Dielectric layer for an electrowetting lens and electrowetting lens
By employing a composite dielectric layer structure in the electrowetting lens, the problem of dielectric layer failure was solved, the service life was extended, and the performance of the dielectric layer was improved, thus promoting the application of electrowetting lenses in optical systems.
Patent Information
- Application Number
- CN202311496692.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-10
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-11-10
AI Technical Summary
The limitations of the dielectric layer material properties and structure of existing electrowetting lenses lead to dielectric failure, resulting in a short service life and affecting their stability and durability in optical systems.
A composite dielectric layer structure is adopted, including at least one inorganic dielectric film and at least one organic dielectric film. By combining two or more films with different barrier properties, the diffusion path of ion penetration is extended, the barrier properties and dielectric constant of the dielectric layer are improved, and the risk of dielectric layer breakdown is reduced.
This extends the service life of the electrowetting lens, increases the breakdown voltage of the dielectric layer, reduces the driving voltage, and enhances the working performance and stability of the electrowetting lens.
Smart Images

Figure CN117389027B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of lens manufacturing technology, and mainly to a dielectric layer for electrowetting lenses and an electrowetting lens. Background Technology
[0002] Electrowetting liquid lenses primarily utilize the electrowetting effect on a medium. By changing the applied voltage, they control the wetting properties of the liquid on the medium's surface, thus achieving zoom capabilities similar to the human eye's lens. Compared to traditional mechanical lenses, electrowetting lenses offer advantages such as simple structure, light weight, low cost, fast zooming, and superior imaging quality, making them highly promising for applications in mobile phones, cameras, and barcode scanners. However, due to limitations in the material properties and structure of the dielectric layer in existing electrowetting lenses, problems such as dielectric failure are prone to occur. This results in a generally short lifespan for electrowetting lenses, limiting their stability and durability in various optical systems.
[0003] Therefore, how to extend the service life of electrowetting lenses is a technical problem that needs to be solved. Summary of the Invention
[0004] In view of the shortcomings of the prior art, the purpose of this application is to provide a dielectric layer for an electrowetting lens and an electrowetting lens, which aims to improve the dielectric constant and barrier properties of the dielectric layer of the electrowetting lens.
[0005] The technical solution of this application is as follows: A dielectric layer for electrowetting a lens, wherein the dielectric layer for electrowetting the lens comprises at least one inorganic dielectric film and at least one organic dielectric film; The inorganic dielectric film is one or a combination of two or more of barium strontium titanate film, silicon dioxide film, aluminum oxide film and tantalum oxide film; The organic dielectric film is one or a combination of two or more of the following: a Pyrelin C film, a polyimide film, or a photoresist film.
[0006] The dielectric layer provided in this application is a composite dielectric thin film structure. By combining two or more organic dielectric thin films and inorganic dielectric thin films with different barrier properties, the diffusion path of ion penetration is extended by utilizing the composite system, so that the prepared dielectric layer has high barrier performance and plays a protective barrier role, thereby avoiding possible erosion caused by ion penetration and improving the service life of electrowetting lenses.
[0007] Furthermore, the dielectric layer for electrowetting the lens comprises at least two inorganic dielectric films and at least one organic dielectric film; the organic dielectric film is disposed between the two inorganic dielectric films.
[0008] Furthermore, the dielectric layer for electrowetting the lens comprises, from bottom to top, a barium strontium titanate film, a Pyrelin C film, and an aluminum oxide film.
[0009] Furthermore, the dielectric layer for electrowetting the lens comprises, from bottom to top, an aluminum oxide film, a Pyrelin C film, and an aluminum oxide film.
[0010] Furthermore, the thickness ratio of the inorganic dielectric film to the organic dielectric film is 1:10 to 10:1; the total thickness of the dielectric layer used for electrowetting the lens ranges from 100nm to 2µm.
[0011] Furthermore, the dielectric constant of the inorganic dielectric film is 5.5-265; the dielectric constant of the organic dielectric film is 2.95-4.1.
[0012] The inorganic dielectric thin film is prepared by chemical vapor deposition or solution method; Furthermore, when the inorganic dielectric film is prepared using the solution method, the following steps are included: Inorganic dielectric material is dissolved in a first solvent to prepare a solution. A mineralizing agent is added dropwise to the solution and stirred to obtain a suspension. The suspension is transferred to a high-pressure hydrothermal reactor and heated and stirred until the reaction is complete. The precipitate obtained after cooling is centrifuged and washed to obtain inorganic dielectric nanoparticles. The inorganic dielectric nanoparticles are dispersed in a second solvent, a surfactant is added, and the mixture is stirred until an inorganic dielectric nanoparticle sol is formed. The inorganic dielectric nanoparticle sol is coated on a substrate, subjected to low-temperature heat treatment in a vacuum atmosphere, and dried to obtain an inorganic dielectric nanoparticle gel. The inorganic dielectric nanoparticle gel is then subjected to low-temperature sintering to obtain an inorganic dielectric film. The first solvent is one of deionized water, anhydrous ethanol, methanol, acetonitrile, ethylene glycol, n-propanol, glacial acetic acid, and ethylene glycol methyl ether; the second solvent is one or both of ethanol and methanol. The concentration range of the inorganic dielectric material in the first solvent is 0.01-10 mol / L; The mineralizing agent is one of sodium hydroxide, potassium hydroxide, tetramethylammonium hydroxide, ammonia, and urea, and the concentration of the mineralizing agent in the first solvent is in the range of 0.5-15 mol / L; The surfactant is one of polyvinylpyrrolidone, oleic acid, tert-butylamine, polyvinyl alcohol, ethanolamine, and hexadecyltrimethylammonium bromide, and the concentration of the surfactant in the second solvent is in the range of 0.1-10 g / L; The inorganic dielectric nanoparticles have a particle size of 5-100 nm, and the concentration of the inorganic dielectric nanoparticles in the second solvent is in the range of 0.001-10 mol / L. The heating and stirring temperature range is 80-250℃, and the heating and stirring time range is 2-72h; The temperature range for the low-temperature heat treatment is 80-350℃; The temperature range for the low-temperature sintering is 80-140℃.
[0013] Furthermore, the Perylene C film is prepared by vacuum vapor deposition, including the following steps: Solid p-chloroxylene dimer raw material is placed in an evaporation chamber and sublimated at 100-160℃ to produce p-chloroxylene dimer gas; The dichloro-p-xylene dimer gas is fed into the pyrolysis chamber, and active 2-chloro-p-xylene monomer molecules are generated at 600-720°C. The 2-chloro-p-xylene monomer molecules were introduced into a vacuum deposition chamber at room temperature and polymerized and deposited on the substrate surface to obtain a Pyrelin C film.
[0014] An electrowetting lens, comprising a dielectric layer for electrowetting the lens as described above.
[0015] The inner diameter of the glass cavity in the electrowetting lens is 0.3-5 mm and the height is 0.1-5 mm; the dielectric constant of the dielectric layer used for the electrowetting lens is 2.95-265.
[0016] The present invention has the following beneficial effects: This invention provides a dielectric layer for electrowetting lenses. This dielectric layer is created by compositing two or more organic and inorganic dielectric films with different barrier properties. The composite system extends the diffusion path of ion penetration, resulting in a dielectric layer with high barrier properties. This avoids potential erosion caused by ion penetration and improves the service life of the electrowetting lens. Simultaneously, this dielectric layer possesses a high and tunable dielectric constant, which helps to increase the breakdown voltage of the dielectric layer and reduce the driving voltage of the electrowetting lens, thereby improving the working performance of the electrowetting lens and contributing to its development. Attached Figure Description
[0017] Figure 1a This is a scanning electron microscope image, magnified 2000x, of the alumina thin film prepared by chemical vapor deposition in Example 1 of this application. Figure 1b This is a scanning electron microscope image magnified 100,000 times of the alumina thin film prepared by chemical vapor deposition in Example 1 of this application.
[0018] Figure 2This is a scanning electron microscope image of the alumina thin film prepared by solution method in Example 3 of this application.
[0019] Figure 3 This is a schematic diagram of the dielectric layer structure in Embodiment 4 of this application.
[0020] Figure 4 This is a schematic diagram of the electrowetting lens in Embodiments 1-4 and Comparative Examples 1-3 of this application.
[0021] Figure 5 The figures show the refractive power test results of the electrowetting lenses in Examples 1-4 and Comparative Examples 1-3 of this application.
[0022] Labeling Explanation: 1. Glass cavity; 2. Lower electrode; 3. Dielectric layer; 31. Strontium barium titanate film; 32. Piriton C film; 33. Alumina film; 4. Hydrophobic layer; 5. Sealant layer; 6. Upper electrode; 7. Transparent top cover; 8. Conductive liquid; 9. Insulating liquid. Detailed Implementation
[0023] This application provides a dielectric layer for an electrowetting lens and an electrowetting lens. To make the objectives, technical solutions, and effects of this application clearer and more explicit, the following provides a more detailed description. It should be understood that the specific embodiments described herein are merely illustrative and are not intended to limit the scope of this application.
[0024] Regarding the short lifespan of electrowetting lenses, the inventors, through extensive and creative research, discovered that one of the reasons for the short lifespan of electrowetting lenses is that the dielectric layer of the electrowetting lens is prone to failure during operation, i.e., losing its dielectric properties. The inventors further analyzed and found that the reasons why the dielectric layer is prone to failure during operation include: (1) Under the action of electrolyte environment and repeated electric field, the dielectric layer is often easily corroded by ion penetration, leading to dielectric failure; (2) If the dielectric constant of the dielectric layer is too low, the required driving voltage is high, but when the external voltage is too high, the dielectric layer is easily broken down.
[0025] Based on the above findings, this application optimizes the composition of the dielectric layer to improve its barrier properties and reduce the problem of dielectric layer failure due to erosion. Simultaneously, it also aims to increase the dielectric constant of the dielectric layer, reducing the risk of dielectric layer breakdown due to a low dielectric constant. The inventive concept of this application is to composite two or more organic and inorganic dielectric films with different barrier properties, utilizing the composite system to extend the diffusion path of ion penetration. This results in a dielectric layer with high barrier properties that provides protection, preventing potential erosion caused by ion penetration, improving the lifespan of the electrowetting lens, and the composite dielectric layer also possesses high dielectric properties, which helps to increase the breakdown voltage of the dielectric layer and reduce the driving voltage of the electrowetting lens, improving the working performance of the electrowetting lens and further promoting the commercial development of electrowetting lenses.
[0026] This application provides a dielectric layer for electrowetting lenses, comprising at least one inorganic dielectric film and at least one organic dielectric film; the inorganic dielectric film may be one or a combination of two or more of barium strontium titanate film, silicon dioxide film, aluminum oxide film and tantalum oxide film; the organic dielectric film may be one or a combination of two or more of pyrene C film, polyimide film or photoresist film.
[0027] In this application, the inorganic dielectric film is a dense inorganic dielectric film. Due to the small bond length and stable properties of inorganic dielectric materials, the inorganic dielectric film has good barrier properties and is less affected by ambient temperature. The main component of the inorganic dielectric film is barium strontium titanate (Ba). x Sr (1-x) Oxides with high dielectric constants, such as TiO3, silicon dioxide (SiO2), aluminum oxide (Al2O3), and tantalum oxide (Ta2O5), are used. These oxides also possess good crystallinity and lattice structure, which, after crystallization, can improve the compactness of the formed inorganic dielectric film, further enhancing its barrier properties. Preferably, the inorganic dielectric film is one or both of barium strontium titanate and aluminum oxide films. The preferred barium strontium titanate and aluminum oxide films have relatively high dielectric strength and dielectric constant, good transparency, and excellent barrier properties, which helps to improve the dielectric and barrier properties of the dielectric layer in the composite dielectric film structure.
[0028] Furthermore, the dielectric constant of inorganic dielectric films ranges from 5.5 to 265. Compared to organic dielectric materials, inorganic dielectric materials often have higher dielectric constants and dielectric strengths. Therefore, the dielectric properties of the dielectric layer in a composite dielectric film structure are mainly determined by the dielectric properties of the inorganic dielectric film. At the same time, the wider range of dielectric constants of inorganic dielectric films endows the dielectric layer with high and tunable dielectric constants, meeting more application requirements for electrowetting lenses.
[0029] In this application, the organic dielectric film is a dense organic dielectric film with good protective and sealing properties. The organic dielectric film can be one or a combination of two or more of the following: a pyrene C film, a polyimide film, or a photoresist film. Pyrene C, polyimide, and photoresist are all organic dielectric materials with good dielectric properties. Pyrene C is a protective polymer material; its molecular penetrating power allows it to form a high-quality protective layer inside and around the device, which is more conducive to the stability of device performance. Polyimide, as one of the organic polymer materials with the best overall performance, belongs to organic materials with high dielectric constant and extremely low dielectric loss. Its high temperature resistance reaches 400℃, which is beneficial to the temperature resistance and performance stability of the device. Photoresist is a key material commonly used in the fabrication of semiconductors and integrated circuits. Through simple processes such as spin coating, exposure, development, and resist removal, the patterning requirements of the dielectric layer can be achieved.
[0030] This application utilizes composite organic dielectric films, which facilitates the extension of the diffusion path for ion penetration and improves the barrier properties of the dielectric layer. Perelin C films, polyimide films, and photoresist films can all be used as organic dielectric films; preferably, the organic dielectric film is a Perelin C film. Compared to other organic dielectric films, Perelin C films offer superior barrier properties, making it more advantageous for obtaining a dielectric layer with high density and dielectric constant. While polyimide and photoresist films can be prepared simply by spin-coating, to leverage the high penetrability of Perelin C molecules and achieve high barrier properties, Perelin C films require vacuum vapor deposition. This application also provides a vacuum vapor deposition method for preparing Perelin C films to further enhance barrier properties.
[0031] Furthermore, the dielectric constant of organic dielectric films ranges from 2.95 to 4.1. Perylene C is a superior organic dielectric material, with relatively higher dielectric constant and dielectric strength than typical organic dielectric materials, exhibiting excellent barrier properties. The dielectric constant range for organic dielectric films is primarily proposed specifically for Perylene C films.
[0032] The dielectric constant of the dielectric layer used for electrowetting lenses in this application can be 2.95-265, for example, 2.95, 3.15, 4.1, 4.5, 5.5, 8.5, 18.5, 27.5, 225, etc., but is not limited to the listed values; other unlisted values within this range are also applicable. Because it is a composite multilayer dielectric film structure, its dielectric constant has a wider range of adjustable characteristics.
[0033] Furthermore, the dielectric layer for electrowetting the lens comprises at least two inorganic dielectric films and at least one organic dielectric film, wherein the organic dielectric film is located between the two inorganic dielectric films. By placing the organic dielectric film between the two inorganic dielectric films, the organic dielectric film, which has good adhesion, can improve the bonding between the dielectric films and further enhance the barrier properties of the dielectric layer.
[0034] Furthermore, the dielectric layer used for electrowetting the lens employs one or a combination of two of the following: barium strontium titanate film or alumina film, as the inorganic dielectric film, and a pyrene C film as the organic dielectric film, thus creating a composite organic and inorganic dielectric layer. Inorganic dielectric films can effectively improve the dielectric constant and barrier properties of the dielectric layer, but the prepared inorganic dielectric films inevitably contain some porosity and grain boundaries. In the preparation of pyrene C films, the active molecules of pyrene C have excellent penetrating power, allowing them to penetrate into finer gaps. Through in-situ polymerization, pyrene C films are formed, filling unavoidable morphological defects in the process, further improving the barrier properties of the dielectric layer, and forming a high-quality, pinhole-free protective layer on the surface of the inorganic dielectric film. Simultaneously, the inorganic dielectric film also enhances the barrier properties of the organic dielectric film formed from pyrene C.
[0035] Furthermore, the dielectric layer used for electrowetting the lens comprises, from bottom to top, an alumina film, a Pyrelin C film, and another alumina film; the Pyrelin C film is located between the two alumina films. In practical applications, the two alumina films are prepared using chemical vapor deposition (CVD) and solution deposition, respectively. The alumina film closer to the lens cavity is prepared using CVD, while the alumina film further away from the lens cavity is prepared using solution deposition. Compared to the liquid phase method, the alumina film on the substrate surface prepared using CVD results in a tighter bond with the substrate, higher density, and better barrier properties. The preparation of the Pyrelin C film is more stringent, requiring vacuum deposition. In this process, the penetrating power of its molecules forms a high-quality protective layer on the previous alumina film. Considering the need to ensure the integrity of the Pyrelin C film when preparing an alumina film on top of it, the solution deposition method, which has lower processing temperature requirements, is chosen. Compared to a single-layer structure, this application achieves improved barrier properties through the construction of a multi-layer structure. Compared to the inorganic dielectric film + Pyrelin C film structure, the combination of inorganic dielectric film + Pyrelin C film + alumina film has better UV resistance and barrier properties. This is because the alumina film can absorb ultraviolet light, reducing the damage of ultraviolet light to other materials and broadening the application of this dielectric layer structure in scenarios requiring long-term UV stability. Due to the better density of the alumina film, the barrier properties of the barium strontium titanate + Pyrelin C + alumina film combination are slightly lower than those of the alumina + Pyrelin C + alumina film combination.
[0036] Furthermore, the dielectric layer used for electrowetting the lens comprises, from bottom to top, a barium strontium titanate film, a Pyrelin C film, and an alumina film; the Pyrelin C film is located between the barium strontium titanate film and the alumina film, and in actual use, the alumina film is located on the side furthest from the lens cavity. Barium strontium titanate has extremely high dielectric constant and high dielectric strength. The higher the dielectric constant of the dielectric layer material, the lower the required driving voltage and the lower the corresponding energy consumption. Furthermore, due to the special dielectric properties and low dielectric loss of barium strontium titanate, the breakdown voltage of the dielectric layer can be further improved. Placing the barium strontium titanate film closer to the lens cavity can improve the working performance of the dielectric layer. During lens use, light passes through from the side furthest from the lens cavity. The alumina film has ultraviolet absorption capabilities, which also helps improve the UV aging resistance of the Pyrelin C film, thus improving the UV aging resistance of the dielectric layer, solving the problem of poor UV aging resistance of the Pyrelin C film, and extending the service life of the electrowetting lens. The interlayer Parylene C film also possesses good light transmittance and low refractive index. Under the protection of the alumina film, it can maintain its optical properties for a longer period of time, reducing interference and improving the optical performance of the electrowetting lens. This combination of dielectric layers exhibits good overall performance, effectively improving the working performance and lifespan of the electrowetting lens.
[0037] In this application, the dielectric layer is prepared from bottom to top. The first inorganic alumina / barium strontium titanate film is prepared by chemical vapor deposition, which has good density, strong dielectric properties, and the processing conditions are relatively friendly to glass substrates with ITO. The second organic pyrene C film can form a further barrier protection for the first inorganic film and repair any defects that may exist. The third alumina film prepared by solution method has good ultraviolet absorption capacity, which makes up for the defect of the second pyrene C film in terms of ultraviolet resistance. At the same time, the multi-layer diffusion path formed is more conducive to improving the barrier properties of the dielectric layer.
[0038] Furthermore, the electrowetting lens includes a lens cavity, which is constructed from an organic or inorganic glass cavity. The lens cavity is fabricated using the following methods: Method 1: For organic materials. Step 1: Prepare the mold. First, in... <100> A silicon nitride thin film is grown on a silicon wafer and photolithography is performed. The silicon nitride is then removed, followed by KOH silicon etching to create a silicon master mold with a 54.7° bevel angle. A nickel mold is then fabricated using an electroplated silicon master mold. The nickel mold has the opposite shape to the silicon mold. The nickel mold possesses sufficient strength to withstand high temperatures and pressures, which is beneficial for the subsequent imprinting process. The second step involves fabricating the cavity. An organic material cavity is prepared using a polymer material such as polymethyl methacrylate (PMMA) or polycarbonate (PC) through a hot-press imprinting process.
[0039] Method 2: For inorganic materials. A transparent glass concave cavity is fabricated using laser processing (femtosecond laser processing technology). Any one of the following substrates can be used: sodium-calcium based glass, borosilicate based glass, alkali-free glass, borosilicate glass, potassium aluminum silicate glass, or sodium silicate glass. A glass cavity with an internal bevel angle of 54.7° is obtained.
[0040] In this application, considering temperature resistance, it is preferred to use an inorganic glass cavity to form the lens cavity.
[0041] In this application, the preferred dielectric layer combination, from bottom to top, is an inorganic dielectric film + an organic dielectric film + an inorganic dielectric film. From the perspective of diffusion paths, the more composite layers there are, the better the barrier properties. However, infinite composites make it very difficult to control the process of single-layer films with low thickness. Moreover, after multiple composites, the structure of the dielectric layer will form a state similar to the mutual doping of organic and inorganic particles. This raises questions about the uniformity of particle mixing and whether there will be pores in the middle. Furthermore, after the dielectric layer is doped, it is difficult to utilize the characteristics of each film, and the dielectric and barrier properties may deteriorate.
[0042] Furthermore, the thickness ratio of the inorganic dielectric film to the organic dielectric film is from 1:10 to 10:1, and the total thickness of the dielectric layer used for electrowetting the lens ranges from 100 nm to 2 μm. Here, the thickness ratio refers to the ratio between the thicknesses of all inorganic dielectric films and all organic dielectric films. If the thickness of the inorganic dielectric film layer is too low, the overall dielectric properties of the dielectric layer will be low, and the barrier properties of the third inorganic dielectric film will be poor. If the thickness of the organic layer is too low, in addition to increasing the processing difficulty, it will also be impossible to form a good transition between the two inorganic dielectric films, resulting in poor barrier properties. Preferably, in this application, the thickness ratio of the inorganic dielectric film to the organic dielectric film is preferably 1:5 to 2:1, the total thickness of the dielectric layer is preferably 1 μm, the thickness of each inorganic dielectric film layer is preferably 0.08 to 0.33 μm, and the thickness of each organic dielectric film layer is preferably 0.33 to 0.83 μm. Within this preferred thickness range, combined with the different preparation processes of each dielectric film in this application, it can be ensured that different dielectric films can effectively exert their respective characteristics, thereby forming a dielectric layer with good overall performance.
[0043] Furthermore, the inorganic dielectric films were prepared using chemical vapor deposition (CVD) or solution methods. More specifically, the inorganic dielectric film located near the lens cavity was prepared using CVD, while the inorganic dielectric film located away from the lens cavity was prepared using solution methods. CVD can produce denser inorganic dielectric films with a compact structure, strong adhesion, and high dielectric constant, reducing grain boundaries or pores and thus improving the dielectric properties and barrier properties of the inorganic dielectric film. Solution methods, on the other hand, allow for control of the specific surface area of the prepared film by adjusting the grain size, thereby affecting its UV absorption. This method is also more accurate and convenient for preparing solid solution inorganic dielectric films with different compositions, such as barium strontium titanate (B). X Sr 1-X In the solution-based preparation of inorganic thin films, the proportion of inorganic dielectric material increases for the other two layers, resulting in stronger dielectric properties.
[0044] Specifically, taking alumina thin films as an example, the process of preparing alumina thin films by chemical vapor deposition includes the following steps: Trimethylaluminum (TMA) was used as a precursor. High-purity argon gas carried the monomer TMA into the reaction chamber, where it underwent a chemical adsorption reaction on the substrate surface for 4 seconds. Excess monomer was then purged with argon gas for 10 seconds. Oxygen gas was introduced into the deposition chamber, and the deposition time was 8 seconds. The reaction chamber temperature was set at 150°C and the process pressure at 0.2 torr. The oxygen and the previously adsorbed TMA monomer underwent an oxygen plasma chemical reaction to generate an alumina film. Excess oxygen and reaction byproducts were then purged with argon gas for 10 seconds. Finally, the alumina film was annealed at 400°C.
[0045] Taking barium strontium titanate thin films as an example, the process of preparing barium strontium titanate thin films by chemical vapor deposition includes the following steps: Will Ba(C 11 H 20 O2)2(C9H 23 N3)(C4H6N2) and Sr2(C 11 H 20 The precursor O2)4(C3H4N2)2(C2H6O) was placed in a quartz boat at the inlet of the reactor pipe and evaporated at 140℃ and 170℃ respectively. Tetraisopropyl titanate (C 12 H 28 The O4Ti precursor is heated to 45°C in an evaporator tube and carried into the reactor by a nitrogen gas flow. At 450°C, a barium strontium titanate film is polymerized and deposited on the surface of a glass cavity with ITO.
[0046] In this application, the dielectric layer is composed of an organic dielectric film and an inorganic dielectric film, wherein the organic dielectric film is preferably a pyrene C film. However, since the vaporization temperature of pyrene C film is around 150°C, chemical vapor deposition (CVD), which requires a higher substrate temperature, is not suitable for preparing inorganic dielectric films on the surface of pyrene C film. To address this issue, this application provides an optimized solution method for preparing inorganic dielectric films on the surface of pyrene C film. The solution method has lower substrate temperature requirements and can effectively control and reduce grain boundaries or pores in the film, thereby controlling the dielectric properties and barrier properties of the film.
[0047] In this application, when inorganic dielectric films are prepared using a solution method, this method mainly combines hydrothermal processing and sol-gel technology. Sol-gel technology is a commonly used process for preparing inorganic films, but research combining hydrothermal processing and sol-gel technology is relatively rare. Specifically, this application uses a hydrothermal process to regulate the inorganic dielectric nanoparticles (including nanoparticle size and dispersion), and then uses a sol-gel process to achieve uniform arrangement of nanocrystals along a specific direction, obtaining a nearly pore-free film. A key feature of the process provided in this application is its low requirement for the temperature resistance of the substrate on which the inorganic dielectric film is grown, thus broadening the application of dielectric layer fabrication.
[0048] Specifically, when inorganic dielectric films are prepared using a solution method, the preparation method includes the following steps: (1) The inorganic dielectric material is dissolved in the first solvent to prepare a solution. A mineralizing agent is added dropwise to the solution and stirred to obtain a suspension. The suspension is transferred to a high-pressure hydrothermal reactor and heated and stirred until the reaction is complete. After cooling to room temperature, a precipitate is obtained. The precipitate is washed by centrifugation with ethanol and deionized water to obtain inorganic dielectric nanoparticles. Inorganic dielectric nanoparticles with high purity, controllable particle size, and good dispersibility can be obtained by hydrothermal method. The particle size of the prepared inorganic dielectric nanoparticles can be 5-100 nm. The first solvent can be one of the following: deionized water, anhydrous ethanol, methanol, acetonitrile, ethylene glycol, n-propanol, glacial acetic acid, and ethylene glycol methyl ether. The concentration range of the inorganic dielectric material in the first solvent is 0.01-10 mol / L; The mineralizing agent can be one of sodium hydroxide (NaOH), potassium hydroxide (KOH), tetramethylammonium hydroxide (TMAH), ammonia, and urea; the concentration of the mineralizing agent in the first solvent is in the range of 0.5-15 mol / L. The heating and stirring temperature range is 80-250℃, and the heating and stirring time range is 2-72h. During the heating and stirring process, a reaction occurs, and once the reaction is complete, an inorganic dielectric nanoparticle solution can be obtained.
[0049] In this application, inorganic dielectric nanoparticles with a particle size of 5-100 nm are first prepared by hydrothermal method. The small particle size of the inorganic dielectric nanoparticles prepared by this method helps to oriented the particles, reduces the existence of pores between particles, and is conducive to the formation of high-quality inorganic dielectric films.
[0050] (2) Disperse the inorganic dielectric nanoparticles in the second solvent, add a surfactant, and stir until a stable inorganic dielectric nanoparticle sol is formed; The second solvent is one or both of ethanol and methanol; ethanol and methanol can be used in combination or alone. The surfactant can be one of polyvinylpyrrolidone, oleic acid, tert-butylamine, polyvinyl alcohol (PVA), ethanolamine, and hexadecyltrimethylammonium bromide (CTAB); the concentration of the surfactant in the second solvent ranges from 0.1 to 10 g / L. The concentration of inorganic dielectric nanoparticles in the second solvent ranges from 0.001 to 10 mol / L, ensuring uniform dispersion of the inorganic dielectric nanoparticles.
[0051] (3) The inorganic dielectric nanoparticle sol is coated on the substrate, and then subjected to low-temperature heat treatment in a vacuum atmosphere and dried to obtain inorganic dielectric nanoparticle gel. The inorganic dielectric nanoparticle gel is then sintered at low temperature to obtain an inorganic dielectric film. The coating method can be either spin coating or dip coating, so that the inorganic dielectric nanoparticle sol is uniformly distributed on the substrate surface. The temperature range of the low-temperature heat treatment is 80-350℃, preferably 80-150℃, and the inorganic dielectric nanoparticle sol is dried to form a hard inorganic dielectric nanoparticle gel. The low-temperature sintering temperature range is 80-140℃, which allows the inorganic dielectric nanoparticle gel to form a dense inorganic dielectric film and remove residual solvent.
[0052] This application employs a hydrothermal method combined with a sol-gel process, enabling the preparation of inorganic dielectric thin films at relatively low temperatures (80-350℃). This method has low temperature requirements on the substrate and allows for effective control of the film's porosity and grain boundaries through process adjustments. The specific temperature can be determined based on the film's performance requirements and process specifications; adjusting the temperature allows for the regulation of the film's properties.
[0053] Taking the preparation of alumina thin films as an example, the specific steps include: (1) Dissolve the aluminum source in the first solvent to prepare a solution, add the mineralizing agent dropwise to the solution, stir to obtain a suspension, transfer the suspension to a 50mL high-pressure hydrothermal reactor with a polytetrafluoroethylene liner, heat and stir until the reaction is complete, cool to room temperature to obtain a precipitate, wash the precipitate with ethanol and deionized water at 8000r / min 3 to 5 times to obtain alumina nanoparticles; the particle size of the alumina nanoparticles is 5-100nm; The aluminum source can be one of aluminum nitrate (Al(NO3)3·9H2O), aluminum sulfate (Al2(SO4)3·18H2O), aluminum isopropoxide (Al(C3H7O)3), and aluminum chloride (AlCl3·6H2O). The concentration of the aluminum source in the first solvent ranges from 0.01 to 10 mol / L.
[0054] (2) Disperse alumina nanoparticles in ethanol solvent, add surfactant, and stir until a stable alumina nanoparticle sol is formed.
[0055] (3) Alumina nanoparticle sol is coated on the substrate and placed in a vacuum drying oven for low-temperature heat treatment. The low-temperature heat treatment temperature is 80-350℃, preferably 80-150℃. After drying, alumina nanoparticle gel is obtained. The alumina nanoparticle gel is sintered at a low temperature of 80-140℃. After low-temperature sintering, an alumina film is obtained.
[0056] Taking the preparation of barium strontium titanate thin films as an example, the specific steps include: (1) The barium source, strontium source and titanium source are dissolved in the first solvent to prepare a solution. A mineralizing agent is added dropwise to the solution and stirred to obtain a suspension. The suspension is transferred to a 50mL high-pressure hydrothermal reactor with a polytetrafluoroethylene liner and heated and stirred until the reaction is complete. After cooling to room temperature, a precipitate is obtained. The precipitate is washed 3-5 times by centrifugation with ethanol and deionized water at 8000r / min to obtain barium strontium titanate nanoparticles. The particle size of the barium strontium titanate nanoparticles is 5-100nm. The barium source can be one of barium acetate (Ba(CH3COO)2) and barium hydroxide (Ba(OH)2·8H2O); The strontium source can be one of strontium acetate (Sr(CH3COO)2) and strontium nitrate (Sr(NO3)2); The titanium source can be one of tetrabutyl titanate (Ti(OC4H9)4) and titanium tetrachloride (TiCl4).
[0057] (2) Disperse barium strontium titanate nanoparticles in ethanol solvent, add surfactant, and stir until a stable alumina nanoparticle sol is formed.
[0058] (3) The sol of barium strontium titanate nanoparticles is coated on the substrate and placed in a vacuum drying oven for low-temperature heat treatment. The low-temperature heat treatment temperature is 80-350℃, preferably 80-150℃. After drying, barium strontium titanate nanoparticle gel is obtained. The barium strontium titanate nanoparticle gel is sintered at a low temperature of 80-140℃. After low-temperature sintering, barium strontium titanate film is obtained.
[0059] Furthermore, the Parylene C thin film was prepared using vacuum vapor deposition. This method mainly employs zoned temperature-controlled atomic layer deposition, which involves a transformation from solid to gas and then back to solid in a vacuum state. Specifically, it includes the following steps: (1) The solid dichloro-p-xylene dimer raw material is placed in the evaporation chamber and sublimated at 100-160℃, preferably 150℃, to produce dichloro-p-xylene dimer gas; Sublimation is carried out at 100-160℃, preferably 150℃. Sublimation at this temperature ensures film quality while reducing costs. This is because the melting / boiling point of the solid dichloro-p-xylene dimer raw material is 165-167℃ (MPa), and the sublimation temperature must be below the melting point of the sublimate; otherwise, it would not be a sublimation process but a liquefaction-revaporization process. If the temperature is too low, the sublimation rate is slow, the film formation time is long, and the deposited film is dense and non-porous, resulting in excellent protective effects. However, considering costs, the sublimation temperature is increased in actual production to increase the sublimation rate. But if sublimation is too fast, the second-stage pyrolysis will not keep up, resulting in incomplete pyrolysis. That is, the molecular bonds connecting the dichloro-p-xylene dimer are not broken, and 2-chloro-p-xylene monomers are not formed. When this state of gas enters the deposition zone, the resulting film is no longer a transparent Pyrelin C film, but rather a film layer filled with dense white particles. This type of membrane has poor density and low protective performance, and cannot meet the requirements of practical applications.
[0060] (2) When the dichloro-p-xylene dimer gas enters the pyrolysis chamber, at a temperature of 600-720°C, preferably 680°C, the molecular bonds of the dichloro-p-xylene dimer molecule are broken, generating active 2-chloro-p-xylene monomer molecules with free radicals.
[0061] If the temperature is below 600℃, the pyrolysis temperature is too low, resulting in incomplete pyrolysis. The C-C bonds between the two methylene groups linking the benzene ring in the dichloro-p-xylene dimer cannot be broken, preventing pyrolysis. The unpyrolyzed gaseous feedstock lacks active sites and cannot polymerize with the active monomer to form a film. However, if the temperature is above 720℃, the pyrolysis temperature is too high, leading to excessive pyrolysis of the gaseous feedstock. This causes the C-Cl bonds on the benzene ring to break, producing gaseous chlorine atoms and a p-xylene active monomer containing three active sites, resulting in additional cross-linking during film formation.
[0062] (3) Active 2-chloro-p-xylene monomer molecules are sent into a vacuum deposition chamber at room temperature (25°C) to polymerize and deposit on the substrate surface to obtain a P-reilin C film.
[0063] Phyllanthus C films can be prepared by vacuum vapor deposition, resulting in pure, uniform, transparent films with good adhesion, excellent barrier properties, and controllable thickness. A unique vacuum vapor deposition process is employed to prepare Phyllanthus C films by using active small molecules to coat any gaps or grain boundaries that may exist in the previous inorganic dielectric film on the substrate surface, further enhancing the barrier properties of the former.
[0064] This application also provides an electrowetting lens, which includes the dielectric layer for electrowetting lenses as described above. By incorporating the dielectric layer for electrowetting lenses provided in this application, the electrowetting lens possesses the characteristics of high and adjustable dielectric constant. While increasing the breakdown voltage of the dielectric layer, it reduces the driving voltage of the electrowetting lens, resulting in advantages such as low driving voltage, high breakdown voltage, and good stability, thus greatly improving the working performance of the electrowetting lens.
[0065] Furthermore, the inner diameter of the glass cavity in the electrowetting lens can be 0.3-5 mm, the height can be 0.1-5 mm, and the dielectric constant of the dielectric layer in the electrowetting lens is 2.95-265.
[0066] The electrowetting lens is an existing structure. A glass cavity 1 with an internal bevel angle of 54.7° is fabricated using laser processing (femtosecond laser processing technology). This laser processing technology is existing technology and will not be described further here. In the specific embodiments and comparative examples of this application, the structure of the electrowetting lens used is as follows: Figure 4 As shown, specifically, it includes a transparent glass cavity 1, and from bottom to top, the glass cavity 1 includes a lower electrode 2, a dielectric layer 3, a hydrophobic layer 4, a sealant layer 5, an upper electrode 6, and a transparent top cover 7. Conductive liquid 8 and insulating liquid 9 are encapsulated inside the glass cavity 1.
[0067] This application also provides a method for preparing the electrowetting lens as described above, specifically including the following steps: The upper electrode is connected to the metal cylindrical outer shell; The lower electrode is coated onto the sidewall of the glass cavity using vacuum sputtering, and then connected to the metal cylindrical shell to form a connector. Inorganic dielectric thin films are prepared using chemical vapor deposition or solution methods. Organic dielectric thin films were prepared by vacuum phase deposition. Inorganic dielectric films and organic dielectric films constitute the dielectric layer; A hydrophobic material is coated onto a dielectric layer using a drop-coating method and then cured to form a hydrophobic layer. The conductive liquid and the insulating liquid are injected sequentially into the connector. Assemble the transparent top cover onto the top of the aforementioned connector, and seal the entire device with sealant to form a sealant layer. The sealing process is carried out in a water bath to prevent air bubbles from forming in the chamber.
[0068] Connect the lower electrode and the upper electrode to the two poles of the AC power supply, respectively.
[0069] Compared with the prior art, the dielectric layer for electrowetting lenses provided by the present invention has the following advantages: The provided dielectric layer is a composite dielectric film structure. By combining two or more organic and inorganic dielectric films with different barrier properties, the diffusion path of ion penetration is extended by utilizing the composite system. This results in a dielectric layer with high barrier properties and a protective barrier function, thereby avoiding possible erosion caused by ion penetration and improving the service life of the electrowetting lens.
[0070] The electrowetting lens provided in this application has good interlayer bonding of the dielectric layer. The inorganic dielectric film provides high dielectric properties and makes the dielectric properties of the dielectric layer tunable, while the organic dielectric film provides excellent protection without pinholes. This results in a composite dielectric layer with good density and barrier properties, which helps to improve the breakdown voltage of the dielectric layer and reduce the driving voltage of the electrowetting lens. The composite dielectric layer has high dielectric properties, and the dielectric properties of the dielectric layer used in the electrowetting lens can be controlled by combining inorganic and organic dielectric films with different dielectric properties. This broadens the application of the dielectric layer in electrowetting lenses and enables the applied electrowetting lens to have good working performance, which can meet the further application requirements of electrowetting lenses.
[0071] The present invention will be further illustrated by specific embodiments below.
[0072] The electrowetting lens structures prepared in the following embodiments and comparative examples are as follows: Figure 4 As shown, specifically, it includes a transparent glass cavity 1, and from bottom to top, the glass cavity 1 includes a lower electrode 2, a dielectric layer 3, a hydrophobic layer 4, a sealant layer 5, an upper electrode 6, and a transparent top cover 7. Conductive liquid 8 and insulating liquid 9 are encapsulated inside the glass cavity 1.
[0073] Example 1 Alumina film was selected as the inorganic dielectric film, and pyrene C film was selected as the organic dielectric film. The dielectric layer structure for electrowetting lenses was prepared by combining alumina film and pyrene C film in a 1:4 thickness ratio.
[0074] The upper electrode is a metal electrode, which is connected to a metal cylindrical shell with an inner diameter of 0.6 mm and a height of 0.5 mm. The lower electrode is a transparent electrode, ITO (tin oxide), which is coated onto the side wall of a transparent glass cavity with an inner diameter of 0.4 mm and a height of 0.3 mm by vacuum sputtering, and then connected to the metal cylindrical shell. An aluminum oxide film is prepared on the surface of the glass cavity with ITO by chemical vapor deposition. A Pyrelin C film is prepared on the surface of the aluminum oxide film by vacuum vapor deposition. A hydrophobic material, Teflon AF1600, is coated onto the Pyrelin C film by drop casting and cured to form a hydrophobic layer. Conductive NaCl ionic liquid and silicone oil insulating liquid are injected into the above connector sequentially. The sealing process is carried out in a water bath to prevent air bubbles from forming in the chamber. An ITO glass is used as a transparent top cover and assembled on the top of the connector. The entire device is sealed with UV adhesive (NOA81) to form a sealing layer. By connecting the transparent ITO electrode and the metal electrode to the two poles of an AC power source, an electrowetting lens is obtained in which the dielectric layer is composed of an alumina film and a Pyrelin C film in sequence from bottom to top.
[0075] The specific process for forming the alumina thin film is as follows: Trimethylaluminum (TMA) was used as a precursor. High-purity argon gas carried the monomer TMA into the reaction chamber, where it underwent a chemical adsorption reaction on the substrate surface for 4 seconds. Excess monomer was then purged with argon gas for 10 seconds. Oxygen gas was introduced into the deposition chamber, and the deposition time was 8 seconds. The reaction chamber temperature was set at 150°C and the process pressure at 0.2 torr. The oxygen and the previously adsorbed TMA monomer underwent an oxygen plasma chemical reaction to generate an alumina film. Excess oxygen and reaction byproducts were then purged with argon gas for 10 seconds. Finally, the alumina film was annealed at 400°C.
[0076] The specific process for forming the Parylene C thin film is as follows: (1) The solid dichloro-p-xylene dimer raw material is placed in the evaporation chamber and sublimated at 150°C to produce dichloro-p-xylene dimer gas; (2) The dichloro-p-xylene dimer gas is introduced into the pyrolysis chamber. At a temperature of about 680°C, the molecular bonds of the dichloro-p-xylene dimer molecules are broken, producing active 2-chloro-p-xylene monomer molecules. (3) Active 2-chloro-p-xylene monomer molecules are sent into a vacuum deposition chamber at room temperature to polymerize and deposit on the surface of alumina film to form a P-reilin C film.
[0077] Scanning electron microscope (SEM) image of the alumina thin film prepared by chemical vapor deposition in Example 1 is shown below. Figure 1a and Figure 1bAs shown, the alumina film prepared by chemical vapor deposition (CVD) bonds more tightly to the ITO-containing glass cavity, exhibits better crystallinity, a smoother film surface, good morphology, and excellent density and barrier properties. Furthermore, the addition of a layer of phenelzine C film utilizes the penetrating power of monomer molecules to form a high-quality, pinhole-free protective layer on its surface. This improves the dielectric properties of the dielectric layer, while the increased diffusion pathways contribute to enhanced barrier properties.
[0078] A voltage was applied to the packaged electrowetting lens, and its refractive power was tested. The test results are as follows: Figure 5 As shown, refractive power was measured for every 5V increase. With a 1µm dielectric layer (0.2µm alumina film + 0.8µm pyrene C film), a refractive power of 1600D was obtained at 80V, and dielectric breakdown that caused the bubble formation occurred at 120V.
[0079] Example 2 Strontium barium titanate film was selected as the inorganic dielectric film, and pyrene C film was selected as the organic dielectric film. The dielectric layer structure for electrowetting lenses was prepared by composite of strontium barium titanate film and pyrene C film at a thickness ratio of 1:4.
[0080] The upper electrode is a metal electrode, connected to a metal cylindrical shell with an inner diameter of 0.6 mm and a height of 0.5 mm. The lower electrode is a transparent ITO electrode, coated onto the sidewall of a transparent glass cavity with an inner diameter of 0.4 mm and a height of 0.3 mm using vacuum sputtering, and then connected to the metal cylindrical shell. A barium strontium titanate film is deposited on the surface of the glass cavity with ITO using chemical vapor deposition, wherein the molar ratio of Ba:Sr:Ti precursors is 1:1:4. A Pyrelin C film is prepared on the surface of the barium strontium titanate film using vacuum vapor deposition. A hydrophobic material, Teflon, is then applied using a drop-coating method. AF1600 was coated onto a Parylene C film and cured to form a hydrophobic layer. Conductive NaCl ionic liquid and silicone oil insulating liquid were sequentially injected into the connector. The sealing process was carried out in a water bath to prevent air bubbles from forming in the chamber. ITO glass was used as a transparent top cover and assembled onto the top of the connector. The entire device was then sealed with UV adhesive (NOA81) to form a sealant layer. The transparent ITO electrode and the metal electrode were connected to the two poles of an AC power supply, respectively, to obtain an electrowetting lens with a dielectric layer consisting of a barium strontium titanate film and a Parylene C film sequentially composited from bottom to top.
[0081] The specific process for forming the barium strontium titanate thin film is as follows: Will Ba(C 11 H 20 O2)2(C9H 23 N3)(C4H6N2) and Sr2(C 11 H 20O2)4(C3H4N2)2(C2H6O) powder was placed in a quartz boat and positioned at the inlet of the reactor pipe, and evaporated at 140℃ and 170℃ respectively. Tetraisopropyl titanate (C 12 H 28 The O4Ti precursor is heated to 45°C in an evaporator tube and introduced into the reactor via a nitrogen stream. At 450°C, a barium strontium titanate film is polymerized and deposited on the surface of a glass cavity containing ITO. The molar ratio of the precursor is Ba:Sr:Ti = 1:1:4.
[0082] The specific process for forming the Parylene C thin film is as follows: (1) The solid dichloro-p-xylene dimer raw material is placed in the evaporation chamber and sublimated at 150°C to produce dichloro-p-xylene dimer gas; (2) The dichloro-p-xylene dimer gas is introduced into the pyrolysis chamber. At a temperature of about 680°C, the molecular bonds of the dichloro-p-xylene dimer molecules are broken, producing active 2-chloro-p-xylene monomer molecules. (3) Active 2-chloro-p-xylene monomer molecules are sent into a vacuum deposition chamber at room temperature to polymerize and deposit on the surface of barium strontium titanate film to form a P-reilin C film.
[0083] A voltage was applied to the packaged electrowetting lens, and its refractive power was tested. The test results are as follows: Figure 5 As shown, refractive power was measured for every 5V increase. With a 1µm dielectric layer (0.2µm barium strontium titanate film + 0.8µm pyrene C film), a refractive power of 1600D was obtained at 75V, and the dielectric breakdown that caused the bubble formation occurred at 125V.
[0084] Example 3 Alumina film was selected as the inorganic dielectric film, and Pyrelin C film was selected as the organic dielectric film. The dielectric layer structure for electrowetting lenses was prepared by composite alumina film: Pyrelin C film: alumina film in a thickness ratio of 1:3:1.
[0085] The upper electrode is a metal electrode, which is connected to a metal cylindrical shell with an inner diameter of 0.6 mm and a height of 0.5 mm. The lower electrode is a transparent ITO electrode, which is coated onto the side wall of a transparent glass cavity with an inner diameter of 0.4 mm and a height of 0.3 mm by vacuum sputtering, and then connected to the metal cylindrical shell. A first layer of alumina film is prepared on the surface of the glass cavity with ITO by chemical vapor deposition. A Pyrelin C film is prepared on the surface of the first layer of alumina film by vacuum vapor deposition. A second layer of alumina film is prepared on the surface of the Pyrelin C film by solution deposition. A hydrophobic material Teflon AF1600 is coated onto the second layer of alumina film by drop casting and cured to form a hydrophobic layer. Conductive NaCl ionic liquid and silicone oil insulating liquid are injected into the above connector in sequence. The sealing process is carried out in a water bath to prevent air bubbles from forming in the chamber. ITO glass is used as a transparent top cover and assembled on the top of the connector. The entire device is sealed with UV adhesive (NOA81) to form a sealing layer. By connecting the transparent ITO electrode and the metal electrode to the two poles of an AC power supply, an electrowetting lens with a dielectric layer composite of two layers of alumina film and a Pyrelin C film is obtained, wherein the Pyrelin C film is located between the two layers of alumina film.
[0086] The specific process for forming the first layer of alumina film is as follows: Using trimethylaluminum as a precursor, high-purity argon gas carries the monomer trimethylaluminum into the reaction chamber, where it undergoes a chemical adsorption reaction on the substrate surface for 4 seconds. Excess monomer is then purged with argon gas for 10 seconds. Oxygen, an oxidizing gas, is introduced into the deposition chamber for 8 seconds. The reaction chamber temperature is set at 150°C, and the process pressure at 0.2 torr. The oxygen reacts with the previously adsorbed trimethylaluminum monomer in an oxygen plasma chemical reaction to generate an alumina film. Excess oxygen and reaction byproducts are then purged with argon gas for 10 seconds. Finally, the alumina film is annealed at 400°C.
[0087] The specific process for forming the Parylene C thin film is as follows: (1) The solid dichloro-p-xylene dimer raw material is placed in the evaporation chamber and sublimated at 150°C to generate dichloro-p-xylene dimer gas; (2) The dichloro-p-xylene dimer gas is sent into the pyrolysis chamber, and at a temperature of about 680°C, the molecular bonds of the dichloro-p-xylene dimer molecules are broken to generate active 2-chloro-p-xylene monomer molecules; (3) The active 2-chloro-p-xylene monomer molecules are sent into the vacuum deposition chamber at room temperature to polymerize and deposit on the surface of the first layer of alumina film to form a Pyrelin C film.
[0088] The specific process for forming the second layer of alumina film is as follows: (1) Dissolve 10.26g of aluminum sulfate powder in 16.5mL of deionized water, and then add 13.5mL of 25% ammonia water to the solution to prepare a 1mol / L colorless and transparent aluminum sulfate solution. The concentration of ammonia water mineralizer in the first solvent is 6mol / L. With stirring, a white suspension is obtained. Transfer the white suspension to a 50mL high-pressure hydrothermal reactor with a polytetrafluoroethylene liner, keep it at 200℃ for 24h, stir until the reaction is complete, and cool to room temperature to obtain a white powder precipitate. Wash it 5 times by centrifugation with ethanol and deionized water at 8000r / min. (2) Disperse 0.3g of white powder in 30mL of ethanol and add 0.18g of surfactant polyvinylpyrrolidone. Stir continuously to form a stable alumina nanoparticle sol. (3) Then coat the alumina nanoparticle sol onto the substrate and use the dip-coating method to make the sol evenly distributed on the substrate surface. The coated substrate is then placed in a vacuum drying oven and dried at 140°C to allow the sol to form a hard gel. Finally, the gel is sintered at a low temperature of approximately 140°C to form a dense alumina film.
[0089] The scanning electron microscope image of the alumina thin film prepared by solution method in Example 3 is shown below. Figure 2 As shown, the crystals on the surface of the thin film are densely packed, with good crystallinity and film compactness. Moreover, the alumina film prepared by solution method contains more nano-sized alumina particles, and the resulting surface morphology has a high specific surface area, which can more effectively absorb ultraviolet rays, effectively reduce the damage of ultraviolet rays to Piriton C, and extend the service life of the dielectric layer of the multilayer structure. Furthermore, the quality of the inorganic thin film can be further optimized by adjusting the process conditions.
[0090] A voltage was applied to the packaged electrowetting lens, and its refractive power was tested. The test results are as follows: Figure 5 As shown, refractive power was measured for every 5V increase. With a 1µm dielectric layer (0.2µm alumina film + 0.6µm pyrene C film + 0.2µm alumina film), a refractive power of 1600D was obtained at 75V, and the dielectric breakdown that caused the bubble formation occurred at 130V.
[0091] Example 4 Strontium barium titanate film and alumina film were selected as the inorganic dielectric film, and Pyrelin C film was selected as the organic dielectric film. A dielectric layer structure for electrowetting lenses was prepared by compositeting Strontium barium titanate film, Pyrelin C film, and alumina film in a thickness ratio of 1:3:1. The specific structure is shown below. Figure 3 As shown, it includes a lower electrode 2, a dielectric layer 3 (including a barium strontium titanate film 31, a pyrene C film 32, and an alumina film 33) and a hydrophobic layer 4.
[0092] The upper electrode is a metal electrode, connected to a metal cylindrical shell with an inner diameter of 0.6 mm and a height of 0.5 mm. The lower electrode is a transparent ITO electrode, coated onto the sidewall of a transparent glass cavity with an inner diameter of 0.4 mm and a height of 0.3 mm using vacuum sputtering, and then connected to the metal cylindrical shell. A barium strontium titanate film is deposited on the surface of the glass cavity with ITO using chemical vapor deposition, with a Ba:Sr:Ti precursor molar ratio of 1:1:4. A Pyrelin C film is prepared on the surface of the barium strontium titanate film using vacuum vapor deposition. An alumina film is prepared on the surface of the Pyrelin C film using a solution method. A hydrophobic material, Teflon, is then applied using a drop-coating method. AF1600 was coated onto an alumina film and cured to form a hydrophobic layer. Conductive NaCl ionic liquid and silicone oil insulating liquid were then injected sequentially into the connector. The sealing process was carried out in a water bath to prevent air bubbles from forming in the chamber. ITO glass was used as a transparent top cover and assembled onto the top of the connector. The entire device was then sealed with UV adhesive (NOA81) to form a sealant layer. The transparent ITO electrode and the metal electrode were connected to the two poles of an AC power supply, respectively, to obtain an electrowetting lens with dielectric layers consisting of a barium strontium titanate film, a Pyrelin C film, and an alumina film, layered sequentially from bottom to top.
[0093] The specific process for forming the barium strontium titanate thin film is as follows: Will Ba(C 11 H 20 O2)2(C9H 23 N3)(C4H6N2) and Sr2(C 11 H 20 O2)4(C3H4N2)2(C2H6O) powder was placed in a quartz boat and positioned at the inlet of the reactor pipe, and evaporated at 140℃ and 170℃ respectively. Tetraisopropyl titanate (C 12 H 28 The O4Ti precursor is heated to 45°C in an evaporator tube and introduced into the reactor via a nitrogen stream. At 450°C, a barium strontium titanate film is polymerized and deposited on the surface of a glass cavity containing ITO. The molar ratio of the precursor is Ba:Sr:Ti = 1:1:4.
[0094] The specific process for forming the Parylene C thin film is as follows: (1) Solid dichloro-p-xylene dimer is placed in an evaporation chamber and sublimated at 150°C to produce dichloro-p-xylene dimer gas; (2) Dichloro-p-xylene dimer gas is sent into a pyrolysis chamber, and at a temperature of about 680°C, the molecular bonds of dichloro-p-xylene dimer molecules are broken to produce active 2-chloro-p-xylene monomer molecules; (3) Active 2-chloro-p-xylene monomer molecules are sent into a vacuum deposition chamber at room temperature to polymerize and deposit on the surface of barium strontium titanate film to form a P-reilin C film.
[0095] The specific process for forming an alumina thin film is as follows: (1) Dissolve 10.26g of aluminum sulfate powder in 16.5mL of deionized water, and then add 13.5mL of 25% ammonia water to the solution to prepare a 1mol / L colorless and transparent aluminum sulfate solution. The concentration of the mineralizing agent ammonia water in the first solvent is 6mol / L. With stirring, a white suspension is obtained. Transfer the white suspension to a 50mL high-pressure hydrothermal reactor with a polytetrafluoroethylene liner, keep it at 200℃ for 24h, stir until the reaction is complete, and cool to room temperature to obtain a white powder precipitate. Wash it 5 times by centrifugation with ethanol and deionized water at 8000r / min. (2) Disperse 0.3g of white powder in 30mL of ethanol, and add 0.18g of surfactant polyvinylpyrrolidone. Stir continuously to form a stable alumina nanoparticle sol. (3) Then coat the alumina nanoparticle sol onto the substrate and use the dip-coating method to make the sol evenly distributed on the substrate surface. The coated substrate is then placed in a vacuum drying oven and dried at 140°C to allow the sol to form a hard gel. Finally, the gel is sintered at a low temperature of approximately 140°C to form a dense alumina film.
[0096] A voltage was applied to the packaged electrowetting lens, and its refractive power was tested. The test results are as follows: Figure 5 As shown, refractive power was measured for every 5V increase. With a 1µm dielectric layer (0.2µm barium strontium titanate film + 0.6µm pyrene C film + 0.2µm alumina film), a refractive power of 1600D was obtained at 70V, and the dielectric breakdown that caused the bubble formation occurred at 135V.
[0097] Comparative Example 1 In comparison, a 1µm monolayer Pyrelin C film was selected as the dielectric layer and prepared using the same vacuum phase deposition method as in the above embodiments. An electrowetting lens was fabricated using the same method as in the above embodiments, and the test results are as follows. Figure 5 As shown, diopter was measured for every 5V increase. With only a 1µm monolayer of Pyrelin C dielectric layer, a diopter of 1600D was obtained at 85V, and dielectric breakdown leading to bubble formation occurred at 95V.
[0098] Comparative Example 2 In comparison, a 1µm monolayer alumina film was selected as the dielectric layer and prepared using the same chemical vapor deposition method as in the above embodiments. An electrowetting lens was fabricated using the same method as in the above embodiments, and the test results are as follows. Figure 5 As shown, refractive power was measured for every 5V increase. With only a 1µm monolayer alumina film dielectric layer, a refractive power of 1600D was obtained at 80V, and dielectric breakdown leading to bubble formation occurred at 105V.
[0099] Comparative Example 3 In comparison, a 1µm monolayer barium strontium titanate film was selected as the dielectric layer and prepared using the same chemical vapor deposition method as in the above embodiments. An electrowetting lens was fabricated using the same method as in the above embodiments, and the test results are as follows. Figure 5 As shown, refractive power was measured for every 5V increase. With only a 1µm monolayer barium strontium titanate dielectric layer, a refractive power of 1600D was obtained at 70V, and dielectric breakdown leading to bubble formation occurred at 90V.
[0100] Performance testing Barrier performance testing. Dielectric films with a total thickness of 1 μm were prepared according to the dielectric layer compositions of Examples 1-4 and Comparative Examples 1-3, respectively. The films with a diameter of 1 m² were tested under a pressure of 1 MPa and a temperature of 23 °C. 2 The water vapor permeation rate of the dielectric film was measured over 24 hours, and its barrier performance was evaluated. The test results are shown in Table 1. Under the same dielectric layer thickness, the single-layer film exhibited higher water vapor permeability, while the composite dielectric film showed higher dielectric layer barrier performance. This indicates that the barrier performance of the composite dielectric film's dielectric layer is significantly higher than that of the single-layer dielectric layer.
[0101] The test results of the dielectric layer breakdown voltage, driving voltage, and water vapor transmission rate of Comparative Examples 1-3 and Examples 1-4 are shown in Table 1: Table 1 Serial Number dielectric layer Dielectric layer thickness Breakdown voltage / V Drive voltage / V <![CDATA[Water vapor transmission rate (g / m 2 ·24h)]]> Comparative Example 1 Parylene C 1um 95 85 10 Comparative Example 2 Alumina 1um 105 80 7 Comparative Example 3 Barium strontium titanate 1um 90 70 9 Example 1 Alumina + Pyrelin C 0.2um + 0.8um 120 80 2 Example 2 Barium strontium titanate + Pyrelin C 0.2um + 0.8um 125 75 2.5 Example 3 Alumina + Pyrelin C + Alumina 0.2um + 0.6um + 0.2um 130 75 1 Example 4 Barium strontium titanate + Pyrelin C + Alumina 0.2um + 0.6um + 0.2um 135 70 1.5 Compared to Comparative Example 1, Example 3 shows a 10-fold increase in barrier properties, a 37% increase in breakdown voltage, and a 12% reduction in driving voltage. Compared to Comparative Example 1, Example 4 shows a 6.7-fold increase in barrier properties, a 42% increase in breakdown voltage, and an 18% reduction in driving voltage. The comparison shows that the dielectric layer of a single-layer Pyrelin C film requires an excessively high driving voltage, and the electrowetting lens of the single-layer film structure has a lower breakdown voltage. In contrast, the composite dielectric film requires a lower driving voltage and has a higher breakdown voltage for the electrowetting lens, making it more advantageous for electrowetting lens applications. Furthermore, comparing water vapor permeability data reveals that the multi-layer film dielectric layer has lower water vapor permeability than the single-layer film dielectric layer. This indicates that the composite dielectric film structure provided in this application significantly improves the barrier properties and breakdown voltage of the dielectric layer while also reducing the driving voltage, effectively improving the working performance of the dielectric layer.
[0102] It should be understood that the application of this application is not limited to the examples above. Those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of this application.
Claims
1. A dielectric layer for electrowetting lenses, characterized in that, The dielectric layer for electrowetting the lens comprises two inorganic dielectric films and one organic dielectric film; the organic dielectric film is disposed between the two inorganic dielectric films. The inorganic dielectric film is one or a combination of two of barium strontium titanate film and alumina film; The organic dielectric film is a Pyrelin C film; The dielectric layer for electrowetting the lens comprises, from bottom to top, a barium strontium titanate film, a Pyrelin C film, and an aluminum oxide film; or, the dielectric layer for electrowetting the lens comprises, from bottom to top, an aluminum oxide film, a Pyrelin C film, and an aluminum oxide film. The inorganic dielectric thin film is prepared by a solution method, including the following steps: Inorganic dielectric material is dissolved in a first solvent to prepare a solution. A mineralizing agent is added dropwise to the solution and stirred to obtain a suspension. The suspension is transferred to a high-pressure hydrothermal reactor and heated and stirred until the reaction is complete. The precipitate obtained after cooling is centrifuged and washed to obtain inorganic dielectric nanoparticles. The inorganic dielectric nanoparticles are dispersed in a second solvent, a surfactant is added, and the mixture is stirred until an inorganic dielectric nanoparticle sol is formed. The inorganic dielectric nanoparticle sol is coated on a substrate, subjected to low-temperature heat treatment in a vacuum atmosphere, and dried to obtain an inorganic dielectric nanoparticle gel. The inorganic dielectric nanoparticle gel is then subjected to low-temperature sintering to obtain an inorganic dielectric film. The first solvent is one of deionized water, anhydrous ethanol, methanol, acetonitrile, ethylene glycol, n-propanol, glacial acetic acid, and ethylene glycol methyl ether; the second solvent is one or both of ethanol and methanol. The concentration range of the inorganic dielectric material in the first solvent is 0.01-10 mol / L; The mineralizing agent is one of sodium hydroxide, potassium hydroxide, tetramethylammonium hydroxide, ammonia, and urea, and the concentration of the mineralizing agent in the first solvent is in the range of 0.5-15 mol / L; The surfactant is one of polyvinylpyrrolidone, oleic acid, tert-butylamine, polyvinyl alcohol, ethanolamine, and hexadecyltrimethylammonium bromide, and the concentration of the surfactant in the second solvent is in the range of 0.1-10 g / L; The inorganic dielectric nanoparticles have a particle size of 5-100 nm, and the concentration of the inorganic dielectric nanoparticles in the second solvent is in the range of 0.001-10 mol / L. The heating and stirring temperature range is 80-250℃, and the heating and stirring time range is 2-72h; The temperature range for the low-temperature heat treatment is 80-350℃; The temperature range for the low-temperature sintering is 80-140℃; The Parylene C film was prepared by vacuum phase deposition. The preparation of the Parylene C film includes the following steps: Solid p-chloroxylene dimer raw material is placed in an evaporation chamber and sublimated at 100-160℃ to produce p-chloroxylene dimer gas; The dichloro-p-xylene dimer gas is fed into the pyrolysis chamber, and active 2-chloro-p-xylene monomer molecules are generated at 600-720°C. The 2-chloro-p-xylene monomer molecules were introduced into a vacuum deposition chamber at room temperature and polymerized and deposited on the substrate surface to obtain a Pyrelin C film.
2. The dielectric layer for electrowetting lenses according to claim 1, characterized in that, The thickness ratio of the inorganic dielectric film to the organic dielectric film is 1:10 to 10:1; the total thickness of the dielectric layer used for electrowetting the lens ranges from 100 nm to 2 μm.
3. The dielectric layer for electrowetting lenses according to claim 1, characterized in that, The dielectric constant of the inorganic dielectric film is 5.5-265; the dielectric constant of the organic dielectric film is 2.95-4.
1.
4. An electrowetting lens, characterized in that, Includes the dielectric layer for electrowetting lenses as described in any one of claims 1-3.
5. The electrowetting lens according to claim 4, characterized in that, The inner diameter of the glass cavity in the electrowetting lens is 0.3-5 mm and the height is 0.1-5 mm; the dielectric constant of the dielectric layer used for the electrowetting lens is 2.95-265.
Citation Information
Patent Citations
Composite dielectric film based on polyimide-inorganic oxide, preparation method thereof and flexible thin film transistor
CN116669432A
Electrowetting element with different dielectric layers
US10133057B1