A porous multi-metallic heterogeneous alkaline hydrogen production electrode, a preparation method therefor and an application thereof
By preparing Ru@NiMoCu heterojunction catalysts on porous metal supports, the problem of high overpotential of NiMo-based catalysts under high current density was solved, achieving low-cost and high-efficiency alkaline hydrogen evolution performance, which is suitable for alkaline water electrolysis to produce hydrogen.
Patent Information
- Application Number
- CN202311324816.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-13
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-10-13
AI Technical Summary
Existing NiMo-based catalysts exhibit high overpotentials, especially at high current densities, during alkaline water electrolysis for hydrogen production, making it difficult to meet industrial demands. Furthermore, traditional precious metal catalysts are costly and difficult to apply in practice.
A porous multi-metal heterostructure alkaline hydrogen production electrode is used to form a Ru@NiMoCu heterojunction catalyst on a self-supporting porous metal support by continuous electrodeposition. Ru is used as the heterostructure substrate and NiMoCu is used as the surface active layer to synergistically improve the catalytic performance.
In a 30wt% alkaline solution, the overpotential is less than 0.17V at a current density of 1000mA·cm⁻², exhibiting excellent alkaline hydrogen evolution catalytic performance and stability at high current densities. The operation is simple, economical and feasible.
Smart Images

Figure CN117403265B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrochemical technology, and in particular relates to a porous multimetallic heterogeneous alkaline hydrogen production electrode, its preparation method and application. Background Technology
[0002] Hydrogen, as a clean fuel with "zero carbon emissions," is considered a key player in the future energy transition. Producing "green hydrogen" through water electrolysis using renewable energy sources such as wind and solar power is considered an important pathway for future hydrogen production. Alkaline water electrolysis is one hydrogen production technology, but compared to acidic environments, it requires additional energy to overcome the breaking of the HO-H bonds. In practice, this results in a slow electrode kinetic process, with drawbacks such as large overpotentials and slow hydrogen production efficiency. Although Pt-based noble metal catalysts can exhibit good alkaline hydrogen evolution reaction (HER) under alkaline conditions, their high price makes them impractical for industrial applications. Therefore, designing and preparing inexpensive alkaline cathode HER catalysts with superior catalytic performance is extremely important for alkaline water electrolysis hydrogen production technology.
[0003] NiMo alloys are considered a promising cathode catalyst for alkaline water electrolysis, exhibiting excellent electrocatalytic performance and resistance to alkaline corrosion. In recent years, although most NiMo-based catalysts can achieve 100 mA cm⁻¹... -2 The overpotential is 0.2V vs. RHE (vs. RHE: relative to the reversible hydrogen electrode), but it is difficult to handle future high currents (≥500mA cm⁻¹). -2 The requirements for alkaline hydrogen production. Patent CN 115029710 B discloses a nanoscale transition metal-based heterostructure Ni / NiMO as a water electrolysis catalyst; however, it only performs well at 10 mA cm⁻¹. -2 While the overpotential of the basic cathode electrode is relatively low at low current densities, it remains high at high current densities, indicating that its electrolytic catalytic performance still needs improvement. Therefore, there is an urgent need to develop novel, highly efficient NiMo-based catalysts to address the low activity of alkaline cathode electrode catalysts and meet the requirements for high-current alkaline hydrogen production. Summary of the Invention
[0004] The purpose of this invention is to overcome the defects of the existing technology and provide a porous multimetal heterogeneous alkaline hydrogen production electrode, its preparation method and application.
[0005] The objective of this invention can be achieved through the following technical solutions:
[0006] A porous multimetallic heterojunction alkaline hydrogen production electrode includes a catalyst support and a heterojunction catalyst deposited on the surface of the catalyst support.
[0007] Furthermore, the catalyst support includes a support body and porous metals (PMs) deposited on the support body.
[0008] Furthermore, the heterojunction catalyst comprises metallic Ru and NiMoCu. x The alloy has Ru as the heterogeneous underlying structure, and NiMoCu x It is the catalytically active surface.
[0009] Furthermore, the support includes one or more of the following: nickel mesh, nickel-chromium alloy mesh, nickel-iron alloy mesh, iron mesh, copper mesh, titanium mesh, nickel foam, iron foam, copper foam, carbon paper, carbon cloth, and porous carbon felt.
[0010] Furthermore, the support was immersed in a prepared 3M HCl solution for 30 minutes, and then rinsed three times with deionized water to remove oxides from the support surface. Subsequently, it was heated in a 0.1M NaCO3 solution for 20 minutes to remove surface organic matter, and then rinsed three times with deionized water.
[0011] Furthermore, the porous metal is one or more of Ni, Fe, or Cu.
[0012] Furthermore, the NiMoCu x The molar ratio of Ni to Mo in the alloy is (1-5):3, preferably 2:3.
[0013] Furthermore, the NiMoCu x In the alloy, x represents the proportion of Cu in the total molar number, and x is 0-20%, preferably 5-20%.
[0014] This invention also provides a method for preparing a porous multimetallic heterogeneous alkaline hydrogen production electrode, comprising the following steps:
[0015] S1: Electrodeposit porous metal PMs in the metal source solution to form a support / PMs electrode;
[0016] S2: Electrodeposit Ru into the support / PMs electrode in the Ru source solution to form a support / PMs / Ru electrode;
[0017] S3: Electrodeposition of NiMoCu in alloy solution on support / PMs / Ru electrode x Alloying was performed to obtain a porous multimetallic heterogeneous alkaline hydrogen production electrode support / PMs / Ru@NiMoCu x .
[0018] Further, in step S1, the metal source solution includes one or more of a nickel source, an iron source, or a copper source. Even further, the concentration of metal ions in the metal source solution is 0.1-0.5M, and 1M NH4Cl is added to the metal source solution as a conductive agent.
[0019] Furthermore, the nickel source includes one or more of nickel chloride, nickel acetate, nickel sulfate, nickel ammonium sulfate, nickel nitrate, or nickel acetylacetonate.
[0020] Furthermore, the iron source includes one or more of ferric chloride, ferrous chloride, ferric acetate, ferric sulfate, ferrous sulfate, ferric nitrate, or ferrous nitrate.
[0021] Furthermore, the copper source includes one or more of copper chloride, copper acetate, copper sulfate, or copper nitrate.
[0022] Further, in step S1, the current density of the electrodeposition is 0.1-2.0 A·cm. -2 Preferably, it is 0.5-2.0 A·cm. -2 More preferably 1.0 A·cm -2 .
[0023] Further, in step S1, the electrodeposition time is 10-150 min, preferably 10-50 min.
[0024] Furthermore, in step S1, the deposition temperature of the electrodeposition is 20-30℃, preferably 25℃.
[0025] Further, in step S2, the Ru source includes one or more of ruthenium chloride, ruthenium acetate, ammonium ruthenium chloride, potassium perruthenium chloride, hexaammineruthenium chloride, tris(2,2′-bipyridine)ruthenium(II) chloride, ruthenium sulfate, or ruthenium nitrate.
[0026] Furthermore, the Ru source solution contains Ru 3+ The concentration of Ru was 0.01-0.1 M, and 0.5 M NaCl was also added to the Ru source solution.
[0027] Further, in step S2, the current density of the electrodeposition is 5-15 mA·cm⁻¹. -2 Preferably 10 mA·cm -2 .
[0028] Furthermore, the electrodeposition time is 2-6 minutes, preferably 3 minutes.
[0029] Furthermore, the electrodeposition temperature is 20-30°C, preferably 25°C.
[0030] Further, in step S3, the nickel source of the alloy solution includes one or more of nickel chloride, nickel acetate, nickel sulfate, nickel ammonium sulfate, nickel nitrate, or nickel acetylacetonate.
[0031] Further, in step S3, the molybdenum source of the alloy solution includes one or more of sodium molybdate, ammonium molybdate, molybdenum chloride, molybdenum nitrate, and molybdenum sulfate.
[0032] Further, in step S3, the copper source of the alloy solution includes one or more of copper chloride, copper acetate, copper sulfate, copper nitrate, or copper acetylacetonate.
[0033] Further, in step S3, the current density of the electrodeposition is 10-40 mA·cm⁻¹. -2 Preferably 15-30 mA·cm -2 More preferably 30 mA·cm -2 .
[0034] Furthermore, the electrodeposition time is 10-30 minutes, preferably 20-30 minutes.
[0035] Furthermore, the electrodeposition temperature is 20-80°C, preferably 30-60°C, and more preferably 60°C.
[0036] This invention also provides the application of a porous multimetal heterogeneous alkaline hydrogen production electrode in alkaline water electrolysis for hydrogen production.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] (1) This invention prepares Ru@NiMoCu supported by continuous multi-step electrodeposition. x A self-supported porous multi-metal heterogeneous alkaline hydrogen production electrode with a heterojunction catalyst. This invention uses self-made porous metal PMs as a support for the heterogeneous catalyst. Compared with traditional commercial metal foams, PMs have higher hydrophilicity, richer porosity, and larger surface area, which can provide a larger adhesion area for the catalyst, facilitate rapid desorption of bubbles, and improve the alkaline hydrogen evolution catalytic performance of this invention.
[0039] (2) This invention prepares Ru@NiMoCu by continuous electrodeposition. x A self-supporting porous multi-metal heterogeneous alkaline hydrogen production electrode, using a heterojunction catalyst and a porous metal support, fully considers the HER catalytic mechanism of the alkaline cathode. To enable rapid first-step splitting of H2O, Ru, a metal with a strong adsorption effect on water molecules, is introduced as the heterostructure substrate, and an alloy NiMoCu is used. xAs a surface active layer, the interfacial synergistic effect between surface Cu atoms and substrate Ru atoms promotes the splitting of H₂O (oxygen-containing intermediate), thereby making it easier for the transition state H to be adsorbed and reduced at active sites around Mo and Ni atoms. The synergistic effect of the heterostructure endows the prepared self-supporting electrode with excellent alkaline HER catalytic performance. This is thanks to the substrate Ru and the surface catalytic active layer NiMoCu. x The synergistic effect of the alkaline hydrogen production electrode of the present invention, in a 30wt% alkaline solution at 1000mA·cm -2 It exhibits a low overpotential (<0.17V) at a given current density, demonstrating excellent alkaline hydrogen evolution catalytic performance, and its performance at 1000 mA·cm⁻¹ for 24 hours is also remarkable. -2 It exhibits excellent stability in current density tests.
[0040] (3) The present invention constructs a Ru-containing heterogeneous catalyst layer by simple electrodeposition under mild conditions, with low Ru loading, and high economic feasibility; the operation is simple and time-saving, and has the potential for industrial application. Attached Figure Description
[0041] Figure 1 This is a scanning electron microscope image of NM as shown in Comparative Example 1.
[0042] Figure 2 NM / PN / Ru@NiMoCu as described in Example 4 x Electron scanning microscope image of the electrode.
[0043] Figure 3 NM / PN / Ru@NiMoCu as described in Example 4 x A schematic diagram of the structure and the linear current-voltage curve of NM compared with Comparative Example 1.
[0044] Figure 4 NM / PN / Ru@NiMoCu from Examples 1-4 x Linear voltammetric curves of the commercial Pt / C catalyst in Comparative Example 2.
[0045] Figure 5 NM / PN / Ru@NiMoCu from Examples 1-4 x Comparative Example 2: Commercial Pt / C catalyst at 1000 mA·cm -2 Potential of current density.
[0046] Figure 6 NM / PN / Ru@NiMoCu as described in Example 4 x Electrode and Comparative Example 3 NM / PN / NiMoCu x Linear voltammetry curves of the electrodes.
[0047] Figure 7NM / PN / Ru@NiMoCu as described in Examples 4-7 x The linear voltammetry curve spectrum.
[0048] Figure 8 NM / PN / Ru@NiMoCu prepared at different electrodeposition temperatures in Examples 4-7 x At 1000mA·cm -2 Potential of current density.
[0049] Figure 9 NM / PN / Ru@NiMoCu as described in Example 4 x Voltage fluctuation test diagram of the electrode under 24-hour constant current density mode. Detailed Implementation
[0050] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.
[0051] Unless otherwise specified, the reagents, methods, instruments, and equipment used in this invention are conventional in the art. Unless otherwise specified, the reagents and materials used in the following examples are all commercially available and of analytical grade.
[0052] Example 1:
[0053] This embodiment provides a porous multimetallic heterogeneous alkaline hydrogen production electrode and its preparation method. The support is a commercially available nickel mesh (NM).
[0054] S1: Support Pretreatment
[0055] NM was immersed in a prepared 3M HCl solution for 30 minutes, and then rinsed three times with deionized water to remove oxides from the support surface. Subsequently, it was heated in 0.1M NaCO3 solution for 20 minutes to remove surface organic matter, followed by three deionized water rinses, and then sealed in a closed container with deionized water.
[0056] S2: Preparation of catalyst support
[0057] Porous metallic nickel PN was prepared by electrodeposition in a nickel source solution (1M ammonium chloride and 0.1M nickel chloride) using clean NM as the cathode and a high-purity nickel rod (purity ≥99.5 At%) as the anode. The electrodeposition current was 1 A·cm. -2 A porous catalyst support NM / PN was prepared by deposition at a temperature of 25℃ and a deposition time of 10 min.
[0058] S3: Fabrication of NM / PN / Ru electrodes
[0059] Using an NM / PN electrode as the cathode and a carbon rod as the anode, Ru metal was deposited in a Ru source solution (0.01 M ruthenium chloride, 0.5 M sodium chloride) at an electrodeposition current of 10 mA·cm⁻¹. -2 The NM / PN / Ru electrode was prepared by deposition at a temperature of 25℃ and a deposition time of 3 minutes.
[0060] S4: Fabrication of NM / PN / Ru@NiMo electrode:
[0061] The NM / PN / Ru electrode is the cathode, and the carbon rod is the anode, in a Ni-containing environment. 2+ MoO4 2- NiMo was deposited in a mixed solution (containing 0.15 M sodium molybdate and 0.1 M nickel chloride, with a Ni:Mo molar ratio of 2:3) at a deposition current density of 30 mA·cm⁻¹. -2 The NM / PN / Ru@NiMo electrode was prepared by electrodeposition at a time of 30 min and a temperature of 60 °C.
[0062] Example 2:
[0063] This embodiment provides a porous multimetallic heterogeneous alkaline hydrogen production electrode and its preparation method. The support is a commercially available nickel mesh (NM).
[0064] S1: Support Pretreatment
[0065] NM was immersed in a prepared 3M HCl solution for 30 minutes, and then rinsed three times with deionized water to remove oxides from the support surface. Subsequently, it was heated in 0.1M NaCO3 solution for 20 minutes to remove surface organic matter, followed by three deionized water rinses, and then sealed in a closed container with deionized water.
[0066] S2: Preparation of catalyst support
[0067] Porous metallic nickel PN was prepared by electrodeposition in a nickel source solution (1M ammonium chloride and 0.1M nickel chloride) using clean NM as the cathode and a high-purity nickel rod (purity ≥99.5 At%) as the anode. The electrodeposition current was 1 A·cm. -2 A porous catalyst support NM / PN was prepared by deposition at a temperature of 25℃ and a deposition time of 10 min.
[0068] S3: Fabrication of NM / PN / Ru electrodes
[0069] Using an NM / PN electrode as the cathode and a carbon rod as the anode, Ru metal was deposited in a Ru source solution (0.01 M ruthenium chloride, 0.5 M sodium chloride) at an electrodeposition current of 10 mA·cm⁻¹. -2 The NM / PN / Ru electrode was prepared by deposition at a temperature of 25℃ and a deposition time of 3 minutes.
[0070] S4: Preparation of NM / PN / Ru@NiMoCu x electrode:
[0071] The NM / PN / Ru electrode is the cathode, and the carbon rod is the anode, in a Ni-containing environment. 2+ MoO4 2- Cu 2+ NiMoCu was deposited in a mixed solution (containing 0.1M nickel chloride, 0.15M sodium molybdate, and 0.013M copper sulfate, with a Ni:Mo:Cu molar ratio of 100:150:13). x Deposition current density 30 mA·cm -2 NM / PN / Ru@NiMoCu was prepared by electrodeposition at a time of 30 min and a temperature of 60 °C. x electrode.
[0072] Example 3:
[0073] This embodiment provides a porous multimetallic heterogeneous alkaline hydrogen production electrode and its preparation method. The support is a commercially available nickel mesh (NM).
[0074] S1: Support Pretreatment
[0075] NM was immersed in a prepared 3M HCl solution for 30 minutes, and then rinsed three times with deionized water to remove oxides from the support surface. Subsequently, it was heated in 0.1M NaCO3 solution for 20 minutes to remove surface organic matter, followed by three deionized water rinses, and then sealed in a closed container with deionized water.
[0076] S2: Preparation of catalyst support
[0077] Porous metallic nickel PN was prepared by electrodeposition in a nickel source solution (1M ammonium chloride and 0.1M nickel chloride) using clean NM as the cathode and a high-purity nickel rod (purity ≥99.5 At%) as the anode. The electrodeposition current was 1 A·cm. -2 A porous catalyst support NM / PN was prepared by deposition at a temperature of 25℃ and a deposition time of 10 min.
[0078] S3: Fabrication of NM / PN / Ru electrodes
[0079] Using an NM / PN electrode as the cathode and a carbon rod as the anode, Ru metal was deposited in a Ru source solution (0.01 M ruthenium chloride, 0.5 M sodium chloride) at an electrodeposition current of 10 mA·cm⁻¹. -2 The NM / PN / Ru electrode was prepared by deposition at a temperature of 25℃ and a deposition time of 3 minutes.
[0080] S4: Preparation of NM / PN / Ru@NiMoCu x electrode:
[0081] The NM / PN / Ru electrode is the cathode, and the carbon rod is the anode, in a Ni-containing environment. 2+ MoO4 2- Cu 2+ NiMoCu was deposited in a mixed solution (containing 0.1M nickel chloride, 0.15M sodium molybdate, and 0.028M copper sulfate, with a Ni:Mo:Cu molar ratio of 100:150:28). x Deposition current density 30 mA·cm -2 NM / PN / Ru@NiMoCu was prepared by electrodeposition at a time of 30 min and a temperature of 60 °C. x electrode.
[0082] Example 4:
[0083] This embodiment provides a porous multimetallic heterogeneous alkaline hydrogen production electrode and its preparation method. The support is a commercially available nickel mesh (NM).
[0084] S1: Support Pretreatment
[0085] NM was immersed in a prepared 3M HCl solution for 30 minutes, and then rinsed three times with deionized water to remove oxides from the support surface. Subsequently, it was heated in 0.1M NaCO3 solution for 20 minutes to remove surface organic matter, followed by three deionized water rinses, and then sealed in a closed container with deionized water.
[0086] S2: Preparation of catalyst support
[0087] Porous metallic nickel PN was prepared by electrodeposition in a nickel source solution (1M ammonium chloride and 0.1M nickel chloride) using clean NM as the cathode and a high-purity nickel rod (purity ≥99.5 At%) as the anode. The electrodeposition current was 1 A·cm. -2 A porous catalyst support NM / PN was prepared by deposition at a temperature of 25℃ and a deposition time of 10 min.
[0088] S3: Fabrication of NM / PN / Ru electrodes
[0089] Using an NM / PN electrode as the cathode and a carbon rod as the anode, Ru metal was deposited in a Ru source solution (0.01 M ruthenium chloride, 0.5 M sodium chloride) at an electrodeposition current of 10 mA·cm⁻¹. -2 The NM / PN / Ru electrode was prepared by deposition at a temperature of 25℃ and a deposition time of 3 minutes.
[0090] S4: Preparation of NM / PN / Ru@NiMoCu x electrode:
[0091] The NM / PN / Ru electrode is the cathode, and the carbon rod is the anode, in a Ni-containing environment. 2+ MoO4 2- Cu2+ NiMoCu was deposited in a mixed solution (containing 0.1M nickel chloride, 0.15M sodium molybdate, and 0.063M copper sulfate, with a Ni:Mo:Cu molar ratio of 100:150:63). x Deposition current density 30 mA·cm -2 NM / PN / Ru@NiMoCu was prepared by electrodeposition at a time of 30 min and a temperature of 60 °C. x electrode.
[0092] Example 5:
[0093] This embodiment provides a porous multimetallic heterogeneous alkaline hydrogen production electrode and its preparation method. The support is a commercially available nickel mesh (NM).
[0094] S1: Support Pretreatment
[0095] NM was immersed in a prepared 3M HCl solution for 30 minutes, and then rinsed three times with deionized water to remove oxides from the support surface. Subsequently, it was heated in 0.1M NaCO3 solution for 20 minutes to remove surface organic matter, followed by three deionized water rinses, and then sealed in a closed container with deionized water.
[0096] S2: Preparation of catalyst support
[0097] Porous metallic nickel PN was prepared by electrodeposition in a nickel source solution (1M ammonium chloride and 0.1M nickel chloride) using clean NM as the cathode and a high-purity nickel rod (purity ≥99.5 At%) as the anode. The electrodeposition current was 1 A·cm. -2 A porous catalyst support NM / PN was prepared by deposition at a temperature of 25℃ and a deposition time of 10 min.
[0098] S3: Fabrication of NM / PN / Ru electrodes
[0099] Using an NM / PN electrode as the cathode and a carbon rod as the anode, Ru metal was deposited in a Ru source solution (0.01 M ruthenium chloride, 0.5 M sodium chloride) at an electrodeposition current of 10 mA·cm⁻¹. -2 The NM / PN / Ru electrode was prepared by deposition at a temperature of 25℃ and a deposition time of 3 minutes.
[0100] S4: Preparation of NM / PN / Ru@NiMoCu x electrode:
[0101] The NM / PN / Ru electrode is the cathode, and the carbon rod is the anode, in a Ni-containing environment. 2+ MoO4 2- Cu 2+NiMoCu was deposited in a mixed solution (containing 0.1M nickel chloride, 0.15M sodium molybdate, and 0.063M copper sulfate, with a Ni:Mo:Cu molar ratio of 100:150:63). x Deposition current density 30 mA·cm -2 NM / PN / Ru@NiMoCu was prepared by electrodeposition at a time of 30 min and a temperature of 20 °C. x electrode.
[0102] Example 6:
[0103] This embodiment provides a porous multimetallic heterogeneous alkaline hydrogen production electrode and its preparation method. The support is a commercially available nickel mesh (NM).
[0104] S1: Support Pretreatment
[0105] NM was immersed in a prepared 3M HCl solution for 30 minutes, and then rinsed three times with deionized water to remove oxides from the support surface. Subsequently, it was heated in 0.1M NaCO3 solution for 20 minutes to remove surface organic matter, followed by three deionized water rinses, and then sealed in a closed container with deionized water.
[0106] S2: Preparation of catalyst support
[0107] Porous metallic nickel PN was prepared by electrodeposition in a nickel source solution (1M ammonium chloride and 0.1M nickel chloride) using clean NM as the cathode and a high-purity nickel rod (purity ≥99.5 At%) as the anode. The electrodeposition current was 1 A·cm. -2 A porous catalyst support NM / PN was prepared by deposition at a temperature of 25℃ and a deposition time of 10 min.
[0108] S3: Fabrication of NM / PN / Ru electrodes
[0109] Using an NM / PN electrode as the cathode and a carbon rod as the anode, Ru metal was deposited in a Ru source solution (0.01 M ruthenium chloride, 0.5 M sodium chloride) at an electrodeposition current of 10 mA·cm⁻¹. -2 The NM / PN / Ru electrode was prepared by deposition at a temperature of 25℃ and a deposition time of 3 minutes.
[0110] S4: Preparation of NM / PN / Ru@NiMoCu x electrode:
[0111] The NM / PN / Ru electrode is the cathode, and the carbon rod is the anode, in a Ni-containing environment. 2+ MoO4 2- Cu 2+NiMoCu was deposited in a mixed solution (containing 0.1M nickel chloride, 0.15M sodium molybdate, and 0.063M copper sulfate, with a Ni:Mo:Cu molar ratio of 100:150:63). x Deposition current density 30 mA·cm -2 NM / PN / Ru@NiMoCu was prepared by electrodeposition at a time of 30 min and a temperature of 40 °C. x electrode.
[0112] Example 7:
[0113] This embodiment provides a porous multimetallic heterogeneous alkaline hydrogen production electrode and its preparation method. The support is a commercially available nickel mesh (NM).
[0114] S1: Support Pretreatment
[0115] NM was immersed in a prepared 3M HCl solution for 30 minutes, and then rinsed three times with deionized water to remove oxides from the support surface. Subsequently, it was heated in 0.1M NaCO3 solution for 20 minutes to remove surface organic matter, followed by three deionized water rinses, and then sealed in a closed container with deionized water.
[0116] S2: Preparation of catalyst support
[0117] Porous metallic nickel PN was prepared by electrodeposition in a nickel source solution (1M ammonium chloride and 0.1M nickel chloride) using clean NM as the cathode and a high-purity nickel rod (purity ≥99.5 At%) as the anode. The electrodeposition current was 1 A·cm. -2 A porous catalyst support NM / PN was prepared by deposition at a temperature of 25℃ and a deposition time of 10 min.
[0118] S3: Fabrication of NM / PN / Ru electrodes
[0119] Using an NM / PN electrode as the cathode and a carbon rod as the anode, Ru metal was deposited in a Ru source solution (0.01 M ruthenium chloride, 0.5 M sodium chloride) at an electrodeposition current of 10 mA·cm⁻¹. -2 The NM / PN / Ru electrode was prepared by deposition at a temperature of 25℃ and a deposition time of 3 minutes.
[0120] S4: Preparation of NM / PN / Ru@NiMoCu x electrode:
[0121] The NM / PN / Ru electrode is the cathode, and the carbon rod is the anode, in a Ni-containing environment. 2+ MoO4 2- Cu 2+NiMoCu was deposited in a mixed solution (containing 0.1M nickel chloride, 0.15M sodium molybdate, and 0.063M copper sulfate, with a Ni:Mo:Cu molar ratio of 100:150:63). x Deposition current density 30 mA·cm -2 NM / PN / Ru@NiMoCu was prepared by electrodeposition at a time of 30 min and a temperature of 80 °C. x electrode.
[0122] The present invention also provides the following comparative examples to demonstrate the beneficial effects of the invention.
[0123] Comparative Example 1:
[0124] This comparative example uses pure nickel mesh (NM) without the addition of porous metals and heterogeneous catalysts. The NM was immersed in a prepared 3M HCl solution for 30 minutes, followed by three deionization rinses to remove surface oxides. It was then heated in a 0.1M NaCO3 solution for 20 minutes to remove surface organic matter, followed by three deionization rinses, and then used for subsequent performance testing.
[0125] Comparative Example 2:
[0126] This comparative example uses commercially available Pt / C as a catalyst. The preparation method for this comparative example is as follows:
[0127] S1: 5 mg of Pt / C catalyst (20 wt%) was dispersed in 10 ml of ethanol, and 200 μL of Nafion solution was added. The mixture was then sonicated in an ice-water bath for 30 minutes.
[0128] S2: Use a high-pressure spray gun to take 1 ml of the ultrasonicated solution from step S1 and spray it onto a 1×2 cm commercial nickel foam.
[0129] S3: After each spraying and drying, weigh the Pt / C catalyst to ensure the loading is 2 mg / cm³. -2 .
[0130] Comparative Example 3:
[0131] This comparative example provides an NM / PN / NiMoCu without the addition of metallic Ru. 20 The electrode is prepared using the following steps:
[0132] S1: Support Pretreatment
[0133] NM was immersed in a prepared 3M HCl solution for 30 minutes, and then rinsed three times with deionized water to remove oxides from the support surface. Subsequently, it was heated in 0.1M NaCO3 solution for 20 minutes to remove surface organic matter, followed by three deionized water rinses, and then sealed in a closed container with deionized water.
[0134] S2: Preparation of catalyst support
[0135] Porous metallic nickel PN was prepared by electrodeposition in a nickel source solution (1M ammonium chloride and 0.1M nickel chloride) using clean NM as the cathode and a high-purity nickel rod (purity ≥99.5 At%) as the anode. The electrodeposition current was 1 A·cm. -2 A porous catalyst support NM / PN was prepared by deposition at a temperature of 25℃ and a deposition time of 10 min.
[0136] S3: Preparation of NM / PN / NiMoCu x electrode:
[0137] The NM / PN electrode is the cathode, and the carbon rod is the anode, in a Ni-containing environment. 2+ MoO4 2- Cu 2+ NiMoCu was deposited in a mixed solution (containing 0.1M nickel chloride, 0.15M sodium molybdate, and 0.063M copper sulfate, with a Ni:Mo:Cu molar ratio of 100:150:63). x Deposition current density 30 mA·cm -2 NM / PN / NiMoCu was prepared by electrodeposition at a time of 30 min and a temperature of 60 °C. x electrode.
[0138] The present invention conducted the following tests on Examples 1-7 and Comparative Examples 1-3 to demonstrate the beneficial effects of the present invention:
[0139] (1) Scanning electron microscopy: The appearance morphology of Example 4 and Comparative Example 1 was characterized using a FEI SIRION 200 / INCA scanning electron microscope.
[0140] (2) Linear voltammetry curves: The linear voltammetry curves were obtained using a three-electrode testing system equipped with a high-sensitivity electrochemical workstation, Reference 3000. The electrolyte was 30 wt% KOH solution, the scan rate was 5 mV / s, and the reference electrode was HgO / Hg.
[0141] (3) Potential test: Select a current density of 1000 mA·cm from the linear voltammetry curve. -2 The potential value at that time.
[0142] (4) Voltage fluctuation test: The test was performed in the Reference 3000 electrochemical workpiece, with the transverse current density set to 1000 mA·cm. -2 The test will last for 24 hours.
[0143] Figure 1 and Figure 2 Nickel mesh and porous NM / PN / Ru@NiMoCu were shown respectively.20 Electrode. Compared to pure nickel mesh, the NM / PN / Ru@NiMoCu electrode in Example 4... x The electrode exhibits a distinct porous structure.
[0144] Figure 3 This indicates that the load is a porous Ru-supported NiMoCu x Compared with the currently commercial NM electrode, the electrode has a smaller overpotential and its catalytic performance is far superior to that of the commercial NM electrode.
[0145] Figure 4 Ru@NiMoCu prepared with Cu sources in different proportions was demonstrated. x Linear voltammetric curves of the catalyst and currently commercial Pt / C catalysts are presented. The data indicate that at high current densities, the porous multimetallic heterogeneous catalyst electrode outperforms the currently commercial Pt / C catalyst electrode.
[0146] Figure 5 Various electrodes were demonstrated at 1000 mA·cm -2 The overpotential value at current density indicates that the catalytic performance gradually improves with increasing Cu content.
[0147] Figure 6 The voltammetric curves before and after the addition of metallic Ru show that the introduction of metallic Ru significantly reduced the overpotential value and significantly improved the catalytic performance.
[0148] Figure 7 Electrodeposition of NiMoCu at different temperatures was demonstrated. x The linear voltammetric curves of the catalyst electrode indicate that the catalyst with the best performance is electrodeposited at 60 °C.
[0149] Figure 8 Electrodeposition of NiMoCu at different temperatures was demonstrated. x Catalyst electrode at 1000 mA·cm -2 The overpotential value at current density indicates the effect of deposition temperature on catalytic performance and proves that the catalyst deposited at 60℃ has the best performance.
[0150] Figure 9 NM / PN / Ru@NiMoCu was demonstrated x The electrode's constant current stability in 30wt% KOH solution for 24 hours indicates that the electrode possesses high catalytic stability at high current density.
[0151] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.
Claims
1. A porous multi-metal heterogeneous alkaline hydrogen production electrode, characterized in that, This includes catalyst supports and heterojunction catalysts deposited on the surface of the catalyst supports; The catalyst support includes a support body and porous metal PMs deposited on the support body; The heterojunction catalyst comprises metallic Ru and NiMoCu. x The alloy has Ru as the heterogeneous underlying structure, and NiMoCu x It is a catalytically active surface; The metal in the porous metal is one or more of nickel, iron, or copper; The NiMoCu x The molar ratio of Ni to Mo in the alloy is (1-5):3, and the proportion of Cu in the total molar number is 0-20%. The method for preparing the porous multimetal heterogeneous alkaline hydrogen production electrode includes the following steps: S1: Electrodeposit porous metal PMs in the metal source solution to form a support / PMs electrode; S2: Electrodeposit Ru into the support / PMs electrode in the Ru source solution to form a support / PMs / Ru electrode; S3: Electrodeposition of NiMoCu in alloy solution on support / PMs / Ru electrode x Alloying was performed to obtain a porous multimetallic heterogeneous alkaline hydrogen production electrode support / PMs / Ru@NiMoCu x .
2. The porous multi-metal heterogeneous alkaline hydrogen production electrode according to claim 1, characterized in that, The support includes one or more of the following: nickel mesh, nickel-chromium alloy mesh, nickel-iron alloy mesh, iron mesh, copper mesh, titanium mesh, nickel foam, iron foam, copper foam, carbon paper, carbon cloth, and porous carbon felt.
3. A method for preparing a porous multimetallic heterogeneous alkaline hydrogen production electrode as described in claim 1, characterized in that, Includes the following steps: S1: Electrodeposit porous metal PMs in the metal source solution to form a support / PMs electrode; S2: Electrodeposit Ru into the support / PMs electrode in the Ru source solution to form a support / PMs / Ru electrode; S3: Electrodeposition of NiMoCu in alloy solution on support / PMs / Ru electrode x Alloying was performed to obtain a porous multimetallic heterogeneous alkaline hydrogen production electrode support / PMs / Ru@NiMoCu x .
4. The method for preparing the porous multimetallic heterogeneous alkaline hydrogen production electrode according to claim 3, characterized in that, In step S1, the metal source solution is one or more of nickel source, iron source, or copper source; The nickel source includes one or more of nickel chloride, nickel acetate, nickel sulfate, nickel ammonium sulfate, nickel nitrate, or nickel acetylacetonate; the iron source includes one or more of ferric chloride, ferrous chloride, ferric acetate, ferric sulfate, ferrous sulfate, ferric nitrate, or ferrous nitrate; and the copper source includes one or more of copper chloride, copper acetate, copper sulfate, or copper nitrate.
5. The method for preparing the porous multimetallic heterogeneous alkaline hydrogen production electrode according to claim 3, characterized in that, In step S1, the current density of the electrodeposition is 0.1-2.0 A·cm. -2 The electrodeposition time is 10-150 min and the electrodeposition temperature is 20-30℃.
6. The method for preparing the porous multimetallic heterogeneous alkaline hydrogen production electrode according to claim 3, characterized in that, In step S2, the Ru source includes one or more of ruthenium chloride, ruthenium acetate, ammonium ruthenium chloride, potassium perruthenium chloride, hexaammineruthenium chloride, tris(2,2′-bipyridine)ruthenium(II) chloride, ruthenium sulfate, or ruthenium nitrate. The current density for electrodeposition is 5-15 mA·cm. -2 The electrodeposition time is 2-6 minutes and the electrodeposition temperature is 20-30℃.
7. The method for preparing the porous multimetallic heterogeneous alkaline hydrogen production electrode according to claim 3, characterized in that, In step S3, the nickel source of the alloy solution includes one or more of nickel chloride, nickel acetate, nickel sulfate, nickel ammonium sulfate, nickel nitrate, or nickel acetylacetonate; the molybdenum source includes one or more of sodium molybdate, ammonium molybdate, molybdenum chloride, molybdenum nitrate, and molybdenum sulfate; and the copper source includes one or more of copper chloride, copper acetate, copper sulfate, copper nitrate, or copper acetylacetonate. The current density of the electrodeposition is 10-40 mA·cm. -2 The electrodeposition time is 10-30 min and the electrodeposition temperature is 20-80℃.
8. The application of the porous multimetallic heterogeneous alkaline hydrogen production electrode as described in claim 1 in alkaline water electrolysis cathode hydrogen production.
Citation Information
Patent Citations
A transition metal-based heterostructure water electrolysis catalyst, its preparation method and application
CN115029710B
Hydrogen evolution catalytic electrode as well as preparation method and application thereof
CN112695339A
Three-dimensional porous Ni-Mo-Cu catalyst and preparation method and application thereof