A two-component room temperature curing epoxy adhesive, its method of preparation and use
By designing a two-component room-temperature curing epoxy adhesive, the problems of nozzle clogging and low preform strength in adhesive jet printing technology are solved, achieving stability in the printing process and high preform strength, and making it suitable for a variety of powder materials.
Patent Information
- Application Number
- CN202311491524.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-09
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-09
AI Technical Summary
Existing adhesive jet printing technologies suffer from limitations in the types of adhesives available, easy nozzle clogging, low print strength, and susceptibility to damage. Solvent-based adhesives also lead to nozzle instability and wear and tear.
A two-component room-temperature curing epoxy adhesive is used, including adhesive component A and component B. Component A is epoxy resin, and component B is room-temperature curing agent, solvent, humectant and surfactant, which are used for mixing powder and spraying respectively. This avoids the adhesive being sprayed directly from the nozzle, solves the nozzle clogging problem through room-temperature curing and improves the strength of the raw blank.
It solves the problem of nozzle clogging, improves printing stability and preform strength, reduces nozzle wear rate, is suitable for various powder systems, and broadens the application range of binders.
Smart Images

Figure CN117384576B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of additive manufacturing technology, specifically relating to a two-component room-temperature curing epoxy adhesive, its preparation method, and its uses. Background Technology
[0002] Binder jetting (BJ), also known as 3D printing, is an additive manufacturing technology based on powder bed technology. This technology uses an inkjet printhead to jet binder onto a layered powder bed. The bonding between the powder particles creates a 3D part preform. Subsequently, the preform undergoes debinding and sintering to obtain a dense part with good mechanical properties. Thanks to its high printing speed and low cost, binder jetting is one of the technologies most likely to be industrialized.
[0003] Materials used in binder jet printing consist of two main parts: powder laid in the powder tank and binder ejected from the printhead. Powder materials include metals, ceramics, and polymers. Binders are broadly classified into inorganic and organic binders. Organic binders are mainly polymer materials, including phenolic binders, furan binders, polyvinyl alcohol, polyethylene glycol, and polyurethane. Inorganic binders are binders with an inorganic matrix, and their adhesive strength primarily comes from the curing of the inorganic base. Currently, the more mature inorganic binders include silicate, phosphate, sulfate, and precursor inorganic binders.
[0004] In existing adhesive jet printing technology, since the adhesive needs to be ejected from the print head, there are at least the following problems during use: (1) Due to the stringent requirements of the print head on the performance of the adhesive, including low viscosity and low solvent polarity, there are fewer types of adhesives that can meet the printing requirements, and the selection of adhesives is limited; (2) Taking the commonly used epoxy resin adhesive as an example, epoxy resin adhesive is usually solvent-based. In order to reduce the viscosity of the system to meet the viscosity requirements of the print head, the adhesive needs to contain a large amount of solvent, which results in a low content of epoxy resin component in the adhesive, that is, a low content of effective adhesive component. This leads to a reduction in the content of epoxy resin acting on the powder system, which cannot effectively bond the powder system. Therefore, the strength of the printed three-dimensional blank is usually not high. The low strength of the three-dimensional blank makes it easy to damage the three-dimensional blank during the subsequent residual powder cleaning process. On the other hand, after printing, the printed parts need to be heat-cured, and the three-dimensional blank is easy to be damaged during the transfer process. (3) Since the adhesive is sprayed directly from the print head, for solvent-based adhesives, such as epoxy resin adhesives, the viscosity of the adhesive system increases due to solvent evaporation or curing of the effective components of epoxy resin, which may cause the print head to be easily clogged, the working state to be unstable and the wear and tear during the printing process.
[0005] Therefore, it is of great significance to study a new type of adhesive suitable for adhesive jet printing technology to effectively solve the above problems. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a two-component room-temperature curing epoxy adhesive, its preparation method, and its applications, which can effectively solve the above-mentioned problems.
[0007] The technical solution adopted in this invention is as follows:
[0008] This invention provides a two-component room-temperature curing epoxy adhesive, comprising adhesive component A and adhesive component B; adhesive component A is used to mix with a base powder to obtain a mixed powder, which is then placed in a powder tank for use; adhesive component B is used to be directly sprayed from a printhead into the powder tank to mix the powder and ink bed; wherein, adhesive component A is epoxy resin; and adhesive component B includes a room-temperature curing agent, a solvent, a humectant, and a surfactant.
[0009] Preferably, the weight ratio of each component in adhesive component A and adhesive component B is as follows:
[0010]
[0011]
[0012] Preferably, the epoxy resin is a bisphenol A type epoxy powder with a particle size of 5µm-50µm.
[0013] Preferably, the room-temperature curing agent is one or a mixture of several of aliphatic polyamines, alicyclic polyamines, low-molecular-weight polyamides, and modified aromatic amines.
[0014] Preferably, the solvent is one or a mixture of ethanol, ethyl acetate and glycerol.
[0015] Preferably, the humectant is one or a mixture of several of glycerol, propylene glycol, and diethylene glycol.
[0016] Preferably, the surfactant is one or a mixture of several of the following: sodium oleate, octadecylamine, sodium laurylate, cocoylamine, sodium stearate, AES, sodium dodecyl sulfate, dodecylamine, and sodium dodecylbenzene sulfonate.
[0017] Preferably, the base powder in the powder cylinder includes metal material powder, ceramic powder, and polymer powder.
[0018] This invention also provides a method for preparing a two-component room-temperature curing epoxy adhesive, comprising the following steps:
[0019] Weigh out the amount of adhesive component A specified in the formula to obtain adhesive component A;
[0020] The preparation method of the adhesive component B is as follows: weigh the room temperature curing agent, solvent, humectant and surfactant according to the formula, and stir the room temperature curing agent, solvent, humectant and surfactant thoroughly until they are mixed evenly to prepare the adhesive component B.
[0021] This invention also provides an application of a two-component room-temperature curing epoxy adhesive, wherein the two-component room-temperature curing epoxy adhesive is used in an adhesive jet printing equipment, specifically comprising:
[0022] Step S1: Mix the binder component A and the base powder thoroughly and evenly to obtain a mixed powder, and then place the mixed powder into the powder cylinder of the jet printing system.
[0023] Step S2: Apply binder component B into the print head of the jet printing system; the print head sprays binder component B onto the surface of the mixed powder according to the design parameters. The binder component B and the binder component A in the mixed powder interact to form a binder, which effectively bonds the base powder in the mixed powder. The raw blank is prepared by printing layer by layer through binder jet printing technology.
[0024] The present invention provides a two-component room-temperature curing epoxy adhesive, its preparation method and uses have the following advantages:
[0025] (1) It solves the problem of easy nozzle clogging, reduces nozzle wear rate, and ensures the stability of the printing process; (2) The system binder is not limited by nozzle viscosity, and the content of effective epoxy components in the system can be adjusted, which can improve the strength of the green blank and reduce the risk of damage to the green blank during transfer or residual powder cleaning; (3) It is applicable to various ceramic powder, metal powder and polymer powder systems, and has a wide range of applications. Attached Figure Description
[0026] Figure 1 This is a schematic diagram illustrating the application principle of the two-component room-temperature curing epoxy adhesive provided by the present invention. Detailed Implementation
[0027] The following embodiments are merely preferred technical solutions of the present invention and are not intended to limit the present invention in any way. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
[0028] This invention provides a two-component room-temperature curing epoxy adhesive, its preparation method, and its applications, offering the following advantages: 1. It broadens the types of adhesives applicable to adhesive jet printing processes. The two-component room-temperature curing epoxy adhesive is suitable for various ceramic powders, metal powders, and polymer powder systems, possessing wide applicability. 2. Through the AB two-component configuration, the adhesive system is not limited by printhead viscosity, and the effective epoxy component content is adjustable, improving the strength of the green body. 3. The AB two-component design separates the epoxy resin and the room-temperature curing agent, preventing the adhesive from curing due to prolonged storage during printing or storage, thus solving the problem of printhead clogging and reducing printhead wear rate.
[0029] Specifically, the present invention provides a two-component room-temperature curing epoxy adhesive, comprising adhesive component A and adhesive component B; adhesive component A is used to mix with a base powder to obtain a mixed powder, which is then placed in a powder cylinder for use; adhesive component B is used to be directly sprayed from the printhead into the powder cylinder to mix the powder bed; wherein, adhesive component A is epoxy resin; and adhesive component B includes a room-temperature curing agent, a solvent, a humectant, and a surfactant.
[0030] The weight ratio of each component in adhesive component A and adhesive component B is as follows:
[0031]
[0032] In this invention, the epoxy resin is a bisphenol A type epoxy powder with a particle size of 5µm-50µm.
[0033] The room-temperature curing agent is one or a mixture of several of aliphatic polyamines, alicyclic polyamines, low-molecular-weight polyamides, and modified aromatic amines.
[0034] The solvent is one or a mixture of ethanol, ethyl acetate, and glycerol. For example, the solvent may include 90 parts by weight of ethanol, 10 parts by weight of ethyl acetate, and 3 parts by weight of glycerol.
[0035] The humectant is one or a mixture of several of glycerol, propylene glycol, and diethylene glycol. The surfactant is one or a mixture of several of sodium oleate, octadecylamine, sodium laurylate, cocoylamine, sodium stearate, AES, sodium lauryl sulfate, dodecylamine, and sodium dodecylbenzene sulfonate.
[0036] The base powder in the powder cylinder includes metal material powder, ceramic powder, and polymer powder.
[0037] This invention also provides a method for preparing a two-component room-temperature curing epoxy adhesive, comprising the following steps:
[0038] Weigh out the amount of adhesive component A specified in the formula to obtain adhesive component A;
[0039] The preparation method of the adhesive component B is as follows: weigh the room temperature curing agent, solvent, humectant and surfactant according to the formula, and stir the room temperature curing agent, solvent, humectant and surfactant thoroughly until they are mixed evenly to prepare the adhesive component B.
[0040] This invention also provides an application of a two-component room-temperature curing epoxy adhesive, wherein the two-component room-temperature curing epoxy adhesive is used in an adhesive jet printing equipment, specifically comprising:
[0041] Step S1: Mix the binder component A and the base powder thoroughly and evenly to obtain a mixed powder, and then place the mixed powder into the powder cylinder of the jet printing system.
[0042] Step S2: Apply binder component B into the print head of the jet printing system; the print head sprays binder component B onto the surface of the mixed powder according to the design parameters. The binder component B and the binder component A in the mixed powder interact to form a binder, which effectively bonds the base powder in the mixed powder. The raw blank is prepared by printing layer by layer through binder jet printing technology.
[0043] The two-component room-temperature curing epoxy adhesive, its preparation method and application provided by the present invention have the following advantages through the AB two-component configuration: (1) It solves the problem of easy nozzle clogging, reduces the nozzle loss rate and ensures the stability of the printing process; (2) The adhesive system is not limited by the nozzle viscosity, and the content of effective epoxy components in the system can be adjusted, which can improve the strength of the green blank and reduce the risk of damage to the green blank during transfer or residual powder cleaning; (3) It can be applied to various ceramic powder, metal powder and polymer powder systems, and has a wide range of applications.
[0044] The advantages of this invention compared to traditional solutions are verified through the following examples:
[0045] Experimental example:
[0046] In this experimental example, the base powder was ceramic powder, specifically silicon carbide powder with a particle size of 45 μm. The binder component A used was Nan Ya E20 epoxy resin with a particle size of 50 μm.
[0047] Step S1, Preparation of mixed powder:
[0048] 9000g of silicon carbide powder and 200g of epoxy resin (i.e. binder component A) were placed in a rotary mixer. The speed was set to 150r / min, with forward rotation for 5min, reverse rotation for 5min, and intermittent rotation for 5min. The time was set to 30min to obtain a uniformly mixed powder, which was denoted as mixed powder B2.
[0049] Step S2, Preparation of adhesive component B:
[0050] Add 10g of room temperature curing agent divinyltriamine, 90g of solvent ethanol, 10g of solvent ethyl acetate, 3g of humectant glycerol, and 0.5g of surfactant sodium dodecyl sulfate to a 100ml beaker equipped with a mechanical stirrer. Set the stirring speed to 150r / min and stir for 5min until homogeneous to prepare adhesive component B.
[0051] Step S3, Printing process:
[0052] Mixed powder B2 containing binder component A and binder component B were applied to the powder cylinder and the print head, respectively. The printing parameters were optimized, and a 36mm*4mm*3mm sample strip was obtained by inkjet printing with binder. The printed blank was placed at room temperature for 24 hours to obtain the printed blank, which was denoted as printed blank S2.
[0053] Example for comparison:
[0054] In this comparative example, the base powder was the same as in the experimental example, using silicon carbide powder with a particle size of 45 μm. The epoxy resin used as the binder was the same as in the experimental example, using Nanya E20 with a particle size of 50 μm.
[0055] Step S1, Preparation of conventional epoxy adhesive:
[0056] 10g of Nanya E20 epoxy resin with a particle size of 50um and 10g of ethyl acetate were added to a 500ml beaker equipped with a mechanical stirrer and stirred until a clear and homogeneous solution was obtained. Then, 1g of polyetheramine, 90g of ethanol, 3g of glycerol and 0.5g of sodium dodecyl sulfate were added in sequence. The stirring speed was set to 150r / min and stirred for 5min until homogeneous. The resulting epoxy binder was denoted as epoxy binder E1.
[0057] Step S2, Printing process:
[0058] Silicon carbide powder and epoxy binder E1 were applied to the powder cylinder and the print head, respectively. The printing parameters were optimized, and a 36mm*4mm*3mm sample strip was obtained by inkjet printing with the binder. The printed blank was placed in an oven and heated at 150℃ for 2 hours to obtain the printed blank, which was denoted as printed blank S1.
[0059] For both experimental and control cases, the following tests were performed:
[0060] (1) Performance testing of powder:
[0061] According to GB / T 1482-1984 standard, the bulk density and Hall flow rate of the 45µm silicon carbide powder in the control example were tested, as well as the bulk density and Hall flow rate of the mixed powder B2 in the test example of this invention were tested. The results are shown in Table 1:
[0062] Table 1 Comparison of Powder Performance
[0063] project Bulk density (g / cm3) Hall flow rate (s) Silicon carbide powder (control example) 1.43 92 Mixed powder B2 (experimental example) 1.42 -
[0064] As can be seen from Table 1, the mixed powder B2 used in this invention, when laid in the powder cylinder, has a similar bulk density to the silicon carbide powder used in conventional solutions, thus meeting the printing requirements of the powder cylinder during printing. Furthermore, when binder component A is added to the silicon carbide powder to obtain mixed powder B2, its flowability decreases, which is beneficial for the powder spreading process of the binder spraying system.
[0065] (2) Performance testing of binder components:
[0066] The viscosity, surface tension, and density of epoxy adhesive E1 in the control example and adhesive component B in the experimental example were tested at room temperature, and the Z-value was calculated. The formula for calculating the Z-value is as follows:
[0067]
[0068] in:
[0069] γ is the surface tension of the binder; ρ is the density of the binder; μ is the viscosity of the binder. L is the nozzle diameter.
[0070] A printhead with a nozzle diameter L of 20µm was selected for printing effect testing. Generally, a Z value between 1 and 10 indicates that the prepared adhesive meets the printhead requirements of the printer.
[0071] The calculation results of the Z value are shown in Table 2.
[0072] Table 2 Comparison of Adhesive Component Properties
[0073]
[0074]
[0075] As shown in Table 2, the Z-values of adhesive component B used in this invention and epoxy adhesive E1 used in conventional solutions are both between 1 and 10, thus both meet the printhead requirements of printers. Furthermore, the viscosity of adhesive component B used in this invention is significantly lower than that of epoxy adhesive E1 used in conventional solutions; therefore, adhesive component B used in this invention is less likely to clog the printhead.
[0076] (3) Testing of the bending strength of the printed blank:
[0077] The specific curing parameters of the printed blank S1 obtained from the control example and the printed blank S2 obtained from the experimental example are shown in Table 3.
[0078] The compression speed was set to 0.5 mm / min. Three-point bending tests were performed on the printed blank S1 obtained from the control example and the printed blank S2 obtained from the experimental example to obtain the bending strength F1. The results are shown in Table 3.
[0079] Table 3 Comparison of Curing Parameters and Bending Strength of Printed Preforms
[0080]
[0081] As shown in Table 3, traditional epoxy adhesive E1 requires 2 hours of heating at 150°C to cure when used in printing. This process necessitates transferring the sample to an oven, which carries the risk of damaging the preform. In contrast, the AB components of this invention only require 24 hours of room temperature curing when used in printing. Therefore, sample transfer is unnecessary, reducing the risk of preform damage.
[0082] Furthermore, as can be seen from Table 3, the flexural strength of the printed blank S2 obtained in the experimental example of the present invention is significantly higher than that of the printed blank S1 obtained in the control example. Therefore, the method of the present invention can improve the strength of the blank.
[0083] Compared with the prior art, the present invention has the following advantages:
[0084] (1) It solves the problem of easy nozzle clogging, reduces nozzle wear rate, and ensures the stability of the printing process; (2) The system binder is not limited by nozzle viscosity, and the content of effective epoxy components in the system can be adjusted, which can improve the strength of the green blank and reduce the risk of damage to the green blank during transfer or residual powder cleaning; (3) It is applicable to various ceramic powder, metal powder and polymer powder systems, and has a wide range of applications.
[0085] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a two-component room-temperature curing epoxy adhesive, characterized in that, It includes binder component A and binder component B; binder component A is used to mix with base powder to obtain mixed powder, which is then placed in a powder cylinder for use; binder component B is used to be sprayed directly from the printhead into the powder cylinder to mix the powder bed; wherein, binder component A is epoxy resin; binder component B includes a room temperature curing agent, solvent, humectant, and surfactant; The weight ratio of each component in adhesive component A and adhesive component B is as follows: 2-30 parts by weight of epoxy resin 5-20 parts by weight of room temperature curing agent 100 parts by weight of solvent 5 parts by weight of moisturizer Surfactant 0.5 parts by weight; The preparation method includes the following steps: Weigh out the amount of adhesive component A specified in the formula to obtain adhesive component A; The preparation method of the adhesive component B is as follows: weigh the room temperature curing agent, solvent, humectant and surfactant according to the formula, stir the room temperature curing agent, solvent, humectant and surfactant thoroughly until they are mixed evenly, and prepare the adhesive component B; The two-component room-temperature curing epoxy adhesive is used in adhesive jet printing equipment, specifically including: Step S1: Mix the binder component A and the base powder thoroughly and evenly to obtain a mixed powder, and then place the mixed powder into the powder cylinder of the jet printing system. Step S2: Apply binder component B into the print head of the jet printing system; the print head sprays binder component B onto the surface of the mixed powder according to the design parameters. The binder component B and the binder component A in the mixed powder interact to form a binder, which effectively bonds the base powder in the mixed powder. The raw blank is prepared by printing layer by layer through binder jet printing technology.
2. The preparation method of a two-component room-temperature curing epoxy adhesive according to claim 1, characterized in that, The epoxy resin is a bisphenol A type epoxy powder with a particle size of 5um-50um.
3. The method for preparing a two-component room-temperature curing epoxy adhesive according to claim 1, characterized in that, The room-temperature curing agent is one or a mixture of several of aliphatic polyamines, alicyclic polyamines, low-molecular-weight polyamides, and modified aromatic amines.
4. The preparation method of a two-component room-temperature curing epoxy adhesive according to claim 1, characterized in that, The solvent is one or a mixture of ethanol, ethyl acetate and glycerol.
5. The method for preparing a two-component room-temperature curing epoxy adhesive according to claim 1, characterized in that, The humectant is one or a mixture of several of glycerol, propylene glycol, and diethylene glycol.
6. The method for preparing a two-component room-temperature curing epoxy adhesive according to claim 1, characterized in that, The surfactant is one or a mixture of several of the following: sodium oleate, octadecylamine, sodium laurylate, cocoylamine, sodium stearate, AES, sodium dodecyl sulfate, dodecylamine, and sodium dodecylbenzene sulfonate.
7. The method for preparing a two-component room-temperature curing epoxy adhesive according to claim 1, characterized in that, The base powder in the powder cylinder includes metal material powder, ceramic powder, and polymer powder.
Citation Information
Patent Citations
Three-dimensional printing forming material with toughness and high adhesive property and preparation method thereof