Method for producing paper and board
By directly injecting water-soluble polymers in solid particulate form, which react in a mixture of alkali metal hydroxides and hypohalides, into fiber suspensions, the problems of large footprint in polyacrylamide solution transportation and dissolution equipment are solved, the drainage and dry strength properties of paper or paperboard are improved, and the production process is simplified.
Patent Information
- Application Number
- CN202280028579.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-15
- Filing Date
- 2022-04-13
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-04-13
AI Technical Summary
In the existing technology, the equipment for transporting and dissolving polyacrylamide solutions occupies a large area, and the reaction requires heating and temperature control, which leads to a complex process and waste of resources in the production of paper or paperboard.
A water-soluble polymer in solid particle form is reacted in a mixture of alkali metal hydroxides and hypohalides, and then directly injected into a fiber suspension, avoiding solution handling and heating of the reaction medium, thus simplifying the operation.
It improves the drainage and dry strength properties of paper or paperboard, reduces equipment footprint and resource consumption, and simplifies the production process.
Smart Images

Figure BDA0004492954710000101 
Figure BDA0004492954710000102
Abstract
Description
Technical Field
[0001] This invention relates to a method for producing paper or paperboard with improved drainage and processability. More specifically, this invention relates to a method involving the reaction of a water-soluble polymer in solid particulate form in a mixture of hydroxides (alkali metal hydroxides and / or alkaline earth metal hydroxides) and hypohalides (alkali metal hypohalides and / or alkali metal hypohalides), which is then directly injected into a fiber suspension for the production of paper or paperboard.
[0002] The present invention also relates to paper and paperboard with improved physical properties obtained by this method. Background Technology
[0003] The paper industry has been seeking to optimize its paper or paperboard production methods, particularly in terms of output, productivity, cost reduction, and finished product quality.
[0004] The uses of polymers as dry strength agents, drainage agents, and machinability agents have been described very extensively.
[0005] Drainage performance refers to the ability of the fiber mat to remove or drain the maximum amount of water before the drying section. Improved drainage performance translates to energy savings and increased production capacity.
[0006] Processability refers to optimizing the operation of a paper machine by improving productivity through better drainage on the table, better drying in the press section, reducing breakage through greater loop cleanliness, and reducing deposits.
[0007] WO 2006 / 075115 describes a method for producing paper or paperboard using at least two dry strength agents:
[0008] - The first reagent was obtained by Hofman degradation reaction on the basis of (co)polymer.
[0009] and
[0010] - A second reagent corresponding to (co)polymers with anionic charge density greater than 0.1 meq / g.
[0011] US 4,110,520 describes the modification of a polymer in solid form. The polymer does not dissolve during the modification process.
[0012] EP 2 536 489 describes an apparatus for dispersing and grinding polymers.
[0013] EP 2 840 100 describes the functionalization of polymers by means of multifunctional compounds.
[0014] US 5,292,821 describes a method for producing paper using cationic polyacrylamide.
[0015] Polyvinylamine is known to improve drainage in the papermaking process.
[0016] Polyvinylamine can be obtained by reacting polyacrylamide in a solution of alkali metal hydroxide and / or alkaline earth metal hydroxide and alkali metal hypohalides and / or alkaline earth metal hypohalides, followed by treatment in an acidic medium.
[0017] When the reaction is carried out directly before the product is injected into the fiber suspension to obtain paper or paperboard, only the polyacrylamide in solution reacts with the alkali metal or alkaline earth metal hydroxide and the hypohalides.
[0018] However, this need for polyacrylamide solutions means either transporting them to paper mills or having equipment within the paper mills for dissolving the polymer in particulate form. In both cases, the footprint of the polymer solution inventory or the dissolving equipment remains substantial.
[0019] Furthermore, this reaction on polyacrylamide requires heating the reaction medium and also requires an exchanger to regulate its temperature at the end of the reaction. Summary of the Invention
[0020] Unexpectedly, the applicant discovered a method involving the reaction of a water-soluble polymer in solid particulate form in a mixture of hydroxides (alkali metal hydroxides and / or alkaline earth metal hydroxides) and hypohalides (alkali metal hypohalides and / or alkali metal hypohalides), which is then directly injected into a fiber suspension used in the production of paper or paperboard, thereby improving drainage and dry strength properties.
[0021] This method can also avoid the entire logistics process (transportation or installation of the dissolution unit) inherent in the handling of water-soluble polymer solutions.
[0022] Furthermore, the method becomes simpler when the polymer dissolves very rapidly in the reaction mixture of alkali metal and / or alkaline earth metal hydroxides and hypohalides, and when heating the reaction medium or using a heat exchanger is not required.
[0023] "Alkali" refers to an alkali metal, preferably lithium, sodium, or potassium. "Alkali metal hydroxide" refers to a hydroxide (OH) of at least one alkali metal. - For example, NaOH, KOH, or NaOH+KOH. This also applies to alkaline earth metal hydroxides.
[0024] "Alkaline earth" refers to alkaline earth metals, preferably calcium or magnesium.
[0025] Hypohalides are oxygen-containing anions, such as hypochlorite (ClO). - .
[0026] "Alkali metal hypohalides" refers to a hypohalide of at least one alkali metal and at least one hypohalide, such as NaOCl, KOBr, or NaOCl+KOBr. The same applies to alkaline earth metal hypohalides.
[0027] Finally, because the molecular weight range of water-soluble polymers in solid particulate form is very large, the method of the present invention allows for an expansion of the current range of drainage agents and dry strength agents compared to similar methods using polyacrylamide in aqueous solution form.
[0028] More specifically, the present invention relates to a method for producing paper or paperboard from a fiber suspension, the method comprising the following steps:
[0029] a) Injecting polymer P2 into a fiber suspension (advantageously an aqueous suspension of cellulose fibers),
[0030] b) Forming paper or paperboard.
[0031] c) Dry paper or cardboard.
[0032] Prior to step a), polymer P2 is prepared from a water-soluble polymer P1 in solid particulate form, wherein P1 is a water-soluble polymer of at least one nonionic monomer selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile.
[0033] The polymer P2 is obtained by reaction Re, which comprises (advantageously consisting of) adding and dissolving solid particles of the water-soluble polymer P1 in an aqueous solution M1, the aqueous solution M1 comprising: (i) an alkali metal hydroxide or an alkaline earth metal hydroxide or a mixture thereof, and (ii) an alkali metal hypohalide or an alkaline earth metal hypohalide or a mixture thereof.
[0034] After adding water-soluble polymer P1 particles, the reaction time of Re is 10 seconds to 5 hours.
[0035] Therefore, during the Re reaction, the water-soluble polymer P1 dissolves in the aqueous solution M1.
[0036] Advantageously, step a) is carried out within a time frame not exceeding 24 hours from the start of reaction Re, that is, from the addition of the solid particles of the water-soluble polymer P1 to the aqueous solution M1.
[0037] In the subsequent parts of the specification and in the claims, all references to "gt" are valid. -1 or kg.t -1The polymer dosages indicated are given as the weight of the polymer per tonne of dry matter. Dry matter is a dry extract obtained by evaporating water from a fiber suspension used in methods for producing paper or paperboard. Dry matter advantageously consists of cellulose fibers and fillers. The term "cellulose fiber" includes any cellulose entity, including fibers, fine fibers, microfibers, or nanofibers. Fiber suspension is understood to refer to a concentrated or diluted slurry based on water and cellulose fibers. Concentrated slurries (thick slurries) with a dry matter concentration typically greater than 1%, or even greater than 3%, are located upstream of a mixing pump (fan pump). Diluted slurries (thin slurries) with a dry matter concentration typically less than 1% are located downstream of a mixing pump.
[0038] The term "polymer" refers to homopolymers and copolymers of at least two different monomers.
[0039] Amphoteric polymers are polymers containing both cationic and anionic charges, preferably with anionic charges being equal to cationic charges.
[0040] As used herein, the term "water-soluble polymer" refers to a polymer that, when stirred at 25°C for 4 hours and at a concentration of 20 g / L... -1 When a polymer is dissolved in deionized water at a concentration of [amount], it produces an aqueous solution without insoluble particles.
[0041] The numerical range includes a lower limit and an upper limit. Therefore, the numerical ranges “0.1 to 1.0” and “0.1 to 1” include the values 0.1 and 1.0.
[0042] The water-soluble polymer P1 is a polymer of at least one nonionic monomer selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile. Preferably, polymer P1 contains at least 50 mol% of at least one of these nonionic monomers.
[0043] The polymer P1 may also contain anionic and / or cationic and / or zwitterionic monomers. Advantageously, polymer P1 does not contain nonionic monomers not selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile.
[0044] The anionic monomer is preferably selected from the group consisting of: monomers having a carboxylic acid functional group and their salts, including acrylic acid, methacrylic acid, itaconic acid, and maleic acid; monomers having a sulfonic acid functional group and their salts, including acrylamide tert-butyl sulfonic acid (ATBS), allyl sulfonic acid, and methyl allyl sulfonic acid and their salts; and monomers having a phosphonic acid functional group and their salts.
[0045] Typically, the anionic monomer salt of polymer P1 is an alkali metal, alkaline earth metal, or ammonium (preferably quaternary ammonium) salt.
[0046] The cationic monomer is preferably selected from the group consisting of: quaternized or salted dimethylaminoethyl acrylate (ADAME), quaternized or salted dimethylaminoethyl methacrylate (MADAME), diallyl dimethyl ammonium chloride (DADMAC), acrylamidopropyl trimethyl ammonium chloride (APTAC), and methacrylamidopropyl trimethyl ammonium chloride (MAPTAC).
[0047] Advantageously, the cationic monomer of polymer P1 has a halide ion (preferably chloride ion) as a counterion.
[0048] The zwitterionic monomer is preferably selected from the group consisting of: sulfobetaine monomers, such as sulfopropyl dimethylammonium ethyl methacrylate, sulfopropyl dimethylammonium propyl methacrylamide, or sulfopropyl-2-vinylpyridine; phosphate betaine monomers, such as ethyltrimethylammonium phosphate ethyl methacrylate; and carboxybetaine monomers.
[0049] Preferably, the water-soluble polymer P1 is a homopolymer or copolymer of acrylamide or methacrylamide.
[0050] Polymer P1 can be linear, structured, or crosslinked. Structured crosslinking agents are particularly selected from sodium allyl sulfonate, sodium methyl allyl sulfonate, sodium methyl allyl disulfonate, methylenebisacrylamide, triallylamine, and triallyl ammonium chloride.
[0051] The structuring of polymer P1 can also be achieved using at least one polyfunctional compound containing at least three heteroatoms selected from N, S, O, and P, and each heteroatom having at least one mobile hydrogen atom. Such polyfunctional compounds can be, in particular, polyethyleneimine or polyamine.
[0052] The reaction Re involves adding and dissolving solid particles of polymer P1 in an aqueous solution M1, which comprises: (i) alkali metal hydroxides and / or alkaline earth metal hydroxides, and (ii) alkali metal hypohalides and / or alkaline earth metal hypohalides. The reaction Re is carried out for 10 seconds to 5 hours to form polymer P2.
[0053] Advantageously, the aqueous solution M1 is an aqueous solution of soda (sodium hydroxide) and sodium hypochlorite.
[0054] Advantageously, the reaction time of polymer P1 in aqueous solution M1 of hypohalide and hydroxide is from 10 seconds to 180 minutes.
[0055] The reaction Re is advantageously carried out at temperatures between 10°C and 30°C, and more advantageously between 20°C and 25°C.
[0056] Preferably, for reaction Re, the coefficient α = (moles of alkali metal and / or alkaline earth metal) hypohalides / (moles of nonionic monomers of polymer P1, such as acrylamide, methacrylamide, N,N-dimethylacrylamide, acrylonitrile or mixtures thereof) is 0.1 to 1.0, and the coefficient β = (moles of alkali metal and / or alkaline earth metal) hydroxides / (moles of alkali metal and / or alkaline earth metal) hypohalides is 0.5 to 4.0.
[0057] The reaction Re is advantageously carried out by adding polymer P1 in the form of solid particles to an aqueous solution M1. Preferably, the solid particles of polymer P1 are in the form of powder, microspheres, solid particles in an oily suspension, or solid particles in an aqueous suspension.
[0058] These different forms of solid particles were obtained using techniques known to those skilled in the art.
[0059] The powder form of polymer P1 can be obtained by gel polymerization, precipitation polymerization or spray drying of reverse emulsion polymers.
[0060] Microspheres of polymer P1 are advantageously obtained by reverse suspension polymerization.
[0061] An oily suspension of solid particles of polymer P1 can be obtained by distillation of the reverse emulsion polymer or by suspension of the polymer in oil. This oily suspension may contain 10-60% by weight of polymer P1 particles.
[0062] An aqueous suspension of solid particles of polymer P1 is advantageously obtained by dispersion polymerization (in brine) or by suspension of the polymer in brine. The aqueous suspension may contain 10 to 50% by weight of polymer P1 particles.
[0063] Even more preferably, polymer P1 is added to the reaction medium in the form of powder produced by gel polymerization or microbeads produced by reverse suspension polymerization.
[0064] When polymer P1 is in powder form, it is preferably dispersed and dissolved in aqueous solution M1 by means of a device for dispersing and grinding the polymer, particularly a PSU (polymer chip unit, document WO2011107683), which is supplied by a loop from aqueous solution M1. Those skilled in the art know how to adjust the production equipment of this type of device to be resistant to aqueous solution M1 containing hydroxides and hypohalides.
[0065] For reaction Re, 0.1 to 20% by weight, more preferably 0.3 to 10% by weight, and even more preferably 0.5 to 3.0% by weight of solid particles of polymer P1 are added to aqueous solution M1 relative to the weight of aqueous solution M1.
[0066] Advantageously, at the end of reaction Re and before its injection into the fiber suspension, polymer P2 can be functionalized with a compound containing at least one aldehyde functional group to produce polymer P3, for example by adding a compound containing at least one aldehyde functional group. Preferably, the compound containing at least one aldehyde functional group is glyoxal.
[0067] Preferably, before injecting the fiber suspension, the pH of the reaction mixture containing polymer P2 obtained from reaction Re can be adjusted to 0.5 to 7.5, more preferably 1.0 to 3.0, by adding acid. Those skilled in the art know how to adjust the pH of this type of reaction medium. pH adjustment is advantageously carried out without the formation of polymer P3.
[0068] According to a preferred embodiment, after homogenizing the fiber suspension in a dilution pump (fan pump), polymer P2 (or P3) is introduced into white water and / or slurry and / or a mixture formed by white water and slurry.
[0069] Advantageously, polymer P2 (or P3) can also be introduced in the papermaking process at the forming wire, for example by spraying or in the form of foam, or at the sizing machine (coating machine).
[0070] Advantageously, 0.1 to 10 kg.t is added to the fiber suspension. -1 Preferably, the dosage is 0.2 to 5.0 kg / t. -1 The polymer P2 (or P3).
[0071] Fiber suspensions may include various cellulose fibers that can be used: virgin fibers, regenerated fibers, chemical pulps, mechanical pulps, microfibrillated cellulose, or nanofibrillated cellulose. Fiber suspensions also include the use of these different cellulose fibers and all types of fillers, such as TiO2, CaCO3 (crushed or precipitated), kaolin, organic fillers, and mixtures thereof.
[0072] Polymer P2 or P3 can be combined with other products for use in papermaking processes, such as inorganic or organic coagulants, dry strength agents, wet strength agents, natural polymers such as starch or carboxymethyl cellulose (CMC), inorganic microparticles such as bentonite microparticles and colloidal silica microparticles, and organic polymers of any ionic type (nonionic, cationic, anionic, or amphoteric) and which may be (but are not limited to) linear, branched, crosslinked, hydrophobic, or associated.
[0073] The following examples illustrate the present invention, but do not limit its scope. Detailed Implementation
[0074] Programs used for application testing:
[0075] a) Type of slurry used
[0076] Regenerated fiber pulp:
[0077] Wet pulp is obtained by disintegrating the dry pulp to achieve a final water concentration of 1% by weight. This is a neutral pH pulp composed of 100% recycled paperboard fibers.
[0078] b) Drainage performance assessment (DDA)
[0079] The DDA ("Dynamic Drainage Analyzer") automatically measures the time (in seconds) required for vacuum removal of fiber suspension deposited on fabric. The polymer is added to the wet slurry (0.6 L of 1.0 wt% slurry) in the DDA cylinder under stirring at 1000 rpm.
[0080] -T=0s: Stirring slurry
[0081] -T = 20s: Add polymer
[0082] -T=30s: Stop stirring and apply at 200mbar (1bar=10mbar). 5 Vacuum drainage for 70 seconds under pressure (Pa).
[0083] The pressure under the fabric is recorded as a function of time. When all water has been removed from the fiber pad, air passes through the pad, causing a sudden change in the slope of the curve representing the pressure under the fabric as a function of time. The time (in seconds) recorded at the point of slope change corresponds to the drainage time. The shorter the time, the better the vacuum drainage effect.
[0084] c) Performance under DSR (dry strength) application, basis weight 90 g.m - 2
[0085] Collect the required amount of slurry to obtain a weight of 90g.m -2 Paper (sheet).
[0086] Wet slurry is introduced into the barrel of the dynamic paper forming machine and agitation is maintained. Various components of the system are then injected into the slurry in a predetermined sequence. Typically, the contact time between each polymer addition is 30 to 45 seconds.
[0087] The paper forming machine employs an automatic dynamic paper forming process: absorbent paper and forming fabric are placed in the rollers of the dynamic paper forming machine, and then the rollers begin to rotate at 1000 rpm, forming a water wall. The treated pulp is spread on the water wall to form a fiber mat on the forming fabric.
[0088] Once the water is drained, the fiber pad is recycled, pressed at an output pressure of 4 bar, and then dried at 117°C. The resulting paper is left overnight in a room with controlled humidity and temperature (50% relative humidity and 23°C). The dry strength properties of all paper obtained through this process are then measured.
[0089] Bursting strength (bursting index) was measured using a Messier Buchel M 405 bursting strength tester according to standard TAPPI T403 om-02. Results are expressed in kPa or as a percentage of a reference value. (kPa·m) 2 The burst strength index, expressed as / g, is determined by dividing this value by the gram weight of the paper being tested.
[0090] According to standard TAPPI T494 om-01, the breaking length was measured in the longitudinal (machine direction) (DBL SM) and transverse (DBL ST) directions using a test AX traction device. The results are expressed in km or as a percentage of a reference value.
[0091] Test products in application testing:
[0092] Polymer P1
[0093] Synthesis of polymer P1-A
[0094] 310 g of water was introduced into a 1-liter reactor equipped with a mechanical stirrer, thermometer, condenser, and nitrogen immersion rod. The pH of the reaction medium was adjusted to 3.3 using a pH buffer solution (30 wt% NaOH aqueous solution and 75 wt% H3PO4 aqueous solution). The medium was heated using a water bath and maintained at a temperature of 79–81 °C. In two consecutive liquid pours, 400 g of 50% acrylamide, 237.8 g of water, and 2.40 g of 100% sodium hypophosphite (Pour 1) were added over 180 minutes. In Liquid Pour 2, 0.48 g of 100% sodium persulfate and 48 g of water were added over 180 minutes. After the liquid pours were completed, the polymer solution was incubated at 80 °C for 120 minutes.
[0095] The resulting polymer P1-A solution had a pH of 5.7, a weight concentration of 20%, and a viscosity of 6000 cps.
[0096] Polymer P1-B: Acrylamide homopolymer in microbead form, sold by SNF under the trade name: Flobeads TM AB300H.
[0097] Polymer P1-C: Acrylamide homopolymer in powder form, sold by SNF under the trade name: FlopamTM FA920BPM.
[0098] Polymers P1-A (aqueous solution), P1-B (microbeads), and P1-C (powder) are all homopolymers of acrylamide, differing only in their physical form.
[0099] Polymer P2
[0100] Synthesis of polymer P2-A
[0101] A 10% by weight P1-A aqueous solution was prepared by diluting 20g of a 20% by weight P1-A aqueous solution with 20g of water. The polymer solution was then heated to 50°C.
[0102] Based on the reaction coefficients α (0.5) and β (2.0), an aqueous solution of 14.29 g of 14.6% (by weight in water) sodium hypochlorite (NaOCl) and 7.5 g of 30% (by weight in water) soda ash was prepared. The aqueous solution of sodium hypochlorite and soda ash was added to the polymer P1-A solution while it was at 50°C. After reacting for 30 seconds, 138.20 g of water was added. Polymer P2-A with a concentration of 2% by weight was obtained.
[0103] Synthesis of polymers P2-B and P2-C
[0104] Based on the coefficients α (0.5) and β (2.0) of the reaction Re, an aqueous solution M1 of 3.11 g of 14.6% (by weight in water) sodium hypochlorite (NaOCl) and 1.63 g of 30% (by weight in water) soda ash was prepared. Then 37.7 g of water was added.
[0105] Under ambient temperature and stirring, 0.87 g of polymer P1-B or P1-C was added to aqueous solution M1. The polymer suspension was dissolved in an aqueous solution of sodium hypochlorite and soda ash and reacted for 120 minutes. Solutions of polymer P2-B or P2-C were obtained, with a final polymer weight concentration of 2%.
[0106] Application testing
[0107] Drainage performance (DDA)
[0108]
[0109] Table 1: Drainage as a polymer function
[0110] Improvements in drainage were observed using polymers P2-B and P2-C (as opposed to polymer P2-A).
[0111] Performance in DSR (dry strength) applications
[0112]
[0113] Table 2: Dry strength as a polymer function
[0114] The bursting resistance was improved by using polymers P2-B and P2-C. The same trend was observed in the fracture length measurements in both the longitudinal (DBL SM) and transverse (DBLST) directions.
Claims
1. A method for producing paper or paperboard from a fiber suspension, comprising the following steps: a) Inject polymer P2 into the fiber suspension. b) Forming paper or paperboard, c) Dry paper or cardboard. Prior to step a), polymer P2 is prepared from a water-soluble polymer P1 in solid particulate form, wherein P1 is a water-soluble polymer of at least one nonionic monomer selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile. The polymer P2 is obtained through reaction Re, which includes adding and dissolving solid particles of the water-soluble polymer P1 in an aqueous solution M1, wherein the aqueous solution M1 comprises: (i) alkali metal hydroxides or alkaline earth metal hydroxides or mixtures thereof, (ii) alkali metal hypohalides or alkaline earth metal hypohalides or mixtures thereof. After adding water-soluble polymer P1 particles, the reaction time of Re is 10 seconds to 5 hours.
2. The method according to claim 1, characterized in that... The water-soluble polymer P1 contains at least 50 mol% of at least one nonionic monomer selected from acrylamide, methacrylamide, N,N-dimethylacrylamide, and acrylonitrile.
3. The method according to claim 1 or 2, characterized in that... The water-soluble polymer P1 is a homopolymer or copolymer of acrylamide or methacrylamide.
4. The method according to claim 1 or 2, characterized in that... For the reaction Re, the coefficient α = the number of moles of the hypohalide / the number of moles of the nonionic monomer of the water-soluble polymer P1 is 0.1 to 1.0, and the coefficient β = the number of moles of the hydroxide / the number of moles of the hypohalide is 0.5 to 4.
0.
5. The method according to claim 1 or 2, characterized in that... The solid particles of the water-soluble polymer P1 are in the form of powder, microspheres, solid particles in an oily suspension, or solid particles in an aqueous suspension.
6. The method according to claim 1 or 2, characterized in that... The solid particles of the water-soluble polymer P1 are in the form of powder produced by gel polymerization or microbeads produced by reverse suspension polymerization.
7. The method according to claim 6, characterized in that... When the solid particles of the water-soluble polymer P1 are in powder form, they are dispersed in an aqueous solution M1 by means of a device for dispersing and grinding the polymer, the device being supplied by a loop of the aqueous solution M1.
8. The method according to claim 1 or 2, characterized in that... 0.1 to 20% by weight of solid particles of water-soluble polymer P1 are added to aqueous solution M1 relative to the weight of aqueous solution M1.
9. The method according to claim 1 or 2, characterized in that... At the end of reaction Re, and before being injected into the fiber suspension, polymer P2 is functionalized with a compound containing at least one aldehyde functional group to produce polymer P3.
10. The method according to claim 9, characterized in that... The compound containing at least one aldehyde functional group is glyoxal.
11. The method according to claim 1 or 2, characterized in that... Before being injected into the aqueous suspension, the pH of the reaction mixture containing polymer P2 obtained from the reaction Re is adjusted to between 0.5 and 7.5 by adding acid.
12. The method according to claim 1 or 2, characterized in that... After homogenizing the fiber suspension in a dilution pump, the polymer P2 is introduced into white water and / or slurry and / or a mixture formed from white water and slurry.
13. The method according to claim 1 or 2, characterized in that... Step a) is carried out within 24 hours from the time the solid particles of the water-soluble polymer P1 are added to the aqueous solution M1.
14. The method according to claim 1 or 2, characterized in that The reaction Re is advantageously carried out at a temperature of 10 to 30°C.
15. The method according to claim 1 or 2, characterized in that... 0.3 to 10% by weight of solid particles of polymer P1 are added to aqueous solution M1 relative to the weight of aqueous solution M1.
Citation Information
Patent Citations
Improved apparatus for dispersing a water-soluble polymer
EP2536489A1
Catonic acrylamide polymers and the applications of these polymers
US5292821A
Method of producing high dry strength paper and cardboard and paper and cardboard thus obtained
WO2006075115A2
Improved apparatus for dispersing a water-soluble polymer
WO2011107683A1
Method of Producing High Dry Strength Paper and Cardboard and Paper and Cardboard Thus Obtained
US20080196851A1