of the stirring needle.
2. The high-current stirring pin with and without disorder for high-load, high-stability friction stir welding according to claim 1, characterized in that, The maximum depth of the threaded groove I (4) and threaded groove II (6) is not less than 0.01 mm, and the pitch is not less than 0.1 mm. The maximum depth and pitch are adjusted according to the diameter of the stirring needle and the requirements.
3. The high-current stirring pin with and without disorder for high-load, high-stability friction stir welding according to claim 1, characterized in that, The maximum depth of the groove (5) is not less than 0.01 mm and the pitch is not less than 0.1 mm. The maximum depth and pitch are adjusted according to the diameter of the stirring needle and the requirements.
4. The high-current stirring pin with and without disorder for high-load, high-stability friction stir welding according to claim 1, characterized in that, The length of the stirring needle is determined by the thickness of the first plate (8) and the second plate (9). The length of the stirring needle is less than the sum of the thicknesses of the first plate (8) and the second plate (9). The length of the upper part (1) of the stirring needle is less than the sum of the thickness of the first plate (8) and the downward pressure of the shoulder.
5. The high-current stirring pin with and without disorder for high-load, high-stability friction stir welding according to claim 4, characterized in that, The first plate (8) and the second plate (9) are made of the same or different materials, such as metal or thermoplastic polymer, and the thickness of the first plate (8) and the second plate (9) is 1-20 mm.
Citation Information
Patent Citations
Welding device and method for improving hook-shaped defects of friction stir welding overlap joint
CN108838510A
A stirring friction lap method based on impinging flow
CN111906432B
Friction stir welding stirring head capable of improving material flow behavior
CN110640296A
Stirring friction overlapping method based on impinging stream
CN111906432A
Non-dip-angle non-thinning friction stir welding tool and welding equipment
CN216264016U