A FeTe 1.5 / FeTe2@C composite microwave absorbing material and its preparation method
Patent Information
- Application Number
- CN202311330109.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-13
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-10-13
AI Technical Summary
[0004]针对现有技术能有效提高过渡金属碲化物吸波材料电磁衰减不足以及反射损耗低、匹配厚度厚和吸波频带窄的问题,本发明提供了一种一维棒状结构的FeTe1.5/FeTe2@C复合吸波材料的制备方法,制备流程简单,易操控且生产成本低,制得的FeTe1.5/FeTe2@C复合吸波材料具有强吸收、匹配厚度薄、有效吸收带宽较宽的特点
Smart Images

Figure CN117384595B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of microwave absorbing materials technology, specifically to a FeTe... 1.5 / FeTe2@C composite microwave absorbing material and its preparation method. Background Technology
[0002] The rapid development of communication equipment, electronic equipment, and high-precision equipment has led to harmful electromagnetic wave (EMW) pollution, a new type of pollution source that poses a serious threat to human health, sensitive military applications, and commercial applications, attracting increasing attention. Therefore, this issue has spurred an urgent pursuit of electromagnetic wave absorbing materials. The development of high-performance absorbing materials with strong absorption, wide absorption bandwidth, and low matching thickness has become a goal.
[0003] Transition metal tellurides, as compounds with unique physicochemical properties such as interfacial superconductivity and topological quantum states, have attracted widespread attention. Tellurides are relatively diverse, including bismuth telluride, cadmium telluride, and cobalt telluride. They possess excellent pyroelectric and photoelectric response characteristics and are widely used in various aspects of life. The unique electron transport properties and morphological diversity of metal tellurides have made them candidates for electromagnetic wave absorbing materials. The unique morphology and size also have a crucial impact on electromagnetic wave absorbing materials, such as 0D (nanoparticles), 1D (nanowires, nanorods), 2D (sheets), and 3D (spheres). Among them, one-dimensional materials have attracted researchers' attention due to their anisotropic structure and modifiability. One-dimensional materials with a high aspect ratio can form an axial carrier channel to promote electron hopping and migration, establishing an effective conductive network. Due to its special crystal structure, one-dimensional rod-shaped FeTe exhibits unique anisotropy and special electron transport properties. x It has the potential to become an electromagnetic wave absorbing material. However, due to the disadvantages of traditional tellurides, such as poor impedance matching, high density, high filler loading, and large matching thickness, it is difficult for most of these materials to achieve strong absorption performance while also being lightweight, thin, and having a wide absorption bandwidth. Summary of the Invention
[0004] To address the shortcomings of existing technologies in effectively improving the electromagnetic attenuation of transition metal telluride absorbing materials, as well as their low reflection loss, thick matching thickness, and narrow absorption bandwidth, this invention provides a one-dimensional rod-shaped FeTe structure. 1.5 The preparation method of FeTe2@C composite microwave absorbing material is simple, easy to control, and has low production cost. The obtained FeTe2@C composite microwave absorbing material has a simple preparation process, is easy to control, and has low production cost. 1.5 / FeTe2@C composite absorbing materials have the characteristics of strong absorption, thin matching thickness, and wide effective absorption bandwidth.
[0005] To achieve the above objectives, the present invention provides the following technical solution: a FeTe 1.5 The preparation method of / FeTe2@C composite microwave absorbing material includes the following steps:
[0006] S1. Dissolve fumaric acid in distilled water, then add ferric nitrate nonahydrate, and continue stirring to obtain an orange suspension;
[0007] S2. The mixed solution is transferred to a reactor for hydrothermal reaction. After the reaction is completed, the mixture is cooled with the furnace, then filtered, washed and dried to obtain MIL-88A.
[0008] S3. Add MIL-88A and dopamine hydrochloride (PDA) to an isopropanol solution, then add ammonia water under rapid stirring. After stirring at room temperature, filter, wash and dry to obtain the MIL-88A@PDA precursor.
[0009] S4. After uniformly mixing MIL-88A@PDA with tellurium powder, place the mixture in a tube furnace and calcine it under inert gas protection. Cool the mixture with the furnace to obtain FeTe. 1.5 / FeTe2@C composite material.
[0010] Preferably, in step S1, the molar ratio of fumaric acid and ferric nitrate nonahydrate is 0.9:(1-1.2).
[0011] Preferably, in step S1, the stirring speed is 400-600 rpm and the reaction time is 8-10 min.
[0012] Preferably, in step S2, the heating rate is 5-8°C / min and the reaction time is 5-6h.
[0013] Preferably, in step S2, the drying temperature is 60-80°C and the drying time is 12-14 hours.
[0014] Preferably, in step S3, the mass ratio of MIL-88A to dopamine hydrochloride is 1:(0.5~1).
[0015] Preferably, in step S3, the stirring speed is 400-600 rpm and the reaction time is 10-12 h.
[0016] Preferably, in step S4, the mass ratio of MIL-88A@PDA to tellurium powder is 1:(1-3).
[0017] Preferably, in step S4, the inert gas includes argon, the heating rate is 2-5℃ / min, the calcination temperature is 600-800℃, and the calcination time is 3-4h.
[0018] This invention provides a FeTe based on the above1.5 / Preparation method of FeTe2@C composite microwave absorbing material 1.5 / FeTe2@C composite microwave absorbing material.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0020] 1. This invention first prepared MIL-88A nanomaterials using fumaric acid and ferric nitrate nonahydrate as raw materials, isopropanol as solvent, and ammonia water as auxiliary hydrothermal treatment. PDA was then introduced to prepare the MIL-88@PDA precursor. Subsequently, tellurization treatment was used to prepare FeTe nanomaterials with a rod-shaped polyhedral core-shell structure. 1.5 The / FeTe2@C composite microwave absorbing material of this invention has a simple preparation process, unique morphology, low cost, and can be repeatedly operated.
[0021] 2. This invention prepares FeTe with a rod-shaped polyhedral core-shell structure via hydrothermal fermentation and tellurization. 1.5 / FeTe2@C material can effectively improve the effective absorption bandwidth and reflection loss intensity of the material, reduce the material matching thickness, and has certain development prospects. The prepared absorbing material has a rod-shaped polyhedral core-shell structure, with abundant heterogeneous interfaces, thin matching thickness, and wide bandwidth. When the matching thickness is 1.50 mm, the filling amount is 20%, and the frequency is 16.64 GHz, the minimum radiation loss (RL) is... min The effective absorption bandwidth (EAB) is -47.60 dB, and the effective absorption bandwidth (EAB) is 3.76 GHz (14.24-18.00 GHz). In addition, the EAB value reaches 4.64 GHz (13.36-18.00 GHz) at a frequency of 15.52 GHz, making it a microwave absorbing material with strong absorption and wide bandwidth. Attached Figure Description
[0022] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the embodiments of the invention to explain the invention and do not constitute a limitation thereof.
[0023] In the attached diagram:
[0024] Figure 1 MIL-88A and FeTe prepared in Example 2 of this invention 1.5 X-ray diffraction pattern of FeTe2@C composite microwave absorbing material;
[0025] Figure 2 The MIL-88A, MIL-88@PDA precursor, and FeTe prepared in Example 2 of this invention are 1.5 Scanning electron microscope image of FeTe2@C microwave absorbing material;
[0026] Figure 3 This is a reflection loss curve of the FTC-1 absorbing material prepared in Example 1 of the present invention with a thickness of 1.0 to 5.5 mm;
[0027] Figure 4 This is a reflection loss curve of the FTC-2 absorbing material prepared in Example 2 of the present invention with a thickness of 1.0 to 5.5 mm;
[0028] Figure 5 This is a reflection loss curve of the FTC-3 absorbing material prepared in Example 3 of the present invention with a thickness of 1.0 to 5.5 mm. Detailed Implementation
[0029] The preferred embodiments of the present invention will be described below with reference to the accompanying drawings. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.
[0030] This invention provides a FeTe 1.5 The preparation method of / FeTe2@C composite microwave absorbing material includes the following steps:
[0031] S1. Fumaric acid was dissolved in distilled water, and then ferric nitrate nonahydrate was added. The mixture was stirred continuously. The molar ratio of fumaric acid to ferric nitrate nonahydrate was 0.9:(1-1.2). An orange suspension was obtained. The stirring speed was 400-600 rpm and the reaction time was 8-10 min.
[0032] S2. The mixed solution is transferred to a reactor for hydrothermal reaction. The heating rate in the reactor is 5-8℃ / min, the reaction time is 5-6h, and after the reaction is completed, the solution is cooled with the furnace, then filtered, washed, and dried. The drying temperature is 60-80℃ and the time is 12-14h to obtain MIL-88A.
[0033] S3. Add MIL-88A and dopamine hydrochloride (PDA) to an isopropanol solution, with a mass ratio of MIL-88A to dopamine hydrochloride of 1:(0.5-1). Then, add ammonia water under rapid stirring at a speed of 400-600 rpm for 10-12 h. After stirring at room temperature, filter, wash, and dry to obtain the MIL-88A@PDA precursor.
[0034] S4. After uniformly mixing MIL-88A@PDA and tellurium powder, with a mass ratio of MIL-88A@PDA to tellurium powder of 1:(1-3), the mixture is placed in a tube furnace and calcined under inert gas protection, with furnace cooling. The inert gas is argon. The heating rate is 2-5℃ / min, the calcination temperature is 600-800℃, and the calcination time is 3-4 hours to obtain FeTe. 1.5 / FeTe2@C composite material.
[0035] The present invention also provides a FeTe based on the above. 1.5 / Preparation method of FeTe2@C composite microwave absorbing material 1.5 / FeTe2@C composite absorbing materials can effectively improve the effective absorption bandwidth and reflection loss intensity of materials, reduce the material matching thickness, and have certain development prospects. The absorbing materials prepared have a rod-shaped polyhedral core-shell structure, with abundant heterogeneous interfaces, thin matching thickness and wide bandwidth.
[0036] Example 1
[0037] A one-dimensional rod-shaped FeTe 1.5 The preparation method of FeTe2@C composite microwave absorbing material includes the following steps:
[0038] (1) 3.6 mmol of C4H4O4 was dissolved in 50 mL of deionized water. The solution was stirred at 70 °C for 10 min, and then 4 mmol of Fe(NO3)2·9H2O was added and stirred for another 10 min to obtain an orange suspension. Then, the mixed solution was transferred to a reaction vessel and placed in an electric heating drying oven. The temperature was increased to 120 °C at a rate of 6 °C / min and kept at this temperature for 6 h. After the reaction was completed, the mixture was cooled to room temperature. The reaction product was washed three times with anhydrous ethanol and distilled water alternately. After filtration, a black solid product was obtained. After drying at 80 °C for 12 h, MIL-88A nanomaterials were obtained.
[0039] (2) Dissolve 0.2g of MIL-88A in 100mL of isopropanol, stir rapidly at 800 rpm and add 0.1g of PDA, continue stirring to obtain an orange suspension. Then, add 1mL of NH3·H2O to the above reaction solution, and immediately form a brownish-gray solution. After stirring for 12h, wash the reaction product three times with anhydrous ethanol and distilled water alternately. After filtration, a brownish-black product is obtained. After drying at 80℃ for 12h, the MIL-88A@PDA precursor is obtained.
[0040] (3) After uniformly mixing 200 mg MIL-88A@PDA and 600 mg Te powder, the mixture was placed in a tube furnace and heated to 650 °C at a rate of 3 °C / min under argon protection. The mixture was calcined for 3 h and then cooled in the furnace to obtain FeTe. 1.5 / FeTe2@C composite microwave absorbing material, denoted as FTC-1.
[0041] Example 2
[0042] A one-dimensional rod-shaped FeTe 1.5The preparation method of FeTe2@C microwave absorbing material includes the following steps:
[0043] (1) 3.6 mmol of C4H4O4 was dissolved in 50 mL of deionized water. The solution was stirred at 70 °C for 10 min, and then 4 mmol of Fe(NO3)2·9H2O was added and stirred for another 10 min to obtain an orange suspension. Then, the mixed solution was transferred to a reaction vessel and placed in an electric heating drying oven. The temperature was increased to 120 °C at a rate of 6 °C / min and kept at this temperature for 6 h. After the reaction was completed, the mixture was cooled to room temperature. The reaction product was washed three times with anhydrous ethanol and distilled water alternately. After filtration, a black solid product was obtained. After drying at 80 °C for 12 h, MIL-88A nanomaterials were obtained.
[0044] (2) Dissolve 0.2g of MIL-88A in 100mL of isopropanol, stir rapidly at 800 rpm and add 0.1g of PDA, continue stirring to obtain an orange suspension. Then, add 1mL of NH3·H2O to the above reaction solution, and immediately form a brownish-gray solution. After stirring for 12h, wash the reaction product three times with anhydrous ethanol and distilled water alternately. After filtration, a brownish-black product is obtained. After drying at 80℃ for 12h, the MIL-88A@PDA precursor is obtained.
[0045] (3) After uniformly mixing 200 mg MIL-88A@PDA and 600 mg Te powder, the mixture was placed in a tube furnace and heated to 700 °C at a rate of 3 °C / min under argon protection. The mixture was calcined for 3 h and then cooled with the furnace to obtain FeTe. 1.5 / FeTe2@C composite microwave absorbing material, denoted as FTC-2.
[0046] Example 3
[0047] A one-dimensional rod-shaped FeTe 1.5 The preparation method of FeTe2@C microwave absorbing material includes the following steps:
[0048] (1) 3.6 mmol of C4H4O4 was dissolved in 50 mL of deionized water. The solution was stirred at 70 °C for 10 min, and then 4 mmol of Fe(NO3)2·9H2O was added and stirred for another 10 min to obtain an orange suspension. Then, the mixed solution was transferred to a reaction vessel and placed in an electric heating drying oven. The temperature was increased to 120 °C at a rate of 6 °C / min and kept at this temperature for 6 h. After the reaction was completed, the mixture was cooled to room temperature. The reaction product was washed three times with anhydrous ethanol and distilled water alternately. After filtration, a black solid product was obtained. After drying at 80 °C for 12 h, MIL-88A nanomaterials were obtained.
[0049] (2) Dissolve 0.2g of MIL-88A in 100mL of isopropanol, stir rapidly at 800 rpm and add 0.1g of PDA, continue stirring to obtain an orange suspension. Then, add 1mL of NH3·H2O to the above reaction solution, and immediately form a brownish-gray solution. After stirring for 12h, wash the reaction product three times with anhydrous ethanol and distilled water alternately. After filtration, a brownish-black product is obtained. After drying at 80℃ for 12h, the MIL-88A@PDA precursor is obtained.
[0050] (3) After uniformly mixing 200 mg MIL-88A@PDA and 600 mg Te powder, the mixture was placed in a tube furnace and heated to 750 °C at a rate of 3 °C / min under argon protection. The mixture was calcined for 3 h and then cooled in the furnace to obtain FeTe. 1.5 / FeTe2@C composite microwave absorbing material, denoted as FTC-3.
[0051] Performance testing:
[0052] 1. The phase structure of the microwave absorbing material of Example 2 was analyzed using an X-ray diffractometer (XRD).
[0053] Figure 1 MIL-88A and FeTe prepared in Example 2 1.5 XRD pattern of / FeTe2@C. From Figure 1 (a) This demonstrates the successful preparation of MIL-88A. From Figure 1 (b) FeTe can be observed simultaneously 1.5 The diffraction peaks of FeTe2, appearing at 2θ = 26.9°, 31.3°, 42.0°, 47.5°, 56.1°, and 58.3°, are attributed to FeTe2. 1.5 The corresponding standard PDF card (JCPDS No. 07-0136) shows that the crystal plane indices are (100), (101), (102), (110), (103), and (112), respectively. Meanwhile, the diffraction peaks of FeTe2 are located at diffraction angles 2θ = 27.0°, 28.5°, 31.9°, 33.2°, 43.9°, 46.8°, 49.4°, 52.6°, 58.5°, and 69.7°, respectively. The corresponding standard PDF card (JCPDS No. 89-1639) shows that the crystal plane indices are (011), (101), (111), (120), (211), (002), (031), (131), (122), and (240), respectively. These results indicate that FeTe2 was successfully prepared. 1.5 / FeTe2@C composite microwave absorbing material.
[0054] 2. The FeTe prepared in Example 2 was examined using a scanning electron microscope (SEM).1.5 The microstructure of the FeTe2@C microwave absorbing material was analyzed.
[0055] Figure 2 MIL-88A, MIL-88A@PDA and FeTe prepared in Example 2 1.5 SEM image of the FeTe2@C composite microwave absorbing material. Figure 2 (a) and (b) are SEM images of MIL-88A at different magnifications. It can be seen that MIL-88A exhibits a rod-shaped polyhedral structure of different sizes. The size of a single nanorod is about 4-5 μm, and the nanorods are stacked on top of each other. Figure 2 (c) and (d) show the results of the MIL-88 sample after PDA coating treatment. PDA is uniformly covered on MIL-88A, and the morphology remains unchanged. Figure 2 (e) and (f) are FeTe 1.5 High-resolution electron microscope (HEM) images of the FeTe2@C composite microwave absorbing material at different magnifications show that the rod-shaped polyhedral microstructure of the sample remains intact and uniform. This can be attributed to the protective effect of the nitrogen-doped carbon shell, which effectively protects the structural stability of the material during high-temperature tellurization. The core-shell rod-shaped structure encapsulated by the carbon shell generates more heterogeneous interfaces, thereby promoting interfacial polarization loss. Simultaneously, the rod-shaped polyhedral structure provides pathways for electron migration and hopping, which is beneficial for electromagnetic wave attenuation.
[0056] 3. The electromagnetic parameters of the sample are analyzed using a vector network analyzer (VNA) to calculate its microwave absorption performance.
[0057] Figure 3 FeTe prepared in Example 1 1.5 Reflection loss curves of FeTe2@C composite absorbing materials with thicknesses ranging from 1.0 to 5.5 mm; Figure 4 FeTe prepared in Example 2 1.5 Reflection loss curves of FeTe2@C composite absorbing materials with thicknesses ranging from 1.0 to 5.5 mm; Figure 5 FeTe prepared in Example 3 1.5 Reflection loss curves of FeTe2@C composite absorbing materials with thicknesses ranging from 1.0 to 5.5 mm. Figure 3 It can be seen that FTC-1 (FeTe prepared in Example 1) 1.5 / FeTe2@C composite microwave absorbing material) at a thickness of 4.00 mm, RL min The value is -30.82dB (14.88GHz), and the EAB value is 1.09GHz (13.85-14.94GHz). (By...) Figure 4 It can be seen that FTC-2 (FeTe prepared in Example 2)1.5 RL of FeTe2@C composite absorbing material min The value is significantly improved compared to FTC-1 and FTC-3, especially when the matching thickness is 1.50mm. min The absorption value is -47.61 dB at 16.64 GHz, and the EAB value is 3.76 GHz (14.24-18.00 GHz), showing a significant improvement in absorption performance. This improvement is attributed to strong electromagnetic attenuation and good impedance matching characteristics. The unique core-shell structure increases the material's interfacial polarization and improves its impedance matching characteristics, while the moderate conductivity provides strong conductive loss, significantly dissipating electromagnetic waves. Figure 5 It can be seen that as the tellurization temperature increases, FTC-3 (FeTe prepared in Example 3) exhibits higher efficiency and lower yield. 1.5 The absorption performance of the FeTe2@C composite absorbing material decreased significantly, RL min The EAB values are -25.08 dB (15.52 GHz) and 4.64 GHz (13.36-18.00 GHz), respectively. Clearly, the sample's RL... min The value of the dielectric constant first increases and then decreases with increasing tellurization temperature. This is because excessively high temperatures can damage the microstructure of the sample, directly affecting the dielectric loss and impedance matching of the material; conversely, when the temperature is too low, the dielectric constant of the sample is low, and it cannot produce high electromagnetic attenuation. Therefore, temperature changes have a significant impact on electromagnetic parameters, and a suitable temperature helps to obtain good microwave absorption performance. FeTe 1.5 / FeTe2@C composite material has excellent electromagnetic wave absorption performance, meeting the requirements of "thin, light, wide, and strong" for microwave absorbing materials.
[0058] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A FeTe 1.5 The preparation method of / FeTe2@C composite microwave absorbing material is characterized by... Includes the following steps: S1. Dissolve fumaric acid in distilled water, then add ferric nitrate nonahydrate, and continue stirring to obtain an orange suspension; S2. The mixed solution is transferred to a reactor for hydrothermal reaction. After the reaction is completed, the mixture is cooled with the furnace, then filtered, washed and dried to obtain MIL-88A. S3. Add MIL-88A and dopamine hydrochloride to an isopropanol solution, then add ammonia water under rapid stirring. After stirring at room temperature, filter, wash and dry to obtain MIL-88A@PDA precursor. S4. After uniformly mixing MIL-88A@PDA with tellurium powder, the mixture is placed in a tube furnace and calcined under inert gas protection. The mixture is then cooled in the furnace to obtain FeTe. 1.5 / FeTe2@C composite material.
2. The FeTe according to claim 1 1.5 The preparation method of FeTe2@C composite microwave absorbing material is characterized by: In step S1, the molar ratio of fumaric acid and ferric nitrate nonahydrate is 0.9:(1-1.2).
3. The FeTe according to claim 1 1.5 The preparation method of FeTe2@C composite microwave absorbing material is characterized by: In step S1, the stirring speed is 400-600 rpm and the reaction time is 8-10 min.
4. The FeTe according to claim 1 1.5 The preparation method of FeTe2@C composite microwave absorbing material is characterized by: In step S2, the heating rate is 5–8 °C / min, and the reaction time is 5–6 h.
5. The FeTe according to claim 1 1.5 The preparation method of FeTe2@C composite microwave absorbing material is characterized by: In step S2, the drying temperature is 60–80°C and the drying time is 12–14 hours.
6. The FeTe according to claim 1 1.5 The preparation method of FeTe2@C composite microwave absorbing material is characterized by: In step S3, the mass ratio of MIL-88A to dopamine hydrochloride is 1:(0.5~1).
7. The FeTe according to claim 1 1.5 The preparation method of FeTe2@C composite microwave absorbing material is characterized by: In step S3, the stirring speed is 400-600 rpm and the reaction time is 10-12 h.
8. The FeTe according to claim 1 1.5 The preparation method of FeTe2@C composite microwave absorbing material is characterized by: In step S4, the mass ratio of MIL-88A@PDA and tellurium powder is 1:(1-3).
9. A FeTe according to claim 1 1.5 The preparation method of FeTe2@C composite microwave absorbing material is characterized by: In step S4, the inert gas includes argon, the heating rate is 2-5℃ / min, the calcination temperature is 600-800℃, and the calcination time is 3-4h.
10. A FeTe based on any one of claims 1-9 1.5 / Preparation method of FeTe2@C composite microwave absorbing material 1.5 / FeTe2@C composite microwave absorbing material.