An electrode loaded with in-situ restructured copper-carbon composite catalyst and a preparation method and application thereof

By preparing electrodes for in-situ reconstructed copper-carbon composite catalysts, the problems of poor selectivity, low activity, and insufficient stability of copper-based composite materials in the CO₂ electroreduction reaction were solved, thereby improving the electrocatalytic performance.

CN117385404BActive Publication Date: 2026-11-24CHN ENERGY NEW ENERGY TECHNOLOGY RESEARCH INSTITUTE CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311133507.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-04
Publication Date
2026-11-24
Estimated Expiration
2043-09-04

AI Technical Summary

Technical Problem

Existing copper-based composite materials suffer from poor selectivity, low activity, and insufficient stability in the CO₂ electroreduction reaction, and their preparation methods are complex and require the control of many parameters.

Method used

An electrode for in-situ reconstructed copper-carbon composite catalyst was prepared by calcining a mixture of copper salt, carbon material, organic solvent and water, mixing it with phosphate buffer solution and drying it, and then mixing it with Nafion ethanol solution and loading it onto a conductive substrate for in-situ electroreduction.

Benefits of technology

The preparation method is simple, and the obtained supported in-situ reconstructed copper-carbon composite catalyst has stable morphology, good electrocatalytic performance, and high reduction activity, thus solving the problems of insufficient selectivity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117385404B_ABST
    Figure CN117385404B_ABST
Patent Text Reader

Abstract

This invention relates to the field of carbon dioxide resource utilization and discloses a method for preparing an electrode for a supported in-situ reconstructed copper-carbon composite catalyst. The method includes the following steps: (1) mixing copper salt, carbon material, organic solvent, and water, and then calcining the mixture in the presence of a protective gas; (2) mixing the calcined product obtained in step (1) with a phosphate buffer solution and then drying it; (3) mixing the dried product obtained in step (2) with a Nafion ethanol solution, and then loading the resulting mixture onto a conductive substrate for in-situ electroreduction to obtain an electrode for the supported in-situ reconstructed copper-carbon composite catalyst. The electrode for the supported in-situ reconstructed copper-carbon composite catalyst prepared by this method exhibits stable catalyst morphology, high reduction activity, good product selectivity, and low preparation cost and simple preparation during CO2 electroreduction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of carbon dioxide resource utilization, specifically to an electrode supported on an in-situ reconstructed copper-carbon composite catalyst, its preparation method, and its application. Background Technology

[0002] The increasing concentration of CO2 in the atmosphere has spurred the development of various CO2 emission reduction and conversion technologies, including thermochemical, photochemical, and electrochemical methods, to convert carbon dioxide into valuable chemical products and fuels and maintain the dynamic balance of the carbon cycle. Electrochemical CO2 reduction is one of the most attractive strategies due to its numerous advantages, including mild reaction conditions operating at room temperature and atmospheric pressure, recyclable electrolytes, and an environmentally friendly driving force through potential synergies with renewable electricity.

[0003] Copper-based composites are currently the only reported metal catalysts capable of efficiently converting CO2 into multi-carbon products, and they are abundant, inexpensive, and readily available. However, they still suffer from poor selectivity, low activity, and insufficient stability. On the one hand, the slow carbon-carbon coupling kinetics at the copper surface limit the efficient formation of multi-carbon products. On the other hand, mass transfer limitations at the electrode interface significantly affect the reaction activity, typically restricting the increase in current density. Therefore, researching ways to improve the activity and selectivity of copper-based composites in the electroreduction of CO2 to multi-carbon products is of great significance.

[0004] The morphology of copper nanocatalysts significantly affects the product selectivity of electrocatalytic CO2 reduction reactions. Previous literature reports the synthesis of copper catalysts with different morphologies through methods such as annealing, thin-film chemical treatment, colloidal synthesis, and solution electrodeposition. The results show that morphological differences do indeed lead to changes in the performance of electrocatalytic CO2 reduction reactions. When copper catalysts undergo CO2 electroreduction reactions at negative potentials, their morphology may change, resulting in electrochemical in-situ reconstruction processes such as fragmentation and agglomeration. Changes in both particle size and morphology ultimately affect the catalyst's performance. For example, Yang Peidong's team reported that closely packed spherical copper particles can be reconstructed into cubic nanostructures after applying a certain potential, yielding multi-carbon products (Copper Nanoparticle Ensembles for Selective Electroreduction of CO2 to C2-C3 Products. Proceedings of the National Academy of Sciences of the United States of America, 2017, 114(40):10560). Sargent et al. employed a surface reconstruction process to adjust the morphology of copper catalysts, thereby improving product selectivity and bias current density in CO2 electroreduction reactions. 2+ Hydrocarbons. Advanced Materials, 2018, 30(49): 1804867. However, existing studies have focused on the structure-activity relationship of the catalyst itself, with insufficient understanding of the dynamic changes in catalyst structure; at the same time, the preparation methods are complex and require control of many parameters. In addition, the phenomenon that the morphology and structure of the catalyst changes in the early stage of the electrocatalytic reaction is not universal. Summary of the Invention

[0005] The purpose of this invention is to overcome the problems of poor product selectivity, low catalytic activity and insufficient stability of CO2 reduction reaction in the prior art, as well as the complex preparation method and many parameters that need to be controlled. This invention provides an electrode for supporting in-situ reconstructed copper-carbon composite catalyst, its preparation method and application.

[0006] To achieve the above objectives, the first aspect of the present invention provides a method for preparing an electrode supported on an in-situ reconstructed copper-carbon composite catalyst, the method comprising the following steps:

[0007] (1) After mixing copper salt, carbon material, organic solvent and water, calcination is carried out in the presence of protective gas;

[0008] (2) The calcined product obtained in step (1) is mixed with a phosphate buffer solution and then dried;

[0009] (3) The dried product obtained in step (2) is mixed with Nafion ethanol solution, and then the mixture is loaded onto a conductive substrate and subjected to in-situ electroreduction to obtain an electrode of copper-carbon composite catalyst supported in situ.

[0010] Preferably, in step (1), the copper salt is selected from one or more of copper nitrate, copper chloride, copper acetate and copper sulfate.

[0011] Preferably, the solid-liquid ratio of copper salt to water is 1-10 mg: 1 mL.

[0012] Preferably, in step (1), the carbon material is selected from one or more of activated carbon, carbon black, carbon nanotubes or graphene.

[0013] Preferably, the solid-liquid ratio of carbon material to water is 5-50 mg: 1 mL.

[0014] Preferably, in step (1), the organic solvent is selected from ethanol and / or propanol.

[0015] Preferably, the volume ratio of organic solvent to water is 0.01-0.1:1.

[0016] Preferably, in step (1), the protective gas is selected from at least one of nitrogen, argon and helium.

[0017] Preferably, the flow rate of the protective gas is 10-300 mL / min, and more preferably 50-100 mL / min.

[0018] Preferably, in step (1), the roasting temperature is 200-600℃, more preferably 250-500℃; and the roasting time is 1-10h, more preferably 1-5h.

[0019] Preferably, in step (2), the solid-liquid ratio of the calcination product to the phosphate buffer solution is 0.5-10 g: 1 L.

[0020] Preferably, in step (2), the phosphate buffer solution is selected from two or more of potassium phosphate, potassium monohydrogen phosphate, potassium dihydrogen phosphate, sodium phosphate, sodium monohydrogen phosphate, and sodium dihydrogen phosphate.

[0021] Preferably, in step (2), the mixing time is 1-13 hours.

[0022] Preferably, in step (3), the solid-liquid ratio of the calcined product to the Nafion ethanol solution is 5-50 mg: 1 mL.

[0023] Preferably, in step (2), the Nafion concentration of the Nafion ethanol solution is 0.1-3% by weight, preferably 0.5-1% by weight.

[0024] Preferably, in step (3), the pre-reduction potential applied by in-situ electroreduction is -0.6 to -1.6V vs. RHE, and more preferably -0.8 to -1.4V vs. RHE.

[0025] A second aspect of the present invention provides an electrode for a supported in-situ reconstructed copper-carbon composite catalyst prepared by the method described above.

[0026] The third aspect of this invention provides the application of the electrode of the supported in-situ reconstructed copper-carbon composite catalyst described above in the electroreduction of CO2.

[0027] A fourth aspect of the present invention provides a method for electroreducing CO2, the method comprising: employing a three-electrode system, wherein the electrode of the previously described supported in-situ reconstructed copper-carbon composite catalyst is used as the working electrode for electroreducing CO2, an Ag / AgCl electrode is used as the reference electrode, a platinum mesh is used as the counter electrode, a soluble bicarbonate solution is used as the electrolyte, a sealed H-type double-cell electrolytic cell is used as the reactor, CO2 is introduced, a voltage is applied, and CO2 is electroreduced in situ.

[0028] Preferably, the CO2 gas flow rate is 5-100 mL / min.

[0029] Preferably, the reaction temperature is 10-60℃.

[0030] Preferably, the voltage is -1.0 to -2.0V vs. RHE.

[0031] The technical method described in this invention has the following advantages compared with the prior art:

[0032] (1) The preparation method of the present invention is simple and requires few parameters to be controlled.

[0033] (2) The electrode of the supported in-situ reconstructed copper-carbon composite catalyst obtained by the present invention has stable morphology, good electrocatalytic performance and high reduction activity. Attached Figure Description

[0034] Figure 1 Here is a SEM image of the sample prepared in Example 1;

[0035] Figure 2 This is a TEM image of the sample prepared in Example 1. Detailed Implementation

[0036] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.

[0037] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0038] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating relative importance or implying the number of technical features indicated. Therefore, unless otherwise stated, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature; "multiple" means two or more. The term "comprising" and any variations thereof mean non-exclusive inclusion, where one or more other features, integers, steps, operations, units, components, and / or combinations thereof may be present or added.

[0039] This invention provides a method for preparing an electrode supported on an in-situ reconstructed copper-carbon composite catalyst, the method comprising the following steps:

[0040] (1) After mixing copper salt, carbon material, organic solvent and water, calcination is carried out in the presence of protective gas;

[0041] (2) The calcined product obtained in step (1) is mixed with a phosphate buffer solution and then dried;

[0042] (3) The dried product obtained in step (2) is mixed with Nafion ethanol solution, and then the mixture is loaded onto a conductive substrate and subjected to in-situ electroreduction to obtain an electrode of copper-carbon composite catalyst supported in situ.

[0043] In the method described in this invention, step (1) yields a carbon material loaded with CuO. x The composite material of particles, in step (2) a composite material of copper phosphate nanosheets loaded on carbon material is obtained, and in step (3) a composite material of carbon material and Cu nanoparticles loaded on conductive matrix is ​​obtained.

[0044] In a preferred embodiment, the specific process of step (1) includes: mixing copper salt, carbon material, organic solvent and water, stirring and evaporating to dryness, and then calcining in the presence of a protective gas.

[0045] In a preferred embodiment, in step (1), the copper salt is a water-soluble copper salt. Specifically, the copper salt can be one or more of copper nitrate, copper chloride, copper acetate, and copper sulfate.

[0046] More preferably, in step (1), the solid-liquid ratio of copper salt and water is 1-10 mg:1 mL; specifically, it can be 1 mg:1 mL, 2 mg:1 mL, 3 mg:1 mL, 4 mg:1 mL, 5 mg:1 mL, 6 mg:1 mL, 7 mg:1 mL, 8 mg:1 mL, 9 mg:1 mL or 10 mg:1 mL.

[0047] In a preferred embodiment, in step (1), the carbon material is selected from one or more of activated carbon, carbon black, carbon nanotubes or graphene.

[0048] More preferably, in step (1), the solid-liquid ratio of carbon material and water is 5-50 mg:1 mL; specifically, it can be 5 mg:1 mL, 10 mg:1 mL, 15 mg:1 mL, 20 mg:1 mL, 25 mg:1 mL, 30 mg:1 mL, 35 mg:1 mL, 40 mg:1 mL, 45 mg:1 mL or 50 mg:1 mL.

[0049] In a preferred embodiment, in step (1), the organic solvent is a hydrophilic organic solvent, specifically, the organic solvent is selected from ethanol and / or propanol.

[0050] More preferably, in step (1), the volume ratio of ethanol to water is 0.01-0.1, specifically, it can be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, or 0.1.

[0051] In this invention, the hydrophilic organic solvent promotes better dispersion of carbon materials in the solution and also facilitates the loading process of copper.

[0052] In a preferred embodiment, in step (1), the mixing method is ultrasonic oscillation.

[0053] More preferably, the ultrasonic oscillation time is 5-60 min, more preferably, the ultrasonic oscillation time is 10-30 min, specifically, it can be 10 min, 15 min, 20 min, 25 min, 30 min or 50 min.

[0054] In a preferred embodiment, in step (1), the temperature for stirring and evaporating is 10-60°C, specifically, it can be 10°C, 20°C, 25°C, 30°C, 40°C, 45°C, 50°C or 60°C.

[0055] The stirring and evaporation process described in this invention mainly removes water and a small amount of organic solvent. Low-temperature stirring and evaporation can keep the evaporation process slow, thereby promoting a more uniform dispersion and loading of the copper precursor in the carbon material.

[0056] In a preferred embodiment, in step (1), the protective gas is selected from one or more of nitrogen, argon and helium.

[0057] In a preferred embodiment, in step (1), the gas flow rate of the protective gas is 10-300 mL / min, preferably 50-100 mL / min; specifically, it can be 50 mL / min, 60 mL / min, 70 mL / min, 80 mL / min, 90 mL / min, 100 mL / min or 200 mL / min.

[0058] In a preferred embodiment, in step (1), the calcination temperature is 200-600℃ and the calcination time is 1-10h, more preferably 250-500℃ and the calcination time is 1-5h; specifically, the calcination temperature is 200℃, 250℃, 300℃, 380℃, 450℃, 500℃, 550℃ or 600℃; the time can be 1h, 2h, 3h, 4h or 5h.

[0059] In a preferred embodiment, in step (2), the initial temperature of roasting is 20-30℃; specifically, it can be 20℃, 21℃, 22℃, 23℃, 24℃, 25℃, 26℃, 27℃, 28℃, 29℃ or 30℃.

[0060] In a preferred embodiment, in step (1), the heating rate during calcination is 1-20°C / min, and more preferably, the heating rate during annealing is 1-10°C / min. Specifically, it can be 1°C / min, 2°C / min, 3°C / min, 5°C / min, 8°C / min, or 10°C / min.

[0061] In this invention, calcination can promote the decomposition of the Cu precursor, thereby obtaining CuO supported on carbon materials. x (x = 0, 0.5, 1). Due to the reducing properties of carbon materials in a high-temperature inert atmosphere, the Cu precursor can be decomposed into Cu, Cu2O and CuO, i.e. Cu species in different valence states, depending on the calcination temperature.

[0062] In a preferred embodiment, step (2) specifically includes: first mixing the calcined product obtained in step (1) with a phosphate buffer solution, then shaking it on a shaker for a second mixing, and then drying it.

[0063] In a preferred embodiment, in step (2), the solid-liquid ratio of the calcined product and the phosphate buffer is 0.5-10 g:1 L. Specifically, it can be 0.5 g:1 L, 1 g:1 L, 2 g:1 L, 3 g:1 L, 4 g:1 L, 5 g:1 L, 6 g:1 L, 7 g:1 L, 8 g:1 L, 9 g:1 L, or 10 g:1 L.

[0064] In a preferred embodiment, in step (2), the phosphate buffer solution is prepared from two or more of potassium phosphate, potassium monohydrogen phosphate, potassium dihydrogen phosphate, sodium phosphate, sodium monohydrogen phosphate, or sodium dihydrogen phosphate.

[0065] In a preferred embodiment, in step (2), the molar ratio of dihydrogen phosphate to monohydrogen phosphate is 1.58, and the pH of the prepared phosphate buffer solution is 7.

[0066] More preferably, the concentration of the phosphate buffer solution is 0.01-0.5 mol / L, specifically, it can be 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L or 0.5 mol / L.

[0067] In this invention, phosphate buffer solution is used to allow CuO loaded on carbon materials to be transported. x It is transformed into nanosheet-like Cu3(PO4)2.

[0068] In a preferred embodiment, in step (2), the first mixing method is stirring and / or ultrasonic vibration.

[0069] More preferably, in step (2), the first mixing time is 5-60 min, more preferably, the mixing time is 30-60 min, specifically, it can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min.

[0070] In a preferred embodiment, in step (2), the shaking time for the second mixing on the shaker is 1-12 hours, specifically 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, and 12 hours.

[0071] In a preferred embodiment, in step (2), the drying temperature is 60-100℃, specifically, it can be 60℃, 70℃, 80℃, 90℃ or 100℃.

[0072] In a preferred embodiment, in step (2), the drying is carried out in an oven for a time of 8-24 hours, specifically 12 hours, 15 hours, 18 hours, 20 hours, 22 hours or 24 hours.

[0073] Preferably, in step (3), the solid-liquid ratio of the calcined product to the Nafion ethanol solution is 5-50 mg:1 mL. Specifically, it can be 5 mg:1 mL, 10 mg:1 mL, 15 mg:1 mL, 20 mg:1 mL, 25 mg:1 mL, 30 mg:1 mL, 35 mg:1 mL, 40 mg:1 mL, 45 mg:1 mL, or 50 mg:1 mL.

[0074] In a preferred embodiment, in step (3), the Nafion ethanol solution is an ethanol solution of a perfluorosulfonic acid polymer, purchased from DuPont Corporation of the United States, with a Nafion concentration of 5% by weight, and diluted with ethanol as a solvent.

[0075] In a preferred embodiment, in step (3), the Nafion concentration of the Nafion ethanol solution is 0.1-3 wt%, more preferably 0.5-1 wt%, specifically, it can be 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, or 1 wt%.

[0076] In step (3), the conductive substrate is a conventional choice in the art. In a preferred embodiment, the conductive substrate is porous carbon paper, which is purchased from Shanghai Hesen Electric Co., Ltd. as model HCP020.

[0077] In a preferred embodiment, in step (3), the pre-reduction potential is -0.6 to -1.6V vs. RHE, more preferably, the pre-reduction potential is -0.8 to -1.4V vs. RHE, specifically, it can be -0.8V vs. RHE, -0.9V vs. RHE, -1.0V vs. RHE, -1.1V vs. RHE, -1.2V vs. RHE, -1.3V vs. RHE, -1.4V vs. RHE, or -1.6V vs. RHE.

[0078] In this invention, vs. RHE refers to the relative reversible hydrogen electrode potential, and the applied potential is relative to the Ag / AgCl reference electrode (saturated KCl solution), which can be converted to the reversible hydrogen electrode potential using the following formula.

[0079] E(vs.RHE)=E(vs.Ag / AgCl)+0.197V+0.0591V×pH

[0080] In the formula, E(vs.Ag / AgCl) is the applied potential relative to the Ag / AgCl reference electrode, and the pH value is obtained by measuring with a pH meter. When the electrolyte is KHCO3, the pH range is 6-8.

[0081] A second aspect of the present invention provides an electrode for a supported in-situ reconstructed copper-carbon composite catalyst prepared by the method described above.

[0082] In a preferred embodiment, the electrode loading of the supported in-situ reconstructed copper-carbon composite catalyst prepared by the method is 0.1-5 mg / cm³. 2 Specifically, the loading capacity can be 0.1 mg / cm³. 2 0.5 mg / cm 2 1mg / cm 2 2mg / cm 2 3mg / cm 2 4mg / cm 2 5mg / cm 2 6mg / cm 2 7mg / cm 2 8mg / cm 2 9mg / cm 2 Or 10mg / cm 2 The loading amount is the in-situ reconstructed copper / carbon composite catalyst loaded to 1 cm³. 2 The amount on the conductive substrate.

[0083] The third aspect of this invention provides the application of the electrode of the supported in-situ reconstructed copper-carbon composite catalyst described above in the electroreduction of CO2.

[0084] A fourth aspect of the present invention provides a method for electroreducing CO2, the method comprising: employing a three-electrode system, wherein the electrode of the previously described supported in-situ reconstructed copper-carbon composite catalyst is used as the working electrode for electroreducing CO2, an Ag / AgCl electrode is used as the reference electrode, a platinum mesh is used as the counter electrode, a soluble bicarbonate solution is used as the electrolyte, a sealed H-type double-cell electrolytic cell is used as the reactor, CO2 is introduced, a power supply is connected, and CO2 is electrolyzed.

[0085] In a preferred embodiment, the soluble bicarbonate solution is potassium bicarbonate with a concentration of 0.1-0.5 mol / L.

[0086] In a preferred embodiment, the CO2 flow rate in the electroreduction of CO2 is 5-100 mL / min; specifically, it can be 5 mL / min, 10 mL / min, 15 mL / min, 20 mL / min, 30 mL / min, 40 mL / min, 50 mL / min, 60 mL / min, 80 mL / min, 90 mL / min or 100 mL / min.

[0087] In a preferred embodiment, the reaction temperature in the application of electroreduction of CO2 is 10-60°C; specifically, it can be 10°C, 15°C, 20°C, 25°C, 30°C, 40°C, 50°C, or 60°C.

[0088] In a preferred embodiment, the voltage in the electroreduction of CO2 is -1.0 to -2.0V vs. RHE; specifically, it can be -1.2V vs. RHE, -1.3V vs. RHE, -1.4V vs. RHE, -1.5V vs. RHE, or -1.6V vs. RHE.

[0089] The following examples further illustrate the electrode for supported in-situ reconstructed copper-carbon composite catalyst, its preparation method, and its application according to the present invention. The examples are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures; however, the scope of protection of the present invention is not limited to the following examples.

[0090] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods in the art. Unless otherwise specified, the experimental materials used in the following embodiments are commercially available.

[0091] Example 1

[0092] (1) Add 70mg copper nitrate, 200mg activated carbon and 0.5mL ethanol to 10mL deionized water and sonicate for 20min. Stir the resulting solution at 25℃ until the water evaporates, then heat it to 400℃ at a heating rate of 2℃ / min and use argon gas at a flow rate of 100mL / min as a protective gas for calcination for 4h.

[0093] (2) Add 0.2g of the calcined product to 200mL of a phosphate buffer solution (pH=7, specifically prepared by mixing 0.83g of potassium dihydrogen phosphate, 0.41g of potassium monohydrogen phosphate and 200mL of deionized water), sonicate for 60min, then shake on a shaker for 4h, and dry in an oven at 80℃ for 12h.

[0094] (3) Disperse 10 mg of the dried product in 0.6 mL of 0.5% Nafion ethanol solution, then take 30 μL and drop it into a 1 cm solution. 2 On a porous carbon paper (1cm × 1cm), a pre-reduction potential of -1.2V vs. RHE is applied for in-situ electroreduction, resulting in a loading of 0.5mg / cm². 2 Copper-based CO2 electroreduction catalyst.

[0095] Example 2

[0096] (1) Add 50mg copper chloride, 300mg activated carbon and 0.5mL ethanol to 20mL deionized water and sonicate for 25min. Stir the resulting solution at 30℃ until the water evaporates, then raise the temperature to 250℃ at a rate of 2℃ / min and calcine with argon gas at a flow rate of 100mL / min for 4h.

[0097] (2) Add 0.3g of the calcined product to 300ml of a phosphate buffer solution (pH=7, specifically prepared by mixing 2.5g of potassium dihydrogen phosphate, 1.24g of potassium monohydrogen phosphate and 300mL of deionized water), sonicate for 40min, then shake on a shaker for 6h, and dry in an oven at 90℃ for 18h.

[0098] (3) Disperse 30 mg of the dried product in 0.6 mL of 0.5% Nafion ethanol solution, then take 30 μL and drop it into a 1 cm solution. 2 On a porous carbon paper (1cm × 1cm), an in-situ electroreduction was performed by applying a pre-reduction potential of -1.0V vs. RHE, resulting in a loading of 1.5mg / cm³. 2 Copper-based CO2 electroreduction catalyst.

[0099] Example 3

[0100] (1) Add 300mg copper sulfate, 600mg activated carbon and 0.5mL ethanol to 50mL deionized water and sonicate for 50min. Stir the resulting solution at 50℃ until the water evaporates, then heat it to 600℃ at a heating rate of 5℃ / min and use argon gas at a flow rate of 100mL / min as a protective gas for calcination for 4h.

[0101] (2) Add 0.6g of the calcined product to 100ml of a phosphate buffer solution (pH=7, specifically prepared by mixing 2.5g of potassium dihydrogen phosphate, 1.24g of potassium monohydrogen phosphate and 100mL of deionized water), sonicate for 50min, then shake on a shaker for 8h, and dry in an oven at 80℃ for 10h.

[0102] (3) Disperse 20 mg of the dried product in 1.2 mL of 0.5% Nafion ethanol solution, then take 30 μL and drop it into a 1 cm solution. 2 On a porous carbon paper (1cm × 1cm), an in-situ electroreduction was performed by applying a pre-reduction potential of -1.4V vs. RHE, resulting in a loading of 0.5mg / cm³. 2 Copper-based CO2 electroreduction catalyst.

[0103] Example 4

[0104] (1) Add 100mg copper acetate, 200mg activated carbon and 0.5mL ethanol to 30mL deionized water and sonicate for 30min. Stir the resulting solution at 45℃ until the water evaporates, then heat it to 450℃ at a heating rate of 5℃ / min and use argon gas at a flow rate of 200mL / min as a protective gas for calcination for 6h.

[0105] (2) Add 0.5g of the calcined product to 500ml of a phosphate buffer solution (pH=7, specifically prepared by mixing 3.7g sodium dihydrogen phosphate, 1.7g sodium monohydrogen phosphate and 500mL water), sonicate for 30min, then shake on a shaker for 4h, and dry in an oven at 90℃ for 10h.

[0106] (3) Disperse 30 mg of the dried product in 1.8 mL of 0.5% Nafion ethanol solution, then take 30 μL and drop it into a 1 cm solution. 2 On a porous carbon paper (1cm × 1cm), an in-situ electroreduction was performed by applying a pre-reduction potential of -1.6V vs. RHE, resulting in a loading of 0.5mg / cm³. 2 Copper-based CO2 electroreduction catalyst.

[0107] Example 5

[0108] (1) Add 80mg copper nitrate, 200mg graphene and 0.5mL ethanol to 20mL deionized water and sonicate for 30min. Stir the resulting solution at 60℃ until the water evaporates, then heat it to 380℃ at a heating rate of 2℃ / min and use argon gas at a flow rate of 100mL / min as a protective gas for calcination for 4h.

[0109] (2) Add 0.4g of the calcined product to 100ml of a phosphate buffer solution (pH=7, specifically prepared by mixing 0.42g of potassium dihydrogen phosphate, 0.21g of potassium monohydrogen phosphate and 100mL of deionized water), sonicate for 60min, then shake on a shaker for 4h, and dry in an oven at 80℃ for 12h.

[0110] (3) Disperse 10 mg of the dried product in 0.6 mL of 0.5% Nafion ethanol solution, then take 30 μL and drop it into a 1 cm solution. 2 On a porous carbon paper (1cm × 1cm), an in-situ electroreduction was performed by applying a pre-reduction potential of -1.2V vs. RHE, resulting in a loading of 0.5mg / cm³. 2 Copper-based CO2 electroreduction catalyst.

[0111] Example 6

[0112] (1) Add 60mg copper nitrate, 300mg activated carbon and 0.5mL ethanol to 30mL deionized water and sonicate for 30min. Stir the resulting solution at 40℃ until the water evaporates, then heat it to 250℃ at a heating rate of 2℃ / min and use argon gas at a flow rate of 100mL / min as a protective gas for calcination for 4h.

[0113] (2) Add 0.6g of the calcined product to 200ml of a phosphate buffer solution (pH=7, specifically prepared by mixing 1.67g of potassium dihydrogen phosphate, 0.83g of potassium monohydrogen phosphate and 200mL of deionized water), sonicate for 60min, then shake on a shaker for 4h, and dry in an oven at 80℃ for 12h.

[0114] (3) Disperse 10 mg of the dried product in 0.6 mL of 0.5% Nafion ethanol solution, then take 30 μL and drop it into a 1 cm solution. 2 On a porous carbon paper (1cm × 1cm), an in-situ electroreduction was performed by applying a pre-reduction potential of -1.2V vs. RHE, resulting in a loading of 0.5mg / cm³. 2 Copper-based CO2 electroreduction catalyst.

[0115] Example 7

[0116] (1) Add 100mg copper nitrate, 250mg carbon nanotubes and 0.5mL ethanol to 20mL deionized water and sonicate for 20min. Stir the resulting solution at 25℃ until the water evaporates, then heat it to 450℃ at a heating rate of 2℃ / min and use argon gas at a flow rate of 100mL / min as a protective gas for calcination for 4h.

[0117] (2) Add 0.8g of the calcined product to 300ml of a phosphate buffer solution (pH=7, specifically prepared by mixing 5g of potassium dihydrogen phosphate, 2.48g of potassium monohydrogen phosphate and 300mL of deionized water), sonicate for 60min, then shake on a shaker for 4h, and dry in an oven at 80℃ for 12h.

[0118] (3) Disperse 10 mg of the dried product in 0.6 mL of 0.5% Nafion ethanol solution, then take 30 μL and drop it into a 1 cm solution. 2 On a porous carbon paper (1cm × 1cm), an in-situ electroreduction was performed by applying a pre-reduction potential of -1.2V vs. RHE, resulting in a loading of 0.5mg / cm³. 2 Copper-based CO2 electroreduction catalyst.

[0119] Example 8

[0120] (1) Add 200mg copper nitrate, 600mg conductive carbon black and 3mL ethanol to 50mL deionized water and sonicate for 20min. Stir the resulting solution at 30℃ until the water evaporates, then heat it to 600℃ at a heating rate of 2℃ / min and use argon gas at a flow rate of 100mL / min as a protective gas for calcination for 4h.

[0121] (2) Add 0.2g of the calcined product to 200ml of a phosphate buffer solution (pH=7, specifically prepared by mixing 0.83g of potassium dihydrogen phosphate, 0.41g of potassium monohydrogen phosphate and 200mL of deionized water), sonicate for 60min, then shake on a shaker for 4h, and dry in an oven at 80℃ for 12h.

[0122] (3) Disperse 10 mg of the dried product in 0.6 mL of 0.5% Nafion ethanol solution, then take 30 μL and drop it into a 1 cm solution. 2 On a porous carbon paper (1cm × 1cm), an in-situ electroreduction was performed by applying a pre-reduction potential of -1.2V vs. RHE, resulting in a loading of 0.5mg / cm³. 2 Copper-based CO2 electroreduction catalyst.

[0123] Comparative Example 1

[0124] The method described in Example 1 was carried out, except that copper nitrate was not added in step (1).

[0125] Comparative Example 2

[0126] The method described in Example 1 is implemented, except that the roasting is not performed in the presence of a protective gas in step (1).

[0127] Comparative Example 3

[0128] The method described in Example 1 was implemented, except that phosphate buffer was not added in step (2).

[0129] Comparative Example 4

[0130] The method described in Example 1 is implemented, except that in-situ electrical reduction is not performed in step (3).

[0131] Test Example 1

[0132] The samples obtained during the preparation process in Example 1 were characterized using SEM, and the results are as follows: Figure 1 As shown.

[0133] As shown in the figure, in the preparation process of Example 1, the carbon material obtained by calcination has CuO loaded on it. x The composite material of particles, after being treated with phosphate-buffered saline (PBS), yields a composite material of copper phosphate nanosheets loaded on carbon material. Then, after in-situ electroreduction, a composite material of carbon material and Cu nanoparticles loaded on porous carbon paper is obtained.

[0134] Test Example 2

[0135] The sample obtained in Example 1 was characterized using TEM, and the results are as follows: Figure 2 As shown.

[0136] As shown in the figure, the sample obtained during the preparation process of Example 1, after calcination, yielded a carbon material with CuO supported on it. x The composite material of particles, after being treated with phosphate-buffered saline (PBS), yields a composite material of copper phosphate nanosheets loaded on carbon material. Then, after in-situ electroreduction, a composite material of carbon material and Cu nanoparticles loaded on porous carbon paper is obtained.

[0137] Test Example 3

[0138] The CO2 electroreduction performance of the materials prepared in the above embodiments and comparative examples was tested:

[0139] Test method: Add 10 mg of the prepared product to 0.6 mL of 0.5% Nafion ethanol solution, microwave oscillation for 30 min, take 30 μL of the mixture, and drop it onto a 1 cm... 2 The cathode electrode is obtained by drying on (1cm×1cm) carbon paper for 3 hours.

[0140] A three-electrode system was employed, using a sealed H-type dual-cell electrolytic cell as the reactor. An Ag / AgCl electrode was used as the reference electrode, and a 2cm × 2cm platinum mesh was used as the counter electrode. 30 mL of 0.1 mol / L KHCO3 solution was added to each cell of the H-type electrolytic cell as the electrolyte. A Nafion 117 proton exchange membrane separated the cathode and anode cells. During detection, CO2 was first introduced into the reactor for 30 min to pre-saturate it. The CO2 flow rate was maintained at a uniform rate throughout the reaction. A gas chromatograph was connected to the outlet for online detection of gaseous products, including CO, C2H4, and H2. After the reaction, the liquid products were collected, and headspace gas chromatography was used to detect alcohols, while liquid NMR was used to detect acids.

[0141] The overall efficiency of electrocatalytic CO2 production is the sum of the efficiencies of the gaseous and liquid phase products. The test conditions are shown in Table 1, and the test results are shown in Table 2.

[0142] The gaseous products H2, CO, and C2H4 were detected online using a Shimadzu GC-2014 gas chromatograph. The liquid product formic acid was detected offline using NMR spectroscopy with a JNM-ECZR instrument. The internal standards used for product analysis were heavy water (D2O) and 6 mmol L⁻¹. -1 An aqueous solution of sodium 3-(trimethylsilyl)-1-propanesulfonate (DSS) was prepared. 500 μL of the reaction liquid, 100 μL of the DSS solution, and 100 μL of D2O were placed in an NMR tube, and the liquid phase products were detected at a frequency of 600 Hz and under water peak suppression conditions.

[0143] The formula for calculating the product Faraday efficiency is as follows:

[0144] FE i(气相产物) =α i ×c i ×v×F×t / Q×100%

[0145] FE i(液相产物) =α i ×c i ×V×F / Q×100%

[0146] α i c is the number of electrons transferred when product i is produced by the electrocatalytic reduction reaction of CO2; i (mol·L -1 The concentration of product i detected; v(L·h) -1 The CO2 flow rate introduced into the reactor; V (L) is the volume of liquid in the electrode chamber; F is the Faraday constant (96485 C·mol⁻¹). -1 ); t(h) is the duration of the reaction; Q(C) is the total amount of charge applied.

[0147] Table 1

[0148]

[0149]

[0150] Table 2

[0151]

[0152]

[0153] As can be seen from the results in Table 2, the electrode of the supported in-situ reconstructed copper-carbon composite catalyst prepared by the method described in this invention has high CO2 electrocatalytic efficiency and high product selectivity.

[0154] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing an electrode supported on an in-situ reconstructed copper-carbon composite catalyst, characterized in that, The method includes the following steps: (1) After mixing copper salt, carbon material, organic solvent and water, calcination is carried out in the presence of protective gas; (2) The calcined product obtained in step (1) is mixed with a phosphate buffer solution and then dried; (3) The dried product obtained in step (2) is mixed with Nafion ethanol solution, and then the resulting mixture is loaded onto a conductive substrate and subjected to in-situ electroreduction to obtain an electrode for in-situ reconstruction of copper-carbon composite catalyst. In step (1), the carbon material is selected from one or more of activated carbon, carbon black, carbon nanotubes or graphene. In step (1), the solid-liquid ratio of carbon material to water is 5-50 mg: 1 mL. In step (1), the roasting temperature is 200-600℃ and the roasting time is 1-10h; In step (2), the solid-liquid ratio of the calcination product to the phosphate buffer solution is 0.5-10 g: 1 L. In step (2), the phosphate buffer solution is selected from two or more of potassium phosphate, potassium monohydrogen phosphate, potassium dihydrogen phosphate, sodium phosphate, sodium monohydrogen phosphate, and sodium dihydrogen phosphate.

2. The method according to claim 1, characterized in that, In step (1), the copper salt is selected from one or more of copper nitrate, copper chloride, copper acetate and copper sulfate.

3. The method according to claim 2, characterized in that, In step (1), the solid-liquid ratio of copper salt and water is 1-10 mg: 1 mL.

4. The method according to any one of claims 1-3, characterized in that, In step (1), the organic solvent is selected from ethanol and / or propanol.

5. The method according to claim 4, characterized in that, In step (1), the volume ratio of organic solvent to water is 0.01-0.1:

1.

6. The method according to claim 1, characterized in that, In step (1), the protective gas is selected from one or more of nitrogen, argon and helium.

7. The method according to claim 6, characterized in that, In step (1), the flow rate of the protective gas is 10-300 mL / min.

8. The method according to claim 7, characterized in that, In step (1), the flow rate of the protective gas is 50-100 mL / min.

9. The method according to claim 1, characterized in that, In step (1), the roasting temperature is 250-500℃ and the roasting time is 1-5h.

10. The method according to claim 1 or 9, characterized in that, In step (2), the mixing time is 1-13 hours.

11. The method according to claim 1, characterized in that, In step (3), the solid-liquid ratio of the calcined product to the Nafion ethanol solution is 5-50 mg: 1 mL.

12. The method according to claim 1 or 11, characterized in that, In step (3), the concentration of Nafion in the Nafion ethanol solution is 0.1-3 by weight.

13. The method according to claim 12, characterized in that, In step (3), the concentration of Nafion in the Nafion ethanol solution is 0.5-1% by weight.

14. The method according to claim 1, characterized in that, In step (3), the pre-reduction potential applied by in-situ electroreduction is -0.6~-1.6V vs. RHE.

15. The method according to claim 14, characterized in that, In step (3), the pre-reduction potential applied by in-situ electroreduction is -0.8~-1.4V vs. RHE.

16. The electrode of the supported in-situ reconstructed copper-carbon composite catalyst prepared by the method of any one of claims 1-15.

17. The application of the electrode of the supported in-situ reconstructed copper-carbon composite catalyst as described in claim 16 in the electroreduction of CO2.

18. A method for the electroreduction of CO2, the method comprising: A three-electrode system is used, with the electrode of the supported in-situ reconstructed copper-carbon composite catalyst as described in claim 16 as the working electrode for electroreduction of CO2, the Ag / AgCl electrode as the reference electrode, the platinum mesh as the counter electrode, the soluble bicarbonate solution as the electrolyte, and the sealed H-type double-cell electrolytic cell as the reactor. CO2 is introduced and the power supply is connected to perform electroreduction of CO2.

19. The method according to claim 18, characterized in that, The flow rate of CO2 gas is 5-100 mL / min.

20. The method according to claim 19, characterized in that, The temperature of the electroreduction reaction is 10-60℃.

21. The method according to claim 20, characterized in that, The voltage for the electroreduction reaction is -1.0 to -2.0 V vs. RHE.

Citation Information

Patent Citations

  • Copper-based catalyst, and preparation method and application thereof

    CN111659394A

  • Copper catalyst and preparation method and application thereof

    CN116334671A