A methylammonium lead halide perovskite thin film, a preparation method and application thereof

By incorporating DmFc into the perovskite precursor and preparing perovskite thin films using a one-step spin-coating method with an MA/ACN solvent system, the controllability and stability issues of existing processes have been resolved, achieving efficient and stable perovskite thin film preparation and improving the performance of solar cells.

CN117396052BActive Publication Date: 2026-11-24NINGBO UNIVERSITY OF TECHNOLOGY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310939642.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-28
Publication Date
2026-11-24
Estimated Expiration
2043-07-28

AI Technical Summary

Technical Problem

Existing perovskite thin film preparation processes suffer from poor controllability and insufficient manufacturability, and the films are prone to decomposition in air, affecting the stability and power conversion efficiency of perovskite solar cells.

Method used

By incorporating 1,1'-dimethylferrocene (DmFc) into the perovskite precursor and using an MA/ACN composite solvent system, a dense and uniform perovskite film can be prepared by a one-step spin coating method, simplifying the process and reducing additional anti-solvent steps.

Benefits of technology

The prepared perovskite thin film has lower defect density, better humidity resistance and heat resistance, and a power conversion efficiency of 16.92%, which significantly improves the performance of perovskite solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117396052B_ABST
    Figure CN117396052B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of solar cell materials, and relates to methylammonium lead halide perovskite film and a preparation method and application thereof. The application develops an environmental treatment strategy by incorporating 1,1'-dimethylferrocene (DmFc) into a methyl lead halide precursor in a volatile composite MA-ACN solvent system, and high-quality perovskite films are obtained by using a simplified one-step coating method without an additional anti-solvent step. The method can be used for preparing dense, smooth, pinhole-free and large-grained perovskite films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solar cell materials technology, and relates to a methylammonium lead halide perovskite thin film, its preparation method and application. Background Technology

[0002] Metal halide perovskites have attracted significant attention from academia and industry due to their unique photoelectric properties, including high absorption coefficients, long carrier diffusion lengths, tunable band gaps, high carrier mobility, and solution processability. Among various methods for depositing perovskite thin films, one-step spin-coating is perhaps one of the simplest and fastest ways to obtain high-quality perovskite films required for high-efficiency perovskite solar cells (PSCs). To produce smooth, dense, pinhole-free films, it is often necessary to add an antisolvent at a specific stage of the process or to employ vacuum treatment. These steps help avoid the extended time required to evaporate excess polar aprotic solvents with high boiling points, such as most commonly used solvents like N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) for photoelectric conversion efficiencies (PCE) greater than 20%. Regardless of the toxicity of the antisolvent, the poor controllability and large-scale applicability of these additional steps may reduce the compatibility of one-step coating processes with scalable deposition techniques for industrial applications of perovskite solar cells.

[0003] To address this, researchers introduced volatile methylamine (MA) solutions into suitable low-boiling-point, low-viscosity solvents, particularly acetonitrile (ACN), as a composite solvent system. This is because it promotes rapid crystallization of perovskite films more readily than high-boiling-point solvents (DMF, DMSO, etc.). They may have used MA gas, but this readily evaporates from the precursor, making it difficult to process before repairing defects in the crystalline perovskite film and hindering large-scale perovskite film deposition. By spin-coating the perovskite precursor salt in an MA / ACN solvent, the volatile MA enhances the solvation ability of ACN, rapidly supersaturating the solute to a critical point, leading to rapid perovskite crystal growth without the need for an additional antisolvent step. Therefore, compared to preparing perovskite films in MA gas and high-boiling-point solvents, this method offers controllability and simplicity, yielding dense, uniform, and high-coverage perovskite films, which is crucial for reducing the commercialization barriers of PSCs. Despite these advances, perovskite films inevitably contain some inherent defects that are prone to diffusion under air conditions, leading to further decomposition of the perovskite film. These defects will adversely affect the stability of PSCs and PCE, becoming one of the major obstacles to their industrial application.

[0004] Significant progress has recently been made in metal halide perovskite solar cells (PSCs), with power conversion efficiency (PCE) increasing from 3.8% to over 25%, partly due to the high-quality perovskite films resulting from an efficient one-step spin-coating process. However, this process often requires an additional anti-solvent step, resulting in poor controllability and manufacturability. While the MA / CAN system can better match the one-step deposition process, some inherent defects within the prepared film are prone to diffusion under atmospheric conditions, leading to further decomposition of the perovskite film and fundamentally limiting the commercialization of PSCs. Summary of the Invention

[0005] The purpose of this invention is to address the aforementioned problems in the prior art by preparing a 1,1′-dimethylferrocene-induced methylammonium lead halide perovskite thin film by incorporating 1,1′-dimethylferrocene (DmFc) into a perovskite precursor.

[0006] The objective of this invention can be achieved through the following technical solutions:

[0007] A methylammonium lead halide perovskite thin film, the thin film comprising, in sequence, a PEDOT:PSS layer, a perovskite layer containing DmFc, and a PCBM layer.

[0008] The present invention also provides a method for preparing the above-mentioned methylammonium lead halide perovskite thin film, the method comprising the following steps:

[0009] S1. Spin-coat PEDOT:PSS solution onto the surface of ITO substrate, and then anneal it to obtain a PEDOT:PSS layer.

[0010] S2. Spin-coat a perovskite precursor solution containing DmFc onto the surface of the PEDOT:PSS layer, and then perform annealing to obtain a perovskite layer containing DmFc.

[0011] S3. Finally, a PCBM solution is coated onto the surface of the perovskite layer containing DmFc.

[0012] This invention introduces 1,1'-dimethylferrocene (DmFc) into the methyl lead halide precursor, which not only restores internal defects in perovskite films but also simplifies the process, eliminating the need for an additional anti-solvent step. Dense, uniform, large-grained perovskite films were prepared at room temperature, exhibiting lower defect density, better humidity resistance, and stronger heat resistance compared to conventional perovskite films, with a PCE as high as 16.92%.

[0013] In the above-mentioned method for preparing a methylammonium lead halide perovskite thin film, the PEDOT:PSS solution in step S1 is EDOT:PSS and deionized water in a volume ratio of 1:(0.5-1.5).

[0014] In the above-mentioned method for preparing a methylammonium lead halide perovskite thin film, the annealing temperature in step S1 is 115-125℃ and the time is 15-25min.

[0015] In the above-mentioned method for preparing a methylammonium lead halide perovskite thin film, the method for preparing the perovskite precursor solution containing DmFc in step S2 specifically includes: dissolving PbI2, MAI and MACl in methylamine ethanol solution and stirring, then adding acetonitrile solution and stirring overnight, and then adding DmFc.

[0016] This invention prepares a high-quality methylammonium lead halide perovskite film induced by 1,1′-dimethylferrocene (DmFc) in a perovskite precursor using an MA / ACN composite solvent system. Since the residual volatile solvent evaporates rapidly during this process, a one-step spin-deposition method is required to stably deposit the perovskite film under normal conditions without an additional anti-solvent step. In DmFc, iron elements are encased between two cyclopentadiene rings, forming a sandwich structure that allows for reversible recovery of defects in the perovskite, resulting in a more stable perovskite film without leaving any raw material-induced defects in the perovskite material. The PCE of PSC is higher than that of the control.

[0017] In the above-mentioned method for preparing a methylammonium lead halide perovskite thin film, the amount of DmFc added is 1-5 mg / mL. -1 This invention enables the preparation of methylammonium lead halide perovskite thin films to achieve optimal performance by controlling the amount of DmFc added.

[0018] In the above-mentioned method for preparing a methylammonium lead halide perovskite thin film, the annealing temperature in step S2 is 95-105℃ and the time is 5-15min.

[0019] The present invention also provides an application of the above-mentioned methylammonium lead halide perovskite thin film in solar cells.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] This invention develops an environmentally friendly treatment strategy in a volatile composite MA-ACN solvent system by incorporating 1,1'-dimethylferrocene (DmFc) into a methyl lead halide precursor. This simplified one-step coating method eliminates the need for an additional anti-solvent step, enabling the preparation of high-quality perovskite films. This method can produce dense, smooth, pinhole-free perovskite films with relatively large particles. 1H-NMR results and XPS analysis proposed a reasonable mechanism for DmFc-doped perovskite films to repair defects. The defect density in the target film was significantly suppressed by PL lifetime and SCLC measurements. These improvements allow for the achievement of more stable perovskite films, not only in terms of moisture resistance but also in terms of heat resistance. Finally, PCE of up to 16.92% was achieved based on PSCs of the target sample. Attached Figure Description

[0022] Figure 1 This is a schematic diagram illustrating the preparation of DmFc-doped perovskite thin films and possible defect recovery mechanisms under atmospheric conditions in Example 1.

[0023] Figure 2 The images show top-view SEM images of the perovskite film of Example 1 and Comparative Example 1, including top-view SEM images (a) and (b) and a cross-sectional SEM image (c) of the perovskite film of Comparative Example 1; top-view SEM images (d) and (e) and a cross-sectional SEM image (f) of the perovskite film of Example 1; and insets in (b) and (e) showing the grain size distribution controlling the perovskite film and the perovskite film of Example 1, respectively.

[0024] Figure 3 The following are comparative spectral diagrams of the perovskite thin film of Example 1 and Comparative Example 1: (a) XRD pattern, (b) absorption spectrum and corresponding Tauc plot, (c) peroxide thin film of Comparative Example 1 and Example 1. 1 1H NMR spectra, with star and triangle symbols representing solvent and water peaks in dimethyl sulfoxide (DMSO)-d6. 1 H NMR spectra, (d) XPS spectra showing I 3d core levels, (e) XPS spectra showing Pb 4f core levels, and (f) XPS spectra showing N1s core levels were used for the peroxide films of Comparative Example 1 and Example 1.

[0025] Figure 4 The steady-state PL(a) and TRPL(b) spectra of the control and target peroxide films on the PEDOT:PSS substrate during the fabrication process of Example 1 are shown. The dark current-voltage characteristics of the pure hole transport layer device based on the control and target peroxide films (c) and (d) are shown on a double logarithmic scale. The inset illustrates the device structure.

[0026] Figure 5 The UV-Vis spectra of Example 1 and the control group are shown below. (a) Comparative Example 1 and (b) The time the film of Example 1 was exposed to ambient air at room temperature, (c) XRD patterns of the film of Comparative Example 1 and (d) The time the film of Example 1 was heated on a hot plate at 85°C, and (e) Comparative Example 1 and (f) Example 1.

[0027] Figure 6The following is a schematic diagram of the thin film structure and performance testing in Example 1: (a) structural schematic diagram, (b) JV curve under dark conditions, (c) JV curve under AM 1.5G, (d) EQE spectrum, (e) steady-state power output, and (f) statistical power conversion efficiency distribution, and (f) histogram of PCE of the device. Detailed Implementation

[0028] The following are specific embodiments of the present invention, which further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0029] Example 1:

[0030] S1. Dissolve 277 mg PbI2, 95 mg MAI, and 8 mg MACl in 500 μl of methylamine ethanol solution and stir for 1 h. Then add 500 μl of acetonitrile solution and stir overnight at room temperature. Finally, add 2 mg / mL of [the solution / preparation]. -1 DmFc yields perovskite precursor solution;

[0031] S2. The ITO substrate was ultrasonically treated in detergent, deionized water, acetone and isopropanol for 20 min in sequence. The cleaned substrate was then treated with plasma for 15 min to remove organic residues.

[0032] S3. Coat the plasma-treated substrate with PEDOT:PSS solution at 6000 rpm for 30 s, and then anneal at 120 °C for 20 min to obtain the PEDOT:PSS layer.

[0033] S4. After cooling, 30 μl of perovskite precursor solution was spin-coated onto the PEDOT:PSS layer at 4000 rpm for 30 s, and then annealed at 100 °C for 10 min to obtain a perovskite layer containing DmFc.

[0034] S5, Add 20mg ml -1 The PCBM chlorobenzene solution was spin-coated onto the perovskite film at a speed of 3000 rpm for 45 seconds.

[0035] S6. The solar cell device is fabricated by evaporating a silver electrode (100 nm) at a rate of 0.1 nm / s through a mask.

[0036] Comparative Example 1:

[0037] S1. Dissolve 277 mg PbI2, 95 mg MAI and 8 mg MACl in 500 μl of methylamine ethanol solution and stir for 1 h. Then add 500 μl of acetonitrile solution and stir overnight at room temperature to complete the preparation of perovskite precursor solution.

[0038] S2. The ITO substrate was ultrasonically treated in detergent, deionized water, acetone and isopropanol for 20 min in sequence. The cleaned substrate was then treated with plasma for 15 min to remove organic residues.

[0039] S3. Coat the plasma-treated substrate with PEDOT / PSS solution by spin coating at 6000 rpm for 30 s, and then anneal at 120 °C for 20 min to obtain the PEDOT:PSS layer.

[0040] S4. After cooling, 30 μl of perovskite precursor solution was spin-coated onto the PEDOT:PSS layer at 4000 rpm for 30 s, and then annealed at 100 °C for 10 min to obtain the perovskite layer.

[0041] S5, Add 20mg ml -1 The PCBM chlorobenzene solution was spin-coated onto the perovskite film at a speed of 3000 rpm for 45 seconds.

[0042] S6. The solar cell device is fabricated by evaporating a silver electrode (100 nm) at a rate of 0.1 nm / s through a mask.

[0043] This invention utilizes a mixed solvent of methylamine ethanol solution (MAES) and acetonitrile (ACN) to prepare a precursor solution, such as... Figure 1 The solution containing 1,1'-dimethylferrocene (DmFc) powder is deep yellow compared to the pale yellow perovskite precursor solution. The perovskite film was prepared by one-step spin-coating in ambient air. Unlike the usual method of using anti-solvents to control crystallization and improve film quality, this method employs a volatile mixed MAES-ACN solvent system. The low-boiling-point MAES-ACN mixed solvent evaporates rapidly during spin-coating, promoting the precursor concentration to reach the critical nucleation concentration for rapid nucleation and subsequent growth. Furthermore, the Fe in DmFc is positioned between two cyclopentadiene rings, forming a "sandwich" structure. This structure effectively shields it from direct replacement by defects in the perovskite. In fact, even after rapid self-exchange reactions, the "sandwich" structure of DmFc in the perovskite remains. This allows for DmFc / DmFc formation. + Redox pairs may play a positive role in healing elemental defects in peroxide films.

[0044] In order to study the effect of DmFc additive on the microstructure of perovskite thin films, the surface morphology of the control and Example 1 films was examined using scanning electron microscopy (SEM). Figure 2 a and 2b show top-view SEM images of the perovskite film in Comparative Example 1, where small nanocrystals with an average grain size of approximately 620 nm are observed. Figure 2(Illustration b) and some irregular crystal particles form a relatively uneven surface. It is worth noting that in Figure 2 Many bright areas marked with red dashed lines in b are clearly visible on the surface of the control sample, which can be identified as typical Schottky defects in PbI2. In contrast, the target peroxide film exhibits a flat surface without visible bright PbI2 nanoparticles. Figure 2 d and 2e). The average grain size is estimated to be approximately 1.19 μm ( Figure 2 (illustration of e), which is almost twice the size of the original perovskite film. This increase in grain size indicates that the DmFc additive in the target perovskite precursor contributes to the growth of perovskite crystals, which may reduce defects and improve the optoelectronic performance of the device, although photoactive perovskite layers of similar thickness have been obtained using the same spin-coating process ( Figure 2 c and 2f).

[0045] To evaluate the crystallinity of the perovskite thin film, X-ray diffraction tests were performed, such as... Figure 3 As shown in Figure a, both samples exhibit dominant diffraction peaks at 14.16° and 28.48°, corresponding to the (110) and (220) crystal planes of typical tetragonal MAPbI3 perovskite. The intensities of these two dominant peaks in the Example 1 film are significantly greater than those in the Comparative Example 1 film, indicating that the crystallinity of the Example 1 perovskite film was improved after introducing DmFc into the precursor solution. Furthermore, fitting the curves near 14.16° revealed that the full width at half maximum (FWHM) of the strongest (110) crystal plane peak in the Example 1 film was smaller than that of the Comparative Example 1 perovskite film. The increase in diffraction peak intensity and decrease in FWHM of both perovskite films indicate that better crystallinity was achieved after introducing DmFc into the perovskite precursor, consistent with the results of the SEM images.

[0046] To investigate the effect of DmFc addition on perovskite defects, steady-state photoluminescence (PL) and time-resolved photoluminescence (TRPL) measurements were performed on the perovskite films of Comparative Example 1 and Example 1 deposited on PEDOT / PSS / ITO substrates. Figure 4 As shown in figure a, the control and target films exhibit almost identical peak positions at approximately 775 nm, indicating that the addition of DmFc does not significantly affect the electronic structure or perovskite energy levels. However, the peak intensity of the control film is much higher than that of the target sample, suggesting that the target film exhibits a reduction in nonradiative recombination losses. Figure 4 As shown in b, the charge recombination kinetics were analyzed using TRPL decay curves. A double exponential model was used to fit the decay curves, and the corresponding parameters were extracted from the function. The fast decay τ1 and slow decay τ2 are attributed to bimolecular recombination and trap-assisted recombination, respectively. The formula for calculating the average PL decay lifetime is as follows: The corresponding key parameters are shown in Table S1. The estimated average lifetime of the control perovskite film is 159.33 ns, which is significantly larger than the average lifetime of the sample in Example 1 (64.26 ns). The smaller τ... avg This indicates more efficient charge extraction between the perovskite film and the charge carrier transport layer, possibly due to the reduction of defects in the target perovskite film caused by the addition of DmFc. To verify the charge carrier transport, this invention fabricated a device based on a pure hole transport layer of ITO / PEDOT:PSS / Perovs-kites / Spiro-OMeTAD / Ag. Figure 4 (See illustration c), and the JV curve was measured under dark conditions. Figure 4 As shown in c and 4d, both JV curves on the double logarithmic scale can be divided into three distinct regions: the Ohmic region, the trap-fill-limit (TFL) region, and the Tong's region. The well density N... t The starting voltage V of the TFL region can be used as a reference. TFL The calculation shows that: Where ε and ε0 represent the relative permittivity and vacuum permittivity, respectively, e is the elementary charge, and L represents the thickness of the peroxide film. Calculations show that the peroxide-based control device has a thickness of 1.13 × 10⁻⁶. 16 cm -3 ( Figure 4 c) This is approximately 1.6 times that of the target sample (7.05 × 10⁻⁶). 15 cm -3 , Figure 4 d). The reduction in defect state density is beneficial for facilitating charge carrier extraction and transport, and may hold promise for improving film stability and device performance. This result is also consistent with photoluminescence (PL) and time-resolved photoluminescence (TRPL) measurements, indicating that the addition of DmFc to perovskites may reduce elemental defects, leading to a significant decrease in the overall defect level, as demonstrated by our NMR findings.

[0047] In order to study the effect of DmFc addition on stability, this invention compared the XRD patterns of control and target perovskite films under different conditions, including exposing the peroxide film in an ambient atmosphere and heating the peroxide film on a hot plate in a nitrogen-filled glove box. Figure 5 Figures a and 5b show the initial moisture resistance of the films of Comparative Example 1 and the reinforcing group after exposure to ambient atmosphere for a period of time at room temperature. After 10 days of exposure, the XRD pattern of the film of Comparative Example 1 shows negligible difference from the initial state of the film. Figure 5a) The perovskite film exhibits two dominant peaks on the (110) and (220) planes of the tetragonal MAPbI3 phase, with no observable PbI2 peaks, indicating that the perovskite has not decomposed into PbI2, or the content of decomposed PbI2 is below the limit of XRD detection. Furthermore, no significant degradation can be observed in the appearance of the perovskite film after 10 days. Figure 5 (Illustration in a). However, after 20 days of exposure, a distinct PbI2 peak was observed in the XRD pattern of the control film, and its intensity gradually increased with prolonged exposure time, indicating further degradation of the film. Meanwhile, as... Figure 5 As shown in the illustration in Figure a, degraded spots become very noticeable on the appearance of the perovskite film, indicating localized degradation. These spots appear to increase after one month. Notably, the color of the perovskite film turns pale yellow after two months of exposure. This color change may be due to the formation of decomposition products or the presence of impurities generated during the degradation process. In contrast, the XRD spectrum of the film in Example 1 ( Figure 5 b) indicates that no significant peaks or changes were observed one month after exposure, suggesting the decomposition of the peroxide material. Similarly, as... Figure 5 As shown in the illustration of b, the film's appearance also showed no obvious signs of degradation. Even after two months of exposure, only a few spots appeared on the surface of the perovskite film. This suggests that the peroxide film bonded with DmFc may possess better stability and durability than the film in Comparative Example 1. For thermal stability testing, the samples were placed in a glove box on a hot plate previously heated to 85°C to determine the changes in the XRD pattern over time. Whether at the start of the test, after 5 hours, 10 hours, or even after a final 20 hours of heating, the film in Comparative Example 1 (… Figure 5 c) and the thin film of Example 1 ( Figure 5 d) No significant XRD changes were observed, indicating that the crystal structure of the samples remained largely unchanged. Therefore, further UV-Vis absorption measurements were performed to compare the differences between these samples. Figure 5 As shown in Figure e, as the heating time increased from 0 to 20 hours, the control sample exhibited almost the same absorption onset, while its intensity decreased with increasing heating time. Specifically, at a wavelength of 650 nm, the intensity of the control film decreased to 98.9% and 96.8% of its initial value after 5 and 10 hours of heating, respectively, and finally to approximately 94.3% after 20 hours. Example 1: Absorption Onset and Intensity of the Thin Film ( Figure 5f) The film exhibited a similar trend to the control perovskite film. However, under the same heating conditions, the strength change of the Example 1 film was significantly less than that of the control film. For example, the strength of the Example 1 sample decreased to 96.5%, while after 20 hours of heating, the strength of the control film was approximately 94.3% of its initial value. Although the absorbed strength of both films decreased over time, the decrease was much smaller, indicating that the Example 1 film has better thermal stability compared to the control film. This is likely due to the reduction in perovskite structural defect density caused by the addition of DmFc to the perovskite film.

[0048] This invention also fabricates a perovskite solar cell (PSC) with a device structure of ITO / PEDOT:PSS / Perovskite / PCBM / Ag, as shown below. Figure 6 As shown in a. Figure 6 b shows the dark-state JV curves of the perovskite solar cells based on the control film and the target film, which can be divided into regions A, B, and C. Regions A and B are related to the leakage current and reverse saturation current density of the PSC, respectively, while region C is related to the series resistance of the solar cell. From region A, it can be seen that the leakage current density of the PSC based on the perovskite film of Example 1 is an order of magnitude lower than that of the control device, indicating that the target device will achieve higher Jsc and FF under illumination. By fitting the JV curve in region B, the saturation current density (J0) of the device of Example 1 can be obtained as 2.68 × 10⁻⁴ mA cm⁻¹. -2 This is greater than the controller's (5.65 × 10⁻³ mA cm⁻¹) -2 The JV is much smaller. The smaller the reverse saturation current density, the higher the Voc under illumination. To verify the evidence from the dark JV curves, the JV curves of the two devices were subsequently measured under simulated sunlight with an intensity of 100 mW cm⁻². The test results are shown in Table 2. As expected, the champion PSC based on the target perovskite thin film achieved significant improvements in key device parameters, such as Jsc (21.95 mA cm⁻²). -2 Voc (0.99V) and FF (77.88%) were compared with the parameters of the control device (20.75mA cm⁻¹). -2 Compared to (0.93V and 69.30%) Figure 6 (See illustration c). Example 1's device achieved a champion PCE of 16.92%, surpassing the controller's performance (13.38%) by a margin of 26%. Table 2 shows the JV parameters of the best performance PSC based on thin-film control and Tatget.

[0049] Furthermore, the consistency of the JV curve between forward and reverse scans of the device in Example 1 is better than that of the control device, as evaluated by the hysteresis index (HI) and a formula. The target device has a HI of 2.36%, which is much lower than the HI of the Comparative Example 1 device (16.44%). The significant suppression of HI in the Example 1 device may be related to the reduced trap density and / or effective charge carrier extraction in the peroxide due to the addition of DmFc.

[0050] Figure 6 d shows the external quantum efficiency (EQE) and comprehensive J of the control and target PSCs. SC Both the control device and the target device exhibited nearly identical cutoff wavelengths, indicating that the addition of DmFc to the perovskite did not alter the perovskite's band gap. Throughout the entire spectral response range, the device of Example 1 exhibited enhanced EQE compared to the control device, resulting in integrated J... sc From the control device 19.18mA cm -2 Increased to 20.99 mA cm -2 This is consistent with the J extracted from JV measurements under simulated sunlight. sc Similar. To assess the power stability of the detector, steady-state power output under continuous illumination for 300 seconds was measured at a bias voltage; this was determined by the initial VMPP through illumination JV measurements. (As shown) Figure 6 As shown in Figure e, the control device exhibits a slight decrease in photocurrent density and PCE before reaching a stable value of 17.21 mA cm⁻¹. -2 And 13.16%, while the device in Example 1 provided 19.13 mA cm⁻¹ from the start to the end of the test. -2 The device exhibits ultra-stable photocurrent density and a PCE of 15.30%. The improved stability under continuous illumination is related to the reduction in hysteresis caused by the bonding of DmFc within the perovskite. To check the repeatability of the device, 32 independent photocurrent cells (PSCs) were fabricated, and the JV characteristics were measured. The histograms of the PCE for these devices are shown below. Figure 6 As shown in f, both PSCs exhibit narrow distributions, with average PSC values ​​of 12.02% and 14.56% based on the control film and target film, respectively. The good performance and high reproducibility of the device are attributed to the high-quality perovskite film and the low trap density in the perovskite, indicating that incorporating DmFc into the perovskite is an effective and promising method for achieving stable and efficient perovskite solar cells in high-humidity ambient air.

[0051] In summary, by incorporating 1,1'-dimethylferrocene (DmFc) into a methyl lead halide precursor, this invention develops an environmentally friendly treatment strategy in a volatile composite MA-ACN solvent system. This simplified one-step coating method eliminates the need for additional anti-solvent steps, enabling the preparation of high-quality perovskite films. This method can produce dense, smooth, pinhole-free perovskite films with relatively large particles. 1H-NMR results and XPS analysis suggest a reasonable mechanism for DmFc-doped perovskite films to repair defects. The defect density in the target film is significantly suppressed by PL lifetime and SCLC measurements. These improvements allow for the achievement of more stable perovskite films, not only in terms of moisture resistance but also in terms of heat resistance. Finally, PSCs based on the target sample achieved a champion PCE of 16.92%, with negligible hysteresis, showing a 1.26-fold improvement over Comparative Example 1.

[0052] The embodiments described herein cover any points not exhaustively within the scope of the technical claims of this invention, as well as new technical solutions formed by equivalent substitutions of one or more technical features in the embodiments. These are all within the scope of the claims of this invention. Furthermore, in all listed or unlisted embodiments of this invention, each parameter in the same embodiment merely represents an instance (i.e., a feasible solution) of its technical solution, and there is no strict coordination or limitation relationship between the parameters. The parameters can be substituted for each other without violating axioms and the claims of this invention, unless otherwise stated.

[0053] The technical means disclosed in this invention are not limited to those described above, but also include technical solutions composed of any combination of the above technical features. The above descriptions are specific embodiments of this invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of this invention, and these improvements and modifications are also considered within the scope of protection of this invention.

[0054] The specific embodiments described herein are merely illustrative of the spirit of the invention. Those skilled in the art to which this invention pertains may make various modifications or additions to the described specific embodiments or use similar methods to substitute them, without departing from the spirit of the invention or exceeding the scope defined by the appended claims.

Claims

1. A methylammonium lead halide perovskite thin film, characterized in that, The thin film comprises, in sequence, a PEDOT:PSS layer, a perovskite layer containing DmFc, and a PCBM layer; The preparation method of the methylammonium lead halide perovskite thin film includes the following steps: S1. Spin-coat PEDOT:PSS solution onto the surface of ITO substrate, and then anneal it to obtain a PEDOT:PSS layer. S2. Spin-coat a perovskite precursor solution containing DmFc onto the surface of the PEDOT:PSS layer, and then perform annealing to obtain a perovskite layer containing DmFc. S3. Finally, a PCBM solution is coated on the surface of the perovskite layer containing DmFc. Specifically, step S2, the preparation method of the perovskite precursor solution containing DmFc, includes: dissolving PbI2, MAI, and MACl in methylamine ethanol solution and stirring, then adding acetonitrile solution and stirring overnight, followed by adding DmFc, with the amount of DmFc added being 1-5 mg / mL. -1 In step S2, the annealing temperature is 95-105℃ and the time is 5-15min.

2. The methylammonium lead halide perovskite thin film according to claim 1, characterized in that, In step S1, the PEDOT:PSS solution is a mixture of EDOT:PSS and deionized water in a volume ratio of 1:(0.5-1.5).

3. The methylammonium lead halide perovskite thin film according to claim 1, characterized in that, In step S1, the annealing temperature is 115-125℃ and the time is 15-25min.

4. The application of the methylammonium lead halide perovskite thin film as described in claim 1 in a solar cell.