Process for the condensation of ketimines and metal-organic frameworks and methods for their preparation
By using metal-organic framework catalysts to carry out ketone-amine condensation reactions at low temperatures, the problems of high temperature and high cost in existing technologies are solved, and the products are easily separated and in high yield. This method is suitable for the synthesis of polyethylene and 4-methyl-1-pentene.
Patent Information
- Application Number
- CN202210780025.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-04
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-07-04
AI Technical Summary
The existing technology for preparing 2,6-bis(imino)pyridine compounds involves high reaction temperatures and complex post-processing, and the products are not easy to separate.
Using metal-organic framework materials as catalysts, ketone-amine condensation reactions are carried out at lower temperatures, and the products are easily separated through specific solvents and post-treatment steps. The catalyst can be reused repeatedly.
This method enables easy separation of the catalyst and product, reduces production costs, and improves the yield and synthesis efficiency of 2,6-bis(imino)pyridine compounds. It is suitable for the synthesis of ligands for polyethylene and 4-methyl-1-pentene.
Smart Images

Figure CN117402107B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of bis(imino)pyridine compounds, specifically to a method for ketamine condensation reaction and a metal-organic framework material and its preparation method. Background Technology
[0002] Polyethylene is a very important synthetic plastic. It is classified into high-density polyethylene (HDPE), linear low-density polyethylene (LLDPE), and low-density polyethylene (LDPE). LLDPE is produced by free radical polymerization of ethylene monomers under pressures exceeding 1000 atmospheres, requiring substantial investment in equipment. HDPE and LLDPE, on the other hand, can be produced from ethylene monomers under low pressure using Ziegler-Natta or metallocene catalysts, which is currently the main industrial method for polyethylene production. In 1990, Exxon first used metallocene catalysts to produce polyethylene, which can prepare polyolefin materials (syndiotactic polystyrene and polypropylene, etc.) that cannot be prepared by Ziegler-Natta catalysts. Regarding polyethylene, compared to Ziegler-Natta catalysts, metallocene catalysts can produce polymer materials with more uniform molecular weight. Currently, major companies such as Dow Chemical and Mitsui Petrochemical have commercialized metallocene-catalyzed polyethylene products. Later transition metal catalysts have strong β-H elimination capabilities, but in ethylene polymerization, they can only produce oligomers. Brookhart et al. discovered that complex catalysts formed by Ni(II) and Pd(II) with sterically hindered diimines as ligands can prepare polyethylene with larger molecular weights. These catalysts are more stable and easier to prepare than Ziegler-Natta catalysts or metallocene catalysts. They can catalyze the copolymerization of olefins with polar monomers, improving the compatibility of polyolefins with other materials and making polyolefin materials easier to modify and utilize. Therefore, the synthesis of 2,6-bis(imino)pyridine compounds becomes a key factor.
[0003] The commonly used industrial method for synthesizing 2,6-bis(imino)pyridine compounds involves using p-toluenesulfonic acid, formic acid, or acetic acid as catalysts to react pyridine diones with aniline derivatives (J.Am.Chem.Soc.1998,120,4049; Angew.Chem.,Int.Ed.Engl.1999,38,428; J.Am.Chem.Soc.1999,121,8728; CN01105268.8; WO 01 / 07491A1). These catalytic reactions must be carried out at 110-150℃, and the post-processing is relatively complex.
[0004] Therefore, it is of great significance to study and develop a method for preparing 2,6-bis(imino)pyridine compounds. Summary of the Invention
[0005] The purpose of this invention is to overcome the problems in the prior art of preparing 2,6-bis(imino)pyridine compounds, such as high reaction temperature, complex post-processing, and difficulty in separating the products.
[0006] To achieve the above objectives, the first aspect of the present invention provides a method for a ketamine condensation reaction, the method comprising carrying out a ketamine condensation reaction of substrate 1 and substrate 2 in the presence of a catalyst and solvent A, wherein substrate 1 is an acyl-substituted pyridine and substrate 2 is an aniline compound, wherein the catalyst is a metal-organic framework material, the ligand of the metal-organic framework material is provided by a substance with the structure shown in formula (1), and the coordinating metal M is selected from Zn, Co and Zr; in formula (1), M' is selected from Li, Na, K, Cs, Ca and Mg;
[0007]
[0008] A second aspect of the present invention provides a metal-organic framework material, which is a metal-organic framework material as defined in any one of claims 1-5 or an acidified product as described in any one of claims 6-9.
[0009] The third aspect of the present invention provides a method for preparing a metal-organic framework material, wherein the preparation method is the method for preparing a metal-organic framework material as defined in any one of claims 6-9.
[0010] Compared with the prior art, the technical solution provided by the present invention has at least the following advantages:
[0011] (1) The metal-organic framework material provided by the present invention has a stable structure and good performance. Furthermore, the catalyst and the product are easy to separate and can be reused repeatedly, which is more environmentally friendly and has a lower cost. It has a very broad application prospect in future industrial applications.
[0012] (2) The catalyst provided by the present invention can be used in the synthesis of 2,6-bis(imino)pyridine compounds. The yield of the catalyst of the present invention is much higher than that of industrial catalysts (p-toluenesulfonic acid, formic acid, acetic acid). Moreover, after the catalyst of the present invention is used repeatedly 10 times, the yield of 2,6-bis(imino)pyridine compounds remains basically unchanged.
[0013] (3) The synthesis method of the 2,6-bis(imino)pyridine compounds prepared in this invention serves as an important ligand for the synthesis of polyethylene catalysts and an important ligand for the synthesis of 4-methyl-1-pentene, thereby improving the synthesis efficiency, reducing the synthesis cost, and greatly reducing the production cost of polyolefins. Detailed Implementation
[0014] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0015] The first aspect of the present invention provides a method for a ketamine condensation reaction, the method comprising carrying out a ketamine condensation reaction of substrate 1 and substrate 2 in the presence of a catalyst and solvent A, wherein substrate 1 is an acyl-substituted pyridine and substrate 2 is an aniline compound, wherein the catalyst is a metal-organic framework material, the ligand of the metal-organic framework material is provided by a substance with the structure shown in formula (1), and the coordinating metal M is selected from Zn, Co and Zr; in formula (1), M' is selected from H, Li, Na, K, Cs, Ca and Mg;
[0016]
[0017] According to some embodiments of the present invention, the metal-organic framework material has a structure as shown in formula (2):
[0018]
[0019] According to some embodiments of the present invention, the specific surface area of the metal-organic framework material is 200-800 m². 2 / g, total pore volume is 1-5mL / g, and most probable pore size is 0.1-3nm.
[0020] Preferably, the specific surface area of the metal-organic framework material is 300-800 m². 2 / g, more preferably 300-500m 2 / g, with a total pore volume of 1.1-3mL / g, more preferably 1.2-2.5mL / g, and a most probable pore size of 0.2-2.5nm, more preferably 0.3-1.5nm.
[0021] According to some embodiments of the present invention, substrate 1 is at least one of 2,6-dicarboxypyridine, 2,6-diacetylpyridine, and 2,6-dipropionylpyridine.
[0022] According to some embodiments of the present invention, substrate 2 is at least one of aniline, 4-fluoroaniline and 4-chloroaniline.
[0023] According to some embodiments of the present invention, the weight ratio of substrate 1, substrate 2, metal-organic framework material and solvent A is (1-5):(0.5-20):(0.01-10):(1-200), preferably (1-4):(1.5-10):(0.5-1):(20-100).
[0024] According to some embodiments of the present invention, the conditions for the ketamine condensation reaction include: a temperature of 40-60°C, preferably 40-45°C; and a time of 1-12 h, preferably 1-8 h.
[0025] According to some embodiments of the present invention, solvent A is at least one of toluene, n-hexane, cyclohexane, petroleum ether, and dioxane, preferably at least one of toluene, n-hexane, and cyclohexane.
[0026] According to some embodiments of the present invention, the method further includes solid-liquid separation, concentration and recrystallization of the product of the ketamine condensation reaction.
[0027] According to some embodiments of the present invention, the method for preparing the metal-organic framework material includes the following steps:
[0028] (1) In the presence of a first solvent and a monobasic acid, the compound shown in formula (3) is subjected to a coordination reaction with the metal source to be coordinated, wherein the monobasic acid has more than 4 carbon atoms.
[0029] (2) Optionally, the product of the coordination reaction is acidified;
[0030] In formula (II), M” is selected from one of Li, Na, K, Cs, Ca and Mg; the metal in the metal source to be coordinated is selected from one of Zr, Cr and Al;
[0031]
[0032] According to some embodiments of the present invention, in step (1), the conditions of the coordination reaction may include: a temperature of 80-200°C, preferably 100-150°C; and a time of 5-30h, preferably 10-24h.
[0033] According to some embodiments of the present invention, the molar ratio of the compound shown in formula (3), the metal source to be coordinated, the monobasic acid and the first solvent can be 1:(1.5-5):(0-20):(1-100); preferably 1:(2-3):(0-10):(2-50).
[0034] In this invention, the addition of an acid (such as acetic acid) in the coordination reaction can act as a template agent, forming catalytically active vacancies on the crystal surface, which can then be used for subsequent modification.
[0035] According to some embodiments of the present invention, the metal source to be coordinated may be selected from ZrCl4, Co(NO3)2 6H2O and Zn(acac)4.
[0036] According to some embodiments of the present invention, the first solvent may be selected from at least one of N,N-dimethylformamide, dimethyl sulfoxide and N-methylpyrrolidone, preferably N,N-dimethylformamide.
[0037] According to some embodiments of the present invention, the monocarboxylic acid is selected from carboxylic acids containing a benzene ring, preferably from C6-C10 carboxylic acids containing a benzene ring, and more preferably from benzoic acid and / or phenylacetic acid.
[0038] In this invention, there are no particular limitations on the post-processing of the coordination reaction in step (1), as long as it meets the requirements of this invention. For example, it can be carried out as follows: the materials of the coordination reaction are centrifuged and filtered (1000-10000 rpm), and washed with a washing solvent (e.g., DMF and methanol in sequence) (which can be repeated 2-5 times); then dried at 90-180℃ for 5-10 hours. There are no particular limitations on the type and amount of washing solvent, as long as it meets the requirements of this invention.
[0039] According to some embodiments of the present invention, in step (1), the preparation step of the compound represented by formula (3) includes: in the presence of a second solvent and a metal halide, terephthalic acid is subjected to a substitution reaction with chlorosulfonate to obtain the compound represented by formula (3).
[0040] According to some embodiments of the present invention, the conditions for the substitution reaction may include: a temperature of 30-100°C, preferably 40-80°C; and a time of 5-30 h, preferably 10-24 h.
[0041] According to some embodiments of the present invention, the molar ratio of terephthalic acid, chlorosulfonate and metal halide can be 1:(0.5-2):(0.01-1), preferably 1:(0.8-1.2):(0.05-0.5).
[0042] According to some embodiments of the present invention, the metal halide is selected from at least one of RuCl3, FeCl3, AlCl3 and PdCl2, preferably selected from at least one of RuCl3, FeCl3 and AlCl3.
[0043] According to some embodiments of the present invention, the second solvent is selected from at least one of dichloromethane, 1,2-dichloromethane and chloroform; preferably dichloromethane.
[0044] According to some embodiments of the present invention, the amount of the second solvent used is 20-100 mL, preferably 30-80 mL, relative to 1 g of terephthalic acid.
[0045] There are no particular limitations on the post-processing operations of the above substitution reaction, as long as they meet the requirements of this invention. Preferably, before obtaining the compound shown in formula (3), the following post-processing operations can be performed: the material from the substitution reaction is filtered and washed with a washing solvent (e.g., dichloromethane and methanol sequentially) (this can be repeated 2-5 times); then dried at 60-100°C for 5-10 hours. There are no particular limitations on the type and amount of washing solvent, as long as they meet the requirements of this invention.
[0046] According to some embodiments of the present invention, in step (2), the acidification is carried out in the presence of an inorganic acid, the concentration of which is 0.1-18.4 mol / L, preferably 1-10 mol / L.
[0047] In this invention, the inorganic acid can be selected from at least one of hydrochloric acid, sulfuric acid, and nitric acid, preferably hydrochloric acid. The nitric acid is preferably dilute nitric acid (concentration can be 0.1-1 mol / L). The sulfuric acid is preferably dilute sulfuric acid (concentration can be 0.1-5 mol / L).
[0048] According to some embodiments of the present invention, the acidification conditions may include: a temperature of -10°C to -100°C, preferably 0°C to 50°C; and a time of 5-30 hours, preferably 10-24 hours.
[0049] According to some embodiments of the present invention, the amount of the inorganic acid used may be 1-10 mol, preferably 1-5 mol, relative to each mole of the compound represented by formula (3).
[0050] Those skilled in the art will understand that after acidification, M” in formula (3) is converted from metal to H, thereby obtaining a strongly acidic sulfonylbenzene ring metal-organic framework material.
[0051] In this invention, before obtaining the metal-organic framework material, the following post-processing operation can be performed: the acidified material system is filtered, and the obtained solid is washed with water (this can be repeated 2-5 times). There is no particular limitation on the amount of water used for washing.
[0052] The synthetic route for 2,6-bis(imino)pyridine compounds in this invention is shown below:
[0053]
[0054] Among them, A 1 and A 2Each independently is H and / or C 1-6 Hydrocarbon groups (e.g., methyl, ethyl, isopropyl, etc.), R 1 R 2 R 3 R 4 R 5 Each is independently H and / or a halogen (e.g., Cl, F, Br, I).
[0055] A second aspect of the present invention provides a metal-organic framework material, which is a metal-organic framework material as defined above or an acidified product as described above.
[0056] A second aspect of the present invention provides a method for preparing a metal-organic framework material, which is the method for preparing a metal-organic framework material as defined above.
[0057] The present invention will be described in detail below through embodiments.
[0058] The raw materials and solvents used in the following examples were all commercially available;
[0059] Specific surface area, total pore volume, and most probable pore size were obtained by nitrogen physical adsorption (purchased from Anton Paconta Instruments, model Autosorb-iQ).
[0060] Example 1
[0061] (1) Add 0.8g of FeCl3, 16.6g of terephthalic acid, 16.5g of sodium chlorosulfonate and 1000mL of dichloromethane to the reaction flask, carry out the substitution reaction at 50℃ for 5h, filter, wash the solid three times with 100mL of dichloromethane and three times with 100mL of methanol, and dry at 80℃ for 8h to obtain a white powder (confirmed by NMR to be the compound shown in formula (3), where M” is Na) 24.9g. Then, carry out the coordination reaction (calcination crystallization) of Zn(acac)4, the compound shown in formula (3), DMF and benzoic acid at a molar ratio of 2.5:1:40:6 at 95℃ for 24h, centrifuge and filter at 4000rpm, wash the solid three times with 50mL of DMF and three times with 50mL of methanol, and dry the solid at 105℃ for 8h to obtain a white solid (metal-organic framework material).
[0062] (2) Add 26 mL of 5 mol / L hydrochloric acid to the white solid obtained in step (1) and acidify it for 3 h under stirring at 25 °C; filter and wash the solid three times with 50 mL of water to obtain the acidified metal-organic framework material (Zn is the metal center).
[0063] The specific surface area is 492.3 m². 2 / g, total pore volume = 2.5mL / g, most probable pore size is 0.6nm.
[0064] Example 2
[0065] (1) Add 1.04 g of RuCl3, 16.6 g of terephthalic acid, 16.5 g of sodium chlorosulfonate and 1000 mL of dichloromethane to the reaction flask, carry out the substitution reaction at 50 °C for 5 h, filter, wash the solid three times with 100 mL of dichloromethane and three times with 100 mL of methanol, and dry at 80 °C for 8 h to obtain a white powder (confirmed by NMR to be the compound shown in formula (3), where M” is Na) 24.9 g. Then, Co(NO3)2 6H2O, the compound shown in formula (3), DMF and benzoic acid are carried out in a molar ratio of 2:1:5:0.5 at 95 °C for 24 h, centrifuge and filter at 5000 rpm, wash the solid three times with 50 mL of DMF and three times with 50 mL of methanol, and dry the solid at 105 °C for 6 h to obtain a white solid (metal-organic framework material).
[0066] (2) Add 22 mL of 5 mol / L hydrochloric acid to the white solid obtained in step (1) and acidify it for 3 h under stirring at 25 °C; filter and wash the solid three times with 50 mL of water to obtain the acidified metal-organic framework material (Co is the metal center).
[0067] Specific surface area is 418 m² 2 / g, total pore volume = 1.9mL / g, most probable pore size is 0.8nm.
[0068] Example 3
[0069] (1) Add 1.04 g of RuCl3, 16.6 g of terephthalic acid, 16.5 g of sodium chlorosulfonate and 1000 mL of dichloromethane to the reaction flask, and carry out the substitution reaction at 50 °C for 24 h. After filtration, the solid is washed three times with 100 mL of dichloromethane and three times with 100 mL of methanol, and dried at 80 °C for 8 h to obtain 24.9 g of white powder (confirmed by NMR to be the compound shown in formula (3), where M” is Na). Then, ZrCl4, the compound shown in formula (3), DMF and benzoic acid are subjected to coordination reaction (calcination crystallization) at 95 °C in a molar ratio of 3:1:80:12 for 24 h. After centrifugation and filtration at 6000 rpm, the solid is washed three times with 50 mL of DMF and three times with 50 mL of methanol, and dried at 105 °C for 5 h to obtain a white solid (metal-organic framework material).
[0070] (2) Add 26 mL of 5 mol / L hydrochloric acid to the white solid obtained in step (1) and acidify it for 1 h under stirring at 50 °C; filter and wash the solid three times with 50 mL of water to obtain the acidified metal-organic framework material (Zr is the metal center).
[0071] Specific surface area is 355 m² 2 / g, total pore volume = 1.5mL / g, most probable pore size is 1.2nm.
[0072] Test Example 1
[0073] The metal-organic framework materials prepared in the above examples and comparative examples were used as catalysts to evaluate their catalytic performance in the preparation of 2,6-bis(imino)pyridine compounds. 0.49 g of 2,6-diacetylpyridine, 0.89 g of 4-fluoroaniline, and 0.3 g of the metal-organic framework material were added to a 100 mL flask. 40 mL of toluene was added, and the mixture was heated to 42 °C. The reaction was stopped after 8 h. The reaction product was then filtered to obtain a single-use metal-organic framework material. The filtered solution was concentrated, and the solid obtained after concentration was recrystallized from methanol (the solid was dissolved in methanol at 80 °C, and the temperature was gradually lowered to 30 °C-0 °C, causing crystals to gradually precipitate, which were then separated by filtration). The solids were weighed, and the yield of the 2,6-bis(imino)pyridine compounds was calculated. The results are shown in Table 1.
[0074] Test Example 2
[0075] The test was conducted according to the method in Test Example 1, except that 4-fluoroaniline was replaced with an equimolar amount of 4-chloroaniline.
[0076] Test Example 3
[0077] This test example illustrates the stability of the metal-organic framework materials prepared in the above embodiments and comparative examples as catalysts.
[0078] 2,6-bis(imino)pyridine compounds were prepared according to the method of Test Example 1, except that the metal-organic framework material obtained from the filtration in Test Example 1 was reused. The average yield of 2,6-bis(imino)pyridine compounds after 5 reuses was calculated, and the results are shown in Table 1. The number of reuses required to reduce the yield of 2,6-bis(imino)pyridine compounds to 95% was also investigated, and the results are shown in Table 1.
[0079] The formula for calculating the yield of 2,6-bis(imino)pyridine compounds is: (amount of 2,6-bis(imino)pyridine compound) ÷ (amount of 2,6-diacetylpyridine) × 100%.
[0080] Table 1
[0081]
[0082] Comparative Test Case 1
[0083] Add 0.49 g of 2,6-diacetylpyridine, 0.89 g of 4-fluoroaniline, and 2.6 mg of p-toluenesulfonic acid to a 100 mL flask. Heat to reflux (110-120 °C) for 24 h. After the reaction is complete, wash twice with saturated sodium carbonate solution and twice with distilled water. Extract the aqueous phase twice with diethyl ether. Dry and concentrate the solid and recrystallize it from methanol (dissolve the solid in methanol at 80 °C, gradually cool to 30 °C-0 °C, crystals gradually precipitate, and then filter to separate). The yield is 80%.
[0084] A comparison of Test Example 1 with Comparative Test Example 1 of this application shows that the method of this invention not only improves the yield of 2,6-bis(imino)pyridine compounds but also reduces the reaction temperature and energy consumption. Furthermore, the catalyst of this invention can be recycled multiple times while maintaining a substantially constant yield, thus reducing production costs. In contrast, the catalyst (p-toluenesulfonic acid) in Comparative Test Example 1 cannot be reused, and the purification process for 2,6-bis(imino)pyridine compounds is complex, increasing production costs.
[0085] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.
Claims
1. A method for ketone-amine condensation reaction, characterized in that, The method includes subjecting substrate 1 and substrate 2 to a ketamine condensation reaction in the presence of a catalyst and solvent A, wherein substrate 1 is at least one of 2,6-dicarboxypyridine, 2,6-diacetylpyridine and 2,6-dipropionylpyridine, and substrate 2 is at least one of aniline, 4-fluoroaniline and 4-chloroaniline, wherein the catalyst is a metal-organic framework material, the ligand of the metal-organic framework material is provided by a substance with the structure shown in formula (1), and the coordinating metal M is selected from one of Zn, Co and Zr; in formula (1), M' is selected from one of Li, Na, K and Cs; (1); The specific surface area of the metal-organic framework material is 200-800 m². 2 / g, total pore volume is 1-5mL / g, most probable pore size is 0.1-3nm; The preparation method of the metal-organic framework material includes the following steps: (1) In the presence of a first solvent and a monobasic acid, the compound shown in formula (3) is subjected to a coordination reaction with the metal source to be coordinated, wherein the monobasic acid is benzoic acid and / or phenylacetic acid; (2) Acidify the product of the coordination reaction; In formula (3), M'' is selected from one of Li, Na, K, and Cs; the metal in the metal source to be coordinated is selected from one of Zn, Co, and Zr. (3)。 2. The method according to claim 1, wherein, The metal-organic framework material has a structure as shown in formula (2): (2)。 3. The method according to claim 1, wherein, The specific surface area of the metal-organic framework material is 300-800 m². 2 / g, with a total pore volume of 1.1-3mL / g and a most probable pore size of 0.2-2.5nm.
4. The method according to claim 1, wherein, The specific surface area of the metal-organic framework material is 300-500 m². 2 / g.
5. The method according to claim 1, wherein, The total pore volume of the metal-organic framework material is 1.2-2.5 mL / g.
6. The method according to claim 1, wherein, The most probable pore size of the metal-organic framework material is 0.3-1.5 nm.
7. The method according to claim 1, wherein, The weight ratio of substrate 1, substrate 2, metal-organic framework material and solvent A is (1-5):(0.5-20):(0.01-10):(1-200). And / or, the conditions for the ketone-amine condensation reaction include: a temperature of 40-60℃; and a time of 1-12h; And / or, solvent A is at least one of toluene, n-hexane, cyclohexane, petroleum ether, and dioxane.
8. The method according to claim 1, wherein, The weight ratio of substrate 1, substrate 2, metal-organic framework material and solvent A is (1-4):(1.5-10):(0.5-1):(20-100).
9. The method according to claim 1, wherein, The conditions for ketone-amine condensation reaction include a temperature of 40-45℃.
10. The method according to claim 1, wherein, The conditions for ketone-amine condensation reaction include a time of 1-8 hours.
11. The method according to claim 1, wherein, Solvent A is at least one of toluene, n-hexane, and cyclohexane.
12. The method according to claim 1, wherein, The method also includes solid-liquid separation, concentration, and recrystallization of the product of the ketone-amine condensation reaction.
13. The method according to claim 1, wherein, In step (1), the conditions for the coordination reaction include: a temperature of 80-200℃ and a time of 5-30h; And / or, the molar ratio of the compound shown in formula (3), the metal source to be coordinated, the monobasic acid, and the first solvent is 1:(1.5-5):(0.5-20):(1-100); And / or, the metal source to be coordinated is selected from one of ZrCl4, Co(NO3)26H2O and Zn(acac)4; And / or, the first solvent is selected from at least one of N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone.
14. The method according to claim 1, wherein, In step (1), the conditions for the coordination reaction include a temperature of 100-150℃.
15. The method according to claim 1, wherein, In step (1), the conditions for the coordination reaction include a time of 10-24 hours.
16. The method according to claim 1, wherein, The molar ratio of the compound shown in formula (3), the metal source to be coordinated, the monobasic acid and the first solvent is 1:(2-3):(0.5-10):(2-50).
17. The method according to claim 1, wherein, The first solvent is N,N-dimethylformamide.
18. The method according to claim 1, wherein, In step (1), the preparation steps of the compound shown in formula (3) include: in the presence of a second solvent and a metal halide, terephthalic acid and chlorosulfonate are subjected to a substitution reaction to obtain the compound shown in formula (3).
19. The method according to claim 18, wherein, The conditions for the substitution reaction include: a temperature of 30-100℃ and a time of 5-30h.
20. The method according to claim 18, wherein, The conditions for the substitution reaction include a temperature of 40-80℃.
21. The method according to claim 18, wherein, The conditions for the substitution reaction include a time of 10-24 hours.
22. The method according to claim 18, wherein, The molar ratio of terephthalic acid, chlorosulfonate, and metal halide is 1:(0.5-2):(0.01-1).
23. The method according to claim 18, wherein, The molar ratio of terephthalic acid, chlorosulfonate, and metal halide is 1:(0.8-1.2):(0.05-0.5).
24. The method according to claim 18, wherein, The metal halide is selected from at least one of RuCl3, FeCl3, AlCl3 and PdCl2.
25. The method according to claim 18, wherein, The metal halide is selected from at least one of RuCl3, FeCl3 and AlCl3.
26. The method according to claim 18, wherein, The second solvent is selected from at least one of dichloromethane, 1,2-dichloroethane, and chloroform.
27. The method according to claim 18, wherein, The second solvent is dichloromethane.
28. The method according to claim 18, wherein, The amount of the second solvent used is 20-100 mL relative to 1 g of terephthalic acid.
29. The method according to claim 18, wherein, The amount of the second solvent used is 30-80 mL relative to 1 g of terephthalic acid.
30. The method according to claim 1, wherein, In step (2), the acidification is carried out in the presence of an inorganic acid selected from at least one of hydrochloric acid, sulfuric acid, and nitric acid; And / or, the acidification conditions include: a temperature of -10°C to -100°C; The time is 5-30 hours.
31. The method according to claim 30, wherein, The amount of the inorganic acid used is 1-10 mol relative to each mole of the compound represented by formula (3).
32. The method according to claim 30, wherein, The inorganic acid is hydrochloric acid.
33. The method according to claim 1, wherein, The acidification conditions include a temperature of 0°C to 50°C.
34. The method according to claim 1, wherein, The acidification conditions include a time of 10-24 hours.
35. The method according to claim 30, wherein, The amount of the inorganic acid used is 1-5 mol relative to each mole of the compound represented by formula (3).
Citation Information
Patent Citations
Halophenyl pyridyl di-imine transition metal compound and its synthesis process and use
CN1139574C
Method for preparing olefin (CO)polymers
WO2001007491A1
Metal organic framework material with sulfonyl benzene ring structure, preparation method and application of metal organic framework material and carboxylic acid esterification method
CN115403493A