Perovskite precursor solution, preparation method of perovskite layer, and perovskite tandem solar cell and preparation method thereof
By using perovskite precursor solutions with specific viscosity and boiling points and airflow-assisted coating technology, the problems of uneven coating and conformal coverage of perovskite layers on large-area pyramid-patterned substrates have been solved, achieving efficient and simplified perovskite layer preparation and improving the performance and production efficiency of perovskite tandem solar cells.
Patent Information
- Application Number
- CN202311250096.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Existing technologies struggle to achieve uniform coating and shape-preserving coverage of perovskite layers on large-area pyramid-patterned substrates, and traditional methods are cumbersome, impacting production efficiency.
By using a perovskite precursor solution with specific viscosity and boiling point, combined with airflow-assisted coating technology, a perovskite layer is formed on a pyramid-patterned substrate. By controlling the volatility and viscosity of the solvent, uniform coating and rapid crystal growth are achieved, avoiding annealing treatment.
Uniform and stable coating and rapid crystallization were achieved on a pyramid-patterned substrate to form an excellent perovskite layer, improving production efficiency and battery performance without the need for additional annealing processes.
Smart Images

Figure CN117412650B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solar cells, and more particularly to a perovskite precursor solution, a method for preparing a perovskite layer, and a perovskite tandem solar cell and the method thereof. Background Technology
[0002] Solution-based perovskite layer fabrication offers advantages in terms of simplicity and speed, which is highly beneficial for improving the production efficiency of perovskite-silicon tandem solar cells. However, solution-based perovskite layer fabrication is generally used in planar perovskite solar cells. In perovskite tandem solar cells with pyramidal textured surfaces, especially on large-area pyramidal textured surfaces, achieving good conformal deposition is difficult. Currently, perovskite layers on perovskite tandem solar cells with pyramidal textured surfaces are typically prepared using a combination of solution-based and vapor deposition methods. This method is relatively cumbersome and detrimental to improving production efficiency. Summary of the Invention
[0003] This invention discloses a method for preparing a perovskite precursor solution, a perovskite layer, and a perovskite tandem solar cell. The perovskite precursor solution is coated onto a pyramidal textured substrate, enabling the preparation of a perovskite layer with both excellent shape retention and crystallization on the pyramidal textured substrate. This solves the problem of achieving shape retention and coverage when preparing a perovskite layer on a pyramidal textured substrate using a solution method.
[0004] To achieve the above objectives, in a first aspect, the present invention discloses a perovskite precursor solution comprising: a perovskite material and a mixed solvent, wherein the viscosity of the mixed solvent is 2 mPa·s to 3.5 mPa·s, the mixed solvent comprises a first solvent, the volume of the first solvent being 10% to 40% of the mixed solvent, and the boiling point of the first solvent being 80°C to 130°C.
[0005] As an optional implementation, in an embodiment of the present invention, the mixed solvent further includes a second solvent, which includes one or both of dimethyl sulfoxide and 1,8-diiodooctane.
[0006] As an optional implementation, in an embodiment of the present invention, the second solvent is composed of the dimethyl sulfoxide and the 1,8-diiodooctane in a mass ratio of 0.4 to 0.8:1.
[0007] As an optional implementation, in the embodiments of the present invention, the first solvent includes one or more of acetonitrile, ethanol, 2-methoxyethanol and isopropanol.
[0008] As an optional implementation, in an embodiment of the present invention, the first solvent is composed of acetonitrile and 2-methoxyethanol in a volume ratio of (0.25 to 0.82):1.
[0009] As an optional implementation, in the embodiments of the present invention, the concentration of the perovskite precursor solution is 0.8 mol / mL to 2 mol / mL.
[0010] Secondly, this application provides a method for preparing a perovskite layer, the method comprising the following steps:
[0011] Provides a base with a pyramidal suede finish;
[0012] The perovskite precursor solution is coated on the substrate to form a perovskite wet film layer, and an airflow with a temperature of 80°C to 130°C and a pressure of 1 MPa to 2 MPa is blown toward the perovskite wet film layer. The temperature of the airflow is not lower than the boiling point of the first solvent, thereby obtaining the perovskite layer.
[0013] As an optional implementation, in an embodiment of the present invention, the thickness of the perovskite layer is 800 nm to 1500 nm.
[0014] As an optional implementation, in embodiments of the present invention, the coating method of the perovskite precursor solution includes any one of slot coating, screen printing, and blade coating; and / or,
[0015] The perovskite precursor solution is coated at a rate of 5 mm / s to 20 mm / s; and / or,
[0016] After the perovskite precursor solution is coated, the thickness of the resulting wet perovskite film is 5 μm to 10 μm; and / or,
[0017] The gas flow is nitrogen or an inert gas.
[0018] As an optional implementation, in the embodiments of the present invention, when using the slit coating method, the slit size is controlled to be 70μm to 110μm.
[0019] Thirdly, this application provides a perovskite tandem solar cell, which includes:
[0020] The perovskite tandem solar cell includes a silicon substrate cell and a first transparent conductive layer, a hole transport layer, a perovskite layer, an electron transport layer, and a second transparent conductive layer sequentially stacked on the silicon substrate cell. The perovskite layer is prepared by the perovskite layer preparation method described in the second aspect. The perovskite tandem solar cell also includes a positive electrode and a negative electrode. The positive electrode forms an ohmic contact with the electron transport layer, and the negative electrode forms an ohmic contact with the silicon substrate cell.
[0021] As an optional implementation, in the embodiments of the present invention, a hole modification layer is further disposed between the perovskite layer and the hole transport layer; and / or, a passivation layer is further disposed between the perovskite layer and the electron transport layer; and / or, a buffer layer is further disposed on the side of the electron transport layer away from the silicon substrate cell, and an antireflection layer is further disposed on the side of the second transparent conductive layer away from the silicon substrate cell.
[0022] As an optional implementation, in embodiments of the present invention, the thickness of the hole transport layer is 15 nm to 25 nm; and / or, the thickness of the electron transport layer is 10 nm to 20 nm; and / or, the thickness of the hole modification layer is 1 nm to 5 nm; and / or, the thickness of the passivation layer is 1 nm to 3 nm; and / or, the thickness of the buffer layer is 10 nm to 20 nm, and the thickness of the antireflection layer is 90 nm to 120 nm. 。
[0023] Fourthly, this application provides a method for fabricating a perovskite tandem solar cell, which includes the following steps:
[0024] Provide silicon-based solar cells;
[0025] A first transparent conductive layer is formed on the front side of the silicon substrate cell;
[0026] A hole transport layer is fabricated on the first transparent conductive layer;
[0027] A perovskite layer is prepared on the hole transport layer, wherein the perovskite layer is prepared by the perovskite layer preparation method described in the second aspect;
[0028] An electron transport layer is fabricated on the perovskite layer;
[0029] A second transparent conductive layer is fabricated on the electron transport layer;
[0030] A positive electrode is fabricated on the second transparent conductive layer, and a negative electrode is fabricated on the back of the silicon substrate cell to obtain the above-mentioned perovskite tandem solar cell.
[0031] As an optional implementation, in an embodiment of the present invention, a hole modification layer is further prepared between the hole transport layer and the perovskite layer, a passivation layer is further prepared between the perovskite layer and the electron transport layer, and a buffer layer is further prepared on the side of the electron transport layer away from the silicon substrate cell.
[0032] As an optional implementation, in an embodiment of the present invention, the hole transport layer, the hole modification layer, the passivation layer, the electron transport layer and / or the buffer layer are fabricated by slot coating.
[0033] As an optional implementation, in an embodiment of the present invention, the hole transport layer is prepared as follows: an aqueous solution of nickel oxide nanocrystals is dissolved in a volatile solvent to obtain a nickel oxide nanocrystal solution; then, the nickel oxide nanocrystal solution is coated to form a wet film of the hole transport layer; subsequently, an airflow at a temperature of 60°C and a wind pressure of 1 MPa is blown toward the surface of the wet film of the hole transport layer to obtain the hole transport layer. The volatile solvent is one or more of ethanol, acetonitrile, and isopropanol; and / or,
[0034] As an optional implementation, in an embodiment of the present invention, the hole transport layer is prepared as follows: an aqueous solution of nickel oxide nanocrystals is dissolved in a volatile solvent to obtain a nickel oxide nanocrystal solution; then, the nickel oxide nanocrystal solution is coated to form a wet film of the hole transport layer; subsequently, an airflow with a temperature of 50°C to 70°C and a pressure of 0.8 MPa to 1.2 MPa is blown toward the surface of the wet film of the hole transport layer to obtain the hole transport layer. The volatile solvent is one or more of ethanol, acetonitrile, and isopropanol; and / or,
[0035] The electron transport layer is prepared by the following method: C 60 Dissolved in chlorobenzene, and mixed with ethanol, yields C 60 Solution, then coat C 60 The solution forms a wet electron transport layer film, and then an airflow with a temperature of 40℃~60℃ and a pressure of 0.6MPa~1MPa is blown towards the surface of the wet electron transport layer film to obtain the electron transport layer; and / or,
[0036] The method for preparing the hole-modified layer is as follows: 2PACz is dissolved in ethanol to obtain a 2PACz solution, then the 2PACz solution is coated to form a wet film of the hole-modified layer, and then an airflow with a temperature of 40℃~50℃ and a pressure of 0.2MPa~0.5MPa is blown towards the surface of the wet film of the hole-modified layer to obtain the hole-modified layer; and / or,
[0037] A passivation layer is further prepared between the perovskite layer and the electron transport layer. The passivation layer is prepared as follows: 2-thiopheneethylamine bromide is dissolved in isopropanol to obtain a 2-thiopheneethylamine bromide solution; then, the 2-thiopheneethylamine bromide solution is coated to form a wet passivation film; subsequently, an airflow with a temperature of 50℃~60℃ and a pressure of 0.4MPa~0.6MPa is blown towards the surface of the wet passivation film to obtain the passivation layer; and / or,
[0038] The buffer layer is prepared as follows: a tin dioxide hydrocolloid solution is dissolved in a mixed solvent of water and ethanol to obtain a tin dioxide solution. The tin dioxide solution is then coated to form a wet buffer film. Subsequently, an airflow with a temperature of 50℃~70℃ and a wind pressure of 0.5MPa~1MPa is blown toward the surface of the wet buffer film to obtain the buffer layer.
[0039] As an optional implementation, in the embodiments of the present invention, during the preparation of the hole transport layer, the concentration of the nickel oxide nanocrystal solution is 10 mg / mL to 15 mg / mL, the slit spacing is 50 μm to 80 μm, the coating speed is 7 mm / s to 14 mm / s, and the thickness of the wet film of the hole transport layer is 2 μm to 5 μm; and / or,
[0040] During the fabrication of the electron transport layer, the C 60 The solution concentration is 0.8 mg / ml to 2.0 mg / ml, the slit spacing is 30 μm to 70 μm, the coating speed is 7 mm / s to 14 mm / s, and the thickness of the wet film of the electron transport layer is 4 μm to 7 μm; and / or,
[0041] During the preparation of the hole-modified layer, the concentration of the 2PACz solution is 0.1 mg / ml to 0.5 mg / ml, the slit spacing is 15 μm to 25 μm, the coating speed is 10 mm / s to 20 mm / s, and the thickness of the passivation layer wet film is 1 μm to 3 μm; and / or,
[0042] During the preparation of the passivation layer, the concentration of the 2-thiophene ethylamine bromide solution is 0.8 mg / ml to 2.0 mg / ml, the slit spacing is 20 μm to 40 μm, the coating speed is 15 mm / s to 25 mm / s, and the thickness of the wet passivation layer is 1 μm to 4 μm; and / or,
[0043] During the preparation of the buffer layer, the concentration of the tin dioxide aqueous colloidal solution is 1.5% to 5%, the slit spacing is 50 μm to 80 μm, the coating speed is 7 mm / s to 14 mm / s, and the thickness of the passivation layer wet film is 1 μm to 5 μm.
[0044] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0045] This invention provides a perovskite precursor solution. The mixed solvent used in this perovskite precursor solution has a viscosity of 2 mPa·s to 3.5 mPa·s. Because the mixed solvent contains a specific proportion of a first solvent with a low boiling point and high volatility, the perovskite precursor solution, when coated onto a pyramidal textured substrate, exhibits relatively low fluidity due to the specific viscosity achieved by adding the first solvent. This allows for uniform coating on the pyramidal textured substrate, forming a perovskite layer with good thickness uniformity, and stable adhesion to the surface of the pyramidal textured substrate. Especially on textured substrates with a pyramid height greater than 2 μm, it can stably cover the pyramid tip without easily depositing to the bottom. Furthermore, due to the addition of the specific proportion of the first solvent, the mixed solvent in the perovskite precursor solution can evaporate rapidly, promoting the rapid in-situ crystallization and growth of the perovskite material in the perovskite precursor, forming a perovskite layer with excellent shape-preserving coverage. The mixed solvent of this perovskite precursor solution can evaporate rapidly and crystallize and grow in situ quickly without annealing, thus obtaining a perovskite layer with no obvious solvent residue and excellent crystal growth effect.
[0046] In summary, by using the above-mentioned perovskite precursor solution, a perovskite layer with both excellent shape retention and crystallization effect can be prepared on a pyramid-patterned substrate. This solves the problem of difficulty in achieving shape retention and coverage when preparing perovskite layers on a pyramid-patterned substrate using solution methods. At the same time, a perovskite layer with excellent crystallization effect can be obtained without further annealing. Attached Figure Description
[0047] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0048] Figure 1 This is a schematic diagram of the structure of the perovskite tandem solar cell disclosed in the embodiments of the present invention;
[0049] Figure 2 This is a schematic diagram of the structure of another perovskite tandem solar cell disclosed in an embodiment of the present invention;
[0050] Figure 3 This is a SEM scan of the perovskite layer in Embodiment 1 of the present invention.
[0051] Icons: 1. Heterojunction base cell; 2. First transparent conductive layer; 3. Hole transport layer; 31. Hole modification layer; 4. Perovskite layer; 41. Passivation layer; 5. Electron transport layer; 51. Buffer layer; 6. Second transparent conductive layer; 71. Positive electrode; 72. Negative electrode; 8. Anti-reflection layer. Detailed Implementation
[0052] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0053] Solution-based perovskite layer fabrication involves coating a perovskite precursor solution to form a wet film, followed by annealing to obtain the perovskite layer. Currently, solution-based perovskite layer fabrication is generally only suitable for planar substrates or small-area pyramidal textured substrates (pyramid height less than 2 μm). It is unsuitable for large-area pyramidal textured substrates because when the perovskite precursor solution is coated onto the pyramidal textured substrate, it tends to deposit at the bottom of the pyramid, failing to cover the apex and potentially leading to short circuits. Commercially available silicon-based solar cells have large pyramidal textured areas, typically greater than 2 μm in height, making it easier for the perovskite precursor solution to deposit at the bottom of the pyramidal texture, hindering conformal growth on large-area pyramidal textured substrates. Currently, when preparing perovskite layers on large-area textured substrates, a vacuum evaporation method is generally used to first deposit a lead iodide layer, and then a cationic solution is applied by solution method to allow the cationic solution to react with the lead iodide layer. Although this method can achieve good shape preservation, it requires two steps of growth, which is cumbersome and not conducive to improving production efficiency.
[0054] Therefore, this application provides a perovskite precursor solution and its preparation method, as well as a perovskite layer tandem solar cell and its preparation method. By using a specific perovskite precursor solution as the solution for preparing the perovskite layer, it solves the problem of the difficulty in achieving conformal growth when preparing perovskite layers on pyramid-patterned substrates using solution methods. At the same time, it has the advantages of simple preparation process, convenient operation, and suitability for industrial production.
[0055] Furthermore, this perovskite precursor solution can prepare perovskite layers with good shape retention on both large-area and small-area pyramid-patterned substrates, demonstrating its wide applicability.
[0056] The technical solution of the present invention will be further described below with reference to the embodiments and accompanying drawings.
[0057] In one aspect, embodiments of this application provide a perovskite precursor solution.
[0058] The perovskite precursor solution includes perovskite material and a mixed solvent. The viscosity of the mixed solvent is 2 mPa·s to 3.5 mPa·s. The mixed solvent includes a first solvent, which accounts for 10% to 40% of the volume of the mixed solvent. The boiling point of the first solvent is 80℃ to 130℃.
[0059] The viscosity of the aforementioned mixed solvent is 2 mPa·s to 3.5 mPa·s. Because the mixed solvent contains a specific proportion of a first solvent with a low boiling point and high volatility, the perovskite precursor solution, when coated onto a pyramid-patterned substrate, exhibits relatively low fluidity due to the specific viscosity of the perovskite precursor solution prepared by adding the first solvent in a specific proportion. This allows for uniform coating on the pyramid-patterned substrate, forming a perovskite layer 4 with good thickness uniformity, and also ensures stable adhesion to the surface of the pyramid-patterned substrate. Especially on pyramid-height substrates, it can stably cover the pyramid tip without easily depositing to the bottom. Furthermore, due to the addition of the first solvent in the aforementioned specific proportion, the mixed solvent in the perovskite precursor solution evaporates rapidly, promoting the rapid in-situ crystallization and growth of the perovskite material in the perovskite precursor, forming a perovskite layer 4 with excellent shape-preserving coverage. The mixed solvent of this perovskite precursor solution can evaporate rapidly and crystallize and grow in situ quickly without the need for annealing, thus obtaining a perovskite layer 4 with no obvious solvent residue and excellent crystal growth effect.
[0060] In summary, by using the above-mentioned perovskite precursor solution, a perovskite layer 4 with excellent shape retention and crystallization effect can be prepared on a pyramid-patterned substrate. This solves the problem that it is difficult to achieve shape retention and coverage when preparing the perovskite layer 4 on a pyramid-patterned substrate using the solution method. At the same time, a perovskite layer 4 with excellent crystallization effect can be obtained without further annealing.
[0061] For example, the viscosity of the mixed solvent can be 2 mPa·s, 2.3 mPa·s, 2.6 mPa·s, 2.9 mPa·s, 3.2 mPa·s, and 3.5 mPa·s, etc. The boiling point of the first solvent is 80°C, 90°C, 100°C, 110°C, 120°C, and 130°C, etc.
[0062] Preferably, the second solvent is one or a combination of two of dimethyl sulfoxide and 1,8-diiodooctane.
[0063] By specifically selecting dimethyl sulfoxide and 1,8-diiodooctane, both with high viscosity, as the second solvent, the viscosity of the mixed solvent is rapidly increased. Adjusting the viscosity of the mixed solvent to the aforementioned specific range improves the application performance of the perovskite precursor solution and enhances its adhesion stability on the pyramid-patterned substrate, enabling the perovskite precursor solution to quickly form a conformal, covering perovskite wet film layer on the pyramid-patterned substrate after coating. Simultaneously, the iodide ions in 1,8-diiodooctane participate in the formation of perovskite crystals, promoting in-situ crystallization of the perovskite material, reducing the fluidity of the perovskite wet film layer, and further enhancing the conformal coverage effect of the perovskite layer 4.
[0064] The perovskite material mentioned above can be a tricationic system material. The perovskite material can be any three of the following tricationic systems: methylamine iodine (MAI), methylimidazolium iodide (FAI), methylamine bromide (MABr), methylimidazolium bromide (FABr), methylamine chloride (MACl), cesium iodide (CsI), and cesium bromide (CsBr). The specific selection of the perovskite material composition does not affect the preparation of the conformal perovskite layer 4 on the pyramid-textured substrate by the above perovskite precursor solution. The specific selection of the perovskite composition is not limited in the embodiments of this application.
[0065] More preferably, the second solvent is composed of dimethyl sulfoxide and 1,8-diiodooctane in a mass ratio of 0.4 to 0.8:1.
[0066] When dimethyl sulfoxide and 1,8-diiodooctane are mixed in the above ratio, the resulting solution has a high viscosity, which is beneficial for the stable adhesion of the perovskite precursor solution to the surface of the pyramid-patterned substrate. At the same time, 1,8-diiodooctane participates in the crystallization reaction of the perovskite layer 4, which helps to promote the formation of perovskite crystals, improve the crystallization effect of the perovskite layer 4, reduce crystallization defects in the perovskite layer 4, and enhance the stability of the perovskite layer 4.
[0067] In some embodiments, the first solvent includes one or more of acetonitrile, ethanol, 2-methoxyethanol, and isopropanol.
[0068] Acetonitrile, ethanol, 2-methoxyethanol and isopropanol have high volatility, which can effectively promote the growth of perovskite grains and facilitate the rapid film formation of the perovskite precursor solution after coating, thereby accelerating the preparation of perovskite layer 4 and reducing preparation time and cost.
[0069] More preferably, the first solvent is composed of acetonitrile and 2-methoxyethanol in a volume ratio of (0.25 to 0.82):1. Exemplarily, the volume ratio of acetonitrile to 2-methoxyethanol can be 0.25:1, 0.3:1, 0.35:1, 0.45:1, 0.55:1, 0.65:1, 0.75:1, 0.82:1, etc.
[0070] In some embodiments, the concentration of the perovskite precursor solution is 0.8 mol / mL to 2 mol / mL.
[0071] The perovskite precursor solution at the above concentration has high viscosity, resulting in better adhesion to large-area pyramidal textured substrates, higher crystallinity after coating, and better film quality. For example, the concentration of the perovskite precursor solution can be 0.8 mol / mL, 1 mol / mL, 1.2 mol / mL, 1.4 mol / mL, 1.6 mol / mL, 1.8 mol / mL, and 2 mol / mL, etc.
[0072] Secondly, embodiments of this application provide a method for preparing a perovskite layer 4.
[0073] The preparation method of perovskite layer 4 is as follows:
[0074] Provides a base with a pyramidal suede finish;
[0075] A perovskite precursor solution is coated on a substrate to form a perovskite wet film layer, and an airflow with a temperature of 80℃~130℃ and a pressure of 1MPa~2MPa is blown toward the perovskite wet film layer. The temperature of the airflow is not lower than the boiling point of the first solvent, thus obtaining the perovskite layer 4.
[0076] When the above-mentioned perovskite precursor solution is used on a pyramid-patterned substrate, it can achieve rapid in-situ crystallization. It can be seen that the above-mentioned perovskite precursor solution is suitable for pyramid-patterned substrates and has excellent applicability to pyramid heights of 2μm to 6μm. For example, the pyramid height of the textured surface can be 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 6.5μm, 6μm, etc.
[0077] In some embodiments, the thickness of the perovskite layer 4 is 800 nm to 1500 nm.
[0078] The perovskite layer 4 of this thickness, prepared using a perovskite precursor solution, exhibits superior conformal growth and excellent light absorption, which is beneficial for improving the light absorption performance of solar cells. For example, the thickness of the perovskite layer 4 can be 800 nm, 900 nm, 1000 nm, 1100 nm, 1200 nm, 1300 nm, 1400 nm, 1500 nm, etc.
[0079] In some embodiments, the coating method for the perovskite precursor solution includes any one of slot coating, screen printing, and blade coating; and / or,
[0080] The coating speed of the perovskite precursor solution is 5 mm / s to 20 mm / s; and / or,
[0081] After coating with the perovskite precursor solution, the resulting wet perovskite film layer has a thickness of 5 μm to 10 μm; and / or,
[0082] The gas flow is nitrogen or an inert gas.
[0083] When perovskite layer 4 is prepared using slot coating, screen printing, and blade coating methods, the perovskite precursor solution exhibits good adhesion on large-area pyramidal textured substrates, which is beneficial for achieving a uniform shape retention effect. However, when spraying or spin coating is used, the perovskite precursor solution shows poor adhesion on large-area pyramidal textured substrates, which is detrimental to achieving a uniform shape retention effect.
[0084] When the coating speed is between 5 mm / s and 20 mm / s, the perovskite precursor solution exhibits good continuity in coating and is less prone to accumulation, which is beneficial for forming a perovskite layer 4 with excellent crystal quality. If the coating speed is too high, the perovskite precursor solution may become discontinuous; if the coating speed is too slow, the perovskite precursor solution may accumulate, thereby reducing the quality of the perovskite layer 4. Examples of coating speeds include 5 mm / s, 7 mm / s, 9 mm / s, 11 mm / s, 13 mm / s, 15 mm / s, 17 mm / s, and 20 mm / s.
[0085] After the perovskite precursor solution is coated, a relatively thick wet film is formed. With a thicker perovskite layer 4, the phenomenon of perovskite precursor solution depositing from the top to the bottom of the pyramid-patterned substrate is less likely to occur. This allows for the formation of a perovskite layer 4 that combines high thickness with good conformability, thereby improving the light absorption and electron transport capabilities of the perovskite layer 4. For example, the thickness of the wet film is 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, and 10 μm.
[0086] In some embodiments, when using the slit coating method, the slit size is controlled to be 70 μm to 110 μm.
[0087] By controlling the slit size to be 70μm to 110μm, it is beneficial for the flow of high-viscosity perovskite precursor solution and also for the formation of a thicker perovskite layer 4, thereby enhancing the light absorption capacity of the perovskite layer 4.
[0088] For example, the slit size can be 70μm, 80μm, 90μm, 100μm and 110μm, etc.
[0089] Thirdly, embodiments of this application provide a perovskite tandem solar cell.
[0090] Reference Figure 1The perovskite tandem solar cell includes a silicon substrate cell and a first transparent conductive layer 2, a hole transport layer 3, a perovskite layer 4, an electron transport layer 5, and a second transparent conductive layer 6 stacked sequentially on the silicon substrate cell. The perovskite layer 4 is prepared by the method of the second aspect of the perovskite layer 4 preparation. The perovskite tandem solar cell also includes a positive electrode 71 and a negative electrode 72. The positive electrode 71 forms an ohmic contact with the electron transport layer 5, and the negative electrode 72 forms an ohmic contact with the silicon substrate cell.
[0091] The perovskite precursor solution described above has a fast evaporation rate, strong adhesion, and slow flow rate. It can evaporate quickly and crystallize into a film in situ, which helps to reduce process time and improve production efficiency.
[0092] The first transparent conductive layer 2 or the second transparent conductive layer 6 can be an indium tin oxide layer or an indium zinc oxide layer, the hole transport layer 3 can be a nickel oxide layer, and the electron transport layer 5 can be a C 60 layer.
[0093] refer to Figure 2 In some embodiments, a hole modification layer 31 is further disposed between the perovskite layer 4 and the hole transport layer 3; and / or, a passivation layer 41 is further disposed between the perovskite layer 4 and the electron transport layer 5; and / or, a buffer layer 51 is further disposed on the electron transport layer 5 away from the silicon substrate cell, and an antireflection layer 8 is further disposed on the side of the second transparent conductive layer 6 away from the silicon substrate cell.
[0094] The hole modification layer 31 can be a 2PACz layer, the passivation layer 41 can be a lithium fluoride layer or a 2-thiophene ethylamine bromide layer, the buffer layer 51 can be a tin dioxide layer, and the anti-reflection layer 8 can be a lithium fluoride or a magnesium fluoride.
[0095] The hole transport layer 3 has a thickness of 15 nm to 25 nm; and / or, the electron transport layer 5 has a thickness of 10 nm to 20 nm; and / or, the hole modification layer 31 has a thickness of 1 nm to 5 nm; and / or, the passivation layer 41 has a thickness of 1 nm to 3 nm; and / or, the buffer layer 51 has a thickness of 10 nm to 20 nm, and the antireflection layer 8 has a thickness of 90 nm to 120 nm.
[0096] For example, the thickness of the hole transport layer 3 can be 15nm, 17nm, 19nm, 21nm, 23nm, and 25nm, etc. The thickness of the hole modification layer 31 can be 1nm, 2nm, 3nm, 4nm, and 5nm, etc. The thickness of the passivation layer 41 can be 1nm, 1.5nm, 2.5nm, and 3nm, etc. The thickness of the buffer layer 51 can be 10nm, 12nm, 14nm, 16nm, 18nm, and 20nm, etc. The thickness of the antireflection layer 8 can be 90nm, 95nm, 100nm, 105nm, 110nm, 115nm, and 120nm, etc.
[0097] Fourthly, embodiments of this application provide a method for fabricating a perovskite tandem solar cell, which includes the following steps:
[0098] Provide silicon-based solar cells;
[0099] A first transparent conductive layer 2 is fabricated on the front side of a silicon substrate solar cell;
[0100] A hole transport layer 3 is fabricated on the first transparent conductive layer 2;
[0101] A perovskite layer 4 is prepared on the hole transport layer 3, and the perovskite layer 4 is prepared by the method of the second aspect of the perovskite layer 4 preparation method.
[0102] An electron transport layer 5 is prepared on the perovskite layer 4;
[0103] A second transparent conductive layer 6 is fabricated on the electron transport layer 5;
[0104] A positive electrode 71 is fabricated on the second transparent conductive layer 6, and a negative electrode 72 is fabricated on the back side of the silicon substrate cell to obtain the above-mentioned perovskite tandem solar cell.
[0105] The perovskite layer 4 prepared by the above method has excellent crystallinity, high thickness and good shape retention, and does not require annealing treatment as in the traditional solution method for perovskite preparation. Therefore, the above perovskite tandem solar cell has excellent energy conversion efficiency, and the preparation time is shortened, thus improving production efficiency.
[0106] In some embodiments, a hole modification layer 31 is further prepared between the hole transport layer 3 and the perovskite layer 4, a passivation layer 41 is further prepared between the perovskite layer 4 and the electron transport layer 5, and a buffer layer 51 is further prepared on the side of the electron transport layer 5 facing away from the silicon substrate; and / or,
[0107] Hole transport layer 3, hole modification layer 31, passivation layer 41, electron transport layer 5 and / or buffer layer 51 are prepared by slot coating.
[0108] The aforementioned functional layers, such as hole transport layer 3, hole modification layer 31, passivation layer 41, electron transport layer 5, and buffer layer 51, can all be prepared by slot coating.
[0109] In the slit coating process, a device that links slit heads with air knives can be used to link multiple heads with air knives. Different slit heads corresponding to different film layers use different coating processes, and the corresponding air knife heating temperature and air flow rate are different. After the slit heads are coated, the air knife heating assists solvent evaporation, which accelerates the film formation speed, reduces the need for subsequent back-off processing, and enables rapid deposition of multi-layer films, thereby reducing time costs.
[0110] Specifically, in the process of sequentially preparing hole transport layer 3, electron transport layer 5, hole modification layer 31, passivation layer 41 and buffer layer 51 using the above-mentioned slit coating method, the raw materials of hole transport layer 3, electron transport layer 5, hole modification layer 31, passivation layer 41 and buffer layer 51 are first prepared into solutions of appropriate concentrations with a certain volatile solvent. The solutions are then uniformly pushed to the slit coating head, and the stage moves at a uniform speed to uniformly coat the solution onto the substrate surface with a pyramidal texture to form a wet film. The uniformity and thickness of the above-mentioned film layers are controlled by adjusting parameters such as slit size, wet film thickness, coating start and end positions, coating speed, and liquid filling time. After coating, the wet film is subjected to solvent evaporation assisted by heated airflow to accelerate film crystal growth, achieve film shape preservation and form the desired thin film.
[0111] In some embodiments, the hole transport layer 3 is prepared as follows: an aqueous solution of nickel oxide nanocrystals is dissolved in a volatile solvent to obtain a nickel oxide nanocrystal solution; then, the nickel oxide nanocrystal solution is coated to form a wet film of the hole transport layer 3; subsequently, an airflow with a temperature of 50°C to 70°C and a pressure of 0.8 MPa to 1.2 MPa is blown towards the surface of the wet film of the hole transport layer 3 to obtain the hole transport layer 3. The volatile solvent is one or more of ethanol, acetonitrile, and isopropanol; and / or,
[0112] The method for preparing electron transport layer 5 is as follows: C 60 Dissolved in chlorobenzene and mixed with ethanol, a C60 solution is obtained. The C60 solution is then coated to form a wet film of electron transport layer 5. Subsequently, an airflow at a temperature of 40°C–60°C and a pressure of 0.6 MPa–1 MPa is blown towards the surface of the wet film of electron transport layer 5 to obtain electron transport layer 5; and / or,
[0113] The hole-modified layer 31 is prepared as follows: 2PACz is dissolved in ethanol to obtain a 2PACz solution. The 2PACz solution is then coated to form a wet film of the hole-modified layer 31. Subsequently, an airflow with a temperature of 40℃~50℃ and a pressure of 0.2MPa~0.5MPa is blown towards the surface of the wet film of the hole-modified layer 31 to obtain the hole-modified layer 31; and / or,
[0114] A passivation layer 41 is also prepared between the perovskite layer 4 and the electron transport layer 5. The passivation layer 41 is prepared as follows: 2-thiophene ethylamine bromide is dissolved in isopropanol to obtain a 2-thiophene ethylamine bromide solution. Then, the 2-thiophene ethylamine bromide solution is coated to form a wet film of passivation layer 41. Subsequently, an airflow with a temperature of 50℃~60℃ and a pressure of 0.4MPa~0.6MPa is blown towards the surface of the wet film of passivation layer 41 to obtain passivation layer 41; and / or,
[0115] The buffer layer 51 is prepared as follows: a tin dioxide hydrocolloid solution is dissolved in a mixed solvent of water and ethanol to obtain a tin dioxide solution. Then, the tin dioxide solution is coated to form a wet film of buffer layer 51. Subsequently, an airflow with a temperature of 50℃~70℃ and a wind pressure of 0.5MPa~1MPa is blown toward the surface of the wet film of buffer layer 51 to obtain buffer layer 51.
[0116] In some embodiments, during the preparation of hole transport layer 3, the concentration of the nickel oxide nanocrystal solution is 10 mg / mL to 15 mg / mL, the slit spacing is 50 μm to 80 μm, the coating speed is 7 mm / s to 14 mm / s, and the thickness of the wet film of hole transport layer 3 is 2 μm to 5 μm; and / or,
[0117] During the fabrication of electron transport layer 5, C 60 The solution concentration is 0.8 mg / ml to 2.0 mg / ml, the slit spacing is 30 μm to 70 μm, the coating speed is 7 mm / s to 14 mm / s, and the thickness of the wet film of electron transport layer 5 is 4 μm to 7 μm; and / or,
[0118] During the preparation of the hole-modified layer 31, the concentration of the 2PACz solution is 0.1 mg / ml to 0.5 mg / ml, the slit spacing is 15 μm to 25 μm, the coating speed is 10 mm / s to 20 mm / s, and the thickness of the wet film of the passivation layer 41 is 1 μm to 3 μm; and / or,
[0119] During the preparation of passivation layer 41, the concentration of the 2-thiophene ethylamine bromide solution is 0.8 mg / ml to 2.0 mg / ml, the slit spacing is 20 μm to 40 μm, the coating speed is 15 mm / s to 25 mm / s, and the thickness of the wet film of passivation layer 41 is 1 μm to 4 μm; and / or,
[0120] During the preparation of buffer layer 51, the concentration of tin dioxide aqueous colloidal solution is 1.5% to 5%, the slit spacing is 50 μm to 80 μm, the coating speed is 7 mm / s to 14 mm / s, and the thickness of the wet film of passivation layer 41 is 1 μm to 5 μm.
[0121] The technical solution of this application will be described below with reference to more specific embodiments and accompanying drawings.
[0122] Example 1
[0123] This application provides a perovskite tandem solar cell, comprising:
[0124] Heterojunction bottom cell 1, the height of the pyramid textured surface of the heterojunction bottom cell is 5μm;
[0125] A first transparent electrode layer is stacked on the front side of the heterojunction bottom cell 1. The material of the first transparent electrode layer is indium tin oxide, and the thickness is 90 nm.
[0126] Hole transport layer 3 is stacked on the side of the transparent electrode layer away from the heterojunction bottom cell 1. The hole transport layer 3 is made of nickel oxide and has a thickness of 17 nm.
[0127] A hole modification layer 31 is stacked on the side of the hole transport layer 3 facing away from the heterojunction bottom cell 1. The hole modification layer 31 is made of [material name missing] and has a thickness of 2 nm.
[0128] The perovskite layer 4 stacked on the side of the hole modification layer 31 away from the heterojunction bottom cell 1 has a thickness of 1000 nm.
[0129] A passivation layer 41 is stacked on the side of the perovskite layer 4 away from the heterojunction bottom cell 1. The material of the passivation layer 41 is 2-thiophene ethylamine bromide, and the thickness is 1.5 nm.
[0130] An electron transport layer 5 is stacked on the side of the passivation layer 41 away from the heterojunction bottom cell 1. The electron transport layer 5 is made of C60 and has a thickness of 15nm.
[0131] A buffer layer 51 is stacked on the side of the electron transport layer 5 away from the heterojunction bottom cell 1. The buffer layer 51 is made of tin dioxide and has a thickness of 15nm.
[0132] A second transparent electrode layer is stacked on the side of the buffer layer 51 away from the heterojunction bottom cell 1. The second transparent electrode layer is indium zinc oxide and has a thickness of 100 nm.
[0133] An antireflection layer 8 is stacked on the side of the second transparent electrode layer away from the heterojunction bottom cell 1. The antireflection layer 8 is made of magnesium fluoride and has a thickness of 110 nm.
[0134] It also includes a positive electrode 71 and a negative electrode 72, both of which are silver electrodes. The thicknesses of the positive electrode 71 and the negative electrode 72 are 275 nm, respectively. The positive electrode 71 forms an ohmic contact with the transparent electrode layer, and the negative electrode 72 forms an ohmic contact with the heterojunction bottom cell 1.
[0135] The fabrication method of the above-mentioned perovskite tandem solar cell is as follows:
[0136] Provide heterojunction bottom cell 1;
[0137] A first transparent conductive layer 2 is prepared on the front side of the heterojunction bottom cell 1 by magnetron sputtering.
[0138] A hole transport layer 3, a hole modification layer 31, a perovskite layer 4, a passivation layer 41, an electron transport layer 5, and a buffer layer 51 are sequentially prepared on the first transparent conductive layer 2 using a slit coating method. The specific steps are as follows:
[0139] Preparation of hole transport layer 3: An aqueous solution of nickel oxide nanocrystals was dissolved in ethanol to obtain a nickel oxide nanocrystal solution with a concentration of 10 mg / mL to 15 mg / mL. Then, the nickel oxide nanocrystal solution was coated using a slit coating method to form a wet film of hole transport layer 3, wherein the slit spacing was 60 μm, the coating speed was 10 mm / s, and the thickness of the wet film of hole transport layer 3 was 3 μm. Subsequently, an airflow with a temperature of 60 °C and a wind pressure of 1 MPa was blown toward the surface of the wet film of hole transport layer 3 to obtain hole transport layer 3.
[0140] Preparation of hole-modified layer 31: 2PACz is dissolved in ethanol to obtain a 2PACz solution with a concentration of 0.1 mg / ml to 0.5 mg / ml. Then, the 2PACz solution is coated by slit coating to form a wet film of hole-modified layer 31, wherein the slit spacing is 20 μm, the coating speed is 15 mm / s, and the thickness of the passivation layer 41 wet film is 1.5 μm. Subsequently, an airflow with a temperature of 45°C and a wind pressure of 0.3 MPa is blown toward the surface of the hole-modified layer 31 wet film to obtain hole-modified layer 31.
[0141] Preparation of perovskite layer 4: The perovskite material Cs 0.05 (FA 0.77 MA 0.23 ) 0.95 Pb(I 0.77 Br 0.23 )3 is dissolved in a mixed solvent to obtain a perovskite precursor solution with a concentration of 0.8 mg / ml to 2.0 mg / ml. The mixed solvent consists of a second solvent with a volume ratio of 80% and a first solvent with a volume ratio of 20%. The second solvent consists of dimethyl sulfoxide and 1,8-diiodooctane in a mass ratio of 0.6:1, and the first solvent consists of acetonitrile and 2-methoxyethanol in a mass ratio of 0.4:1. The perovskite precursor solution is coated onto the hole modification layer 31 to form a perovskite wet film layer, and an airflow with a temperature of 120°C and a wind pressure of 1.5 MPa is blown toward the perovskite wet film layer. The temperature of the airflow is not lower than the boiling point of the first solvent, thus obtaining the perovskite layer 4.
[0142] Preparation of passivation layer 41: 2-Thiophene ethylamine bromide is dissolved in isopropanol to obtain a 2-thiophene ethylamine bromide solution with a concentration of 0.8 mg / ml to 2.0 mg / ml. The 2-thiophene ethylamine bromide solution is then coated to form a wet film of passivation layer 41, wherein the slit spacing is 30 μm, the coating speed is 20 mm / s, and the thickness of the wet film of passivation layer 41 is 2 μm. Subsequently, an airflow at a temperature of 55°C and a pressure of 0.5 MPa is blown towards the surface of the wet film of passivation layer 41 to obtain passivation layer 41; and / or,
[0143] Preparation of electron transport layer 5: C60 is dissolved in chlorobenzene and doped with ethanol to obtain a C60 solution with a concentration of 0.8 mg / ml to 2.0 mg / ml. Then, the C60 solution is coated to form a wet film of electron transport layer 5, wherein the slit spacing is 50 μm, the coating speed is 10 mm / s, and the thickness of the wet film of electron transport layer 5 is 5 μm. Subsequently, an airflow with a temperature of 50°C and a wind pressure of 0.8 MPa is blown toward the surface of the wet film of electron transport layer 5 to obtain electron transport layer 5.
[0144] Preparation of buffer layer 51: A tin dioxide hydrocolloid solution is dissolved in a mixed solvent of water and ethanol to obtain a tin dioxide solution with a concentration of 1.5% to 5%. Then, the tin dioxide solution is coated to form a wet film of buffer layer 51, wherein the slit spacing is 60 μm, the coating speed is 10 mm / s, and the thickness of the passivation layer 41 wet film is 3 μm. Subsequently, an airflow with a temperature of 60 °C and a wind pressure of 0.7 MPa is blown toward the surface of the wet film of buffer layer 51 to obtain buffer layer 51.
[0145] A second transparent electrode layer was prepared on the buffer layer 51 by magnetron sputtering.
[0146] A positive electrode 71 is deposited in the second transparent electrode layer to form an ohmic contact between the positive electrode 71 and the second transparent electrode layer.
[0147] A negative electrode 72 is deposited on the back side of the heterojunction bottom cell 1, so that the negative electrode 72 and the heterojunction bottom cell 1 form an ohmic contact.
[0148] An antireflection layer 8 was prepared on the second transparent electrode layer by vapor deposition.
[0149] Example 2
[0150] This application provides a perovskite tandem solar cell, which differs from Example 1 in that: in the step of preparing the perovskite layer 4, the volume ratio of the second solvent is 90%, the volume ratio of the first solvent is 10%, and the rest is the same as in Example 1.
[0151] Example 3
[0152] This application provides a perovskite tandem solar cell, which differs from Embodiment 1 in that:
[0153] In the step of preparing the perovskite layer 4, the volume ratio of the second solvent is 70%, the volume ratio of the first solvent is 30%, and the rest is consistent with Example 1.
[0154] Example 4
[0155] This application provides a perovskite tandem solar cell, which differs from Embodiment 1 in that:
[0156] In the step of preparing the perovskite layer 4, the volume ratio of the second solvent is 40%, the volume ratio of the first solvent is 60%, and the rest is consistent with Example 1.
[0157] Example 5
[0158] This application provides a perovskite tandem solar cell, which differs from Embodiment 1 in that:
[0159] In the step of preparing perovskite layer 4, the second solvent is dimethyl sulfoxide, and the rest is consistent with Example 1.
[0160] Comparative Example 1
[0161] This application provides a perovskite tandem solar cell as a comparative example, which differs from Example 1 in that:
[0162] In the step of preparing the perovskite layer 4, only the second solvent is used in the mixed solvent, and the first solvent is not used. The rest is consistent with Example 1.
[0163] Comparative Example 2
[0164] This application provides a perovskite tandem solar cell as a comparative example, which differs from Example 1 in that:
[0165] In the step of preparing the perovskite layer 4, only the first solvent is used in the mixed solvent, and the second solvent is not used. The rest is consistent with Example 1.
[0166] Experiment 1
[0167] The perovskite layer of Example 1 was scanned by SEM, and the results are shown in [Figure number missing]. Figure 3 .
[0168] pass Figure 3 It can be seen that the perovskite layer grows in a conformal manner along the pyramidal textured surface, proving that the perovskite layer prepared on the pyramidal textured substrate by the above-mentioned perovskite precursor solution has a better conformal effect.
[0169] Experiment 2
[0170] The performance of perovskite tandem solar cells was tested using the Wavelabs solar simulator under the following conditions: AM1.5, 1000 W / m². 2 The test environment temperature was 25℃. Before testing, the light source was calibrated to simulate sunlight intensity using a standard silicon cell. Performance tests included power conversion efficiency (PCE), open-circuit voltage (Voc), short-circuit current (Jsc), and fill factor (FF).
[0171] Table 1
[0172] PCE (%) Voc(V) FF (%) <![CDATA[Jsc(mA / cm 2 )]]> Example 1 27.79 1.737 75.50 21.19 Example 2 27.46 1.713 74.88 21.40 Example 3 28.67 1.736 76.80 21.50 Example 4 27.28 1.713 72.56 21.95 Example 5 26.34 1.679 73.30 21.40 Comparative Example 1 25.94 1.674 72.42 21.40 Comparative Example 2 24.51 1.647 70.29 21.17
[0173] As can be seen from the data in Table 1, compared with Comparative Example 1, the perovskite tandem solar cell in Example 1 shows a 1.85% increase in PCE, a 0.063V increase in Voc, a 3.08% increase in FF, and a 0.21mA / cm decrease in Jsc. 2 This demonstrates that in the perovskite precursor solution, using only the second solvent with higher viscosity in the mixed solvent, without adding the first solvent with a lower boiling point, results in poor crystal quality of the perovskite layer. This leads to a significant decrease in Voc and FF of the perovskite layer, ultimately resulting in a significant reduction in the PCE of the perovskite tandem solar cell. Compared to Comparative Example 2, the perovskite tandem solar cell in Example 1 shows a 3.28% increase in PCE, a 0.09V increase in Voc, a 5.21% increase in FF, and a 0.02mA / cm decrease in Jsc. 2 This study demonstrates that in the perovskite precursor solution, using only the first solvent with a lower boiling point in the mixed solvent without adding the second solvent with a higher viscosity results in a decrease in the crystal quality of the obtained perovskite layer and a relatively reduced shape retention effect, leading to a significant decrease in Voc, FF, and PCE of the perovskite layer.
[0174] The test results from Example 1, Comparative Example 1, and Comparative Example 2 show that when a first solvent with a lower boiling point is mixed with a second solvent with a higher viscosity in a specific ratio, the perovskite layer prepared from the perovskite precursor solution can achieve conformal coverage on the surface of the pyramid-patterned substrate while obtaining a better crystallization effect. This surpasses the conformal effect of perovskite layer preparation on pyramid-patterned substrate using the solution method. Furthermore, by using a combination of coating and immediate air knife heating process, the perovskite layer prepared from this perovskite precursor solution can rapidly crystallize and grow in situ without annealing, resulting in a perovskite layer with excellent crystal quality.
[0175] The foregoing has provided a detailed description of the perovskite precursor solution, the preparation method of the perovskite layer, and the perovskite tandem solar cell and its preparation method disclosed in the embodiments of the present invention. Specific examples have been used to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the perovskite precursor solution, the preparation method of the perovskite layer, and the perovskite tandem solar cell and its preparation method, as well as their core ideas. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A perovskite precursor solution, characterized in that, The mixture includes perovskite material and a mixed solvent, wherein the viscosity of the mixed solvent is 2 mPa·s to 3.5 mPa·s, the mixed solvent includes a first solvent, the volume of which accounts for 10% to 40% of the mixed solvent, and the boiling point of the first solvent is 80°C to 130°C. The mixed solvent further includes a second solvent, which includes one or both of dimethyl sulfoxide and 1,8-diiodooctane.
2. The perovskite precursor solution according to claim 1, characterized in that, The second solvent is composed of the dimethyl sulfoxide and the 1,8-diiodooctane in a mass ratio of 0.4 to 0.8:
1.
3. The perovskite precursor solution according to claim 1, characterized in that, The first solvent includes one or more of acetonitrile, ethanol, 2-methoxyethanol and isopropanol.
4. The perovskite precursor solution according to claim 3, characterized in that, The first solvent is composed of the acetonitrile and the 2-methoxyethanol in a volume ratio of (0.25~0.82):
1.
5. The perovskite precursor solution according to claim 1, characterized in that, The concentration of the perovskite precursor solution is 0.8 mol / mL to 2 mol / mL.
6. A method for preparing a perovskite layer, characterized in that, Includes the following steps: Provides a base with a pyramidal suede finish; A perovskite precursor solution as described in any one of claims 1-5 is coated on the substrate to form a perovskite wet film layer, and an airflow with a temperature of 80°C to 130°C and a wind pressure of 1 MPa to 2 MPa is blown toward the perovskite wet film layer, wherein the temperature of the airflow is not lower than the boiling point of the first solvent, thereby obtaining the perovskite layer.
7. The method for preparing the perovskite layer according to claim 6, characterized in that, The thickness of the perovskite layer is 800 nm to 1500 nm.
8. The method for preparing a perovskite layer according to claim 6, characterized in that, The coating method for the perovskite precursor solution includes any one of slot coating, screen printing, and blade coating; and / or, The perovskite precursor solution is coated at a rate of 5 mm / s to 20 mm / s; and / or, After the perovskite precursor solution is coated, the thickness of the resulting perovskite wet film is 5 μm to 10 μm; and / or, The gas flow is nitrogen or an inert gas.
9. The method for preparing a perovskite layer according to claim 8, characterized in that, When using the slit coating method, the slit size is controlled to be 70 μm to 110 μm.
10. A perovskite tandem solar cell, characterized in that, The perovskite tandem solar cell includes a silicon substrate cell and a first transparent conductive layer, a hole transport layer, a perovskite layer, an electron transport layer, and a second transparent conductive layer sequentially stacked on the silicon substrate cell. The perovskite layer is prepared by the perovskite layer preparation method according to any one of claims 6-9. The perovskite tandem solar cell also includes a positive electrode and a negative electrode. The positive electrode forms an ohmic contact with the electron transport layer, and the negative electrode forms an ohmic contact with the silicon substrate cell.
11. The perovskite tandem solar cell according to claim 10, characterized in that, A hole modification layer is further disposed between the perovskite layer and the hole transport layer; and / or, a passivation layer is further disposed between the perovskite layer and the electron transport layer; and / or, a buffer layer is further disposed on the side of the electron transport layer away from the silicon substrate cell, and an antireflection layer is further disposed on the side of the second transparent conductive layer away from the silicon substrate cell.
12. The perovskite tandem solar cell according to claim 11, characterized in that, The hole transport layer has a thickness of 15 nm to 25 nm; and / or, the electron transport layer has a thickness of 10 nm to 20 nm; and / or, the hole modification layer has a thickness of 1 nm to 5 nm; and / or, the passivation layer has a thickness of 1 nm to 3 nm; and / or, the buffer layer has a thickness of 10 nm to 20 nm, and the antireflection layer has a thickness of 90 nm to 120 nm.
13. A method for fabricating a perovskite tandem solar cell, characterized in that, Includes the following steps: Provide silicon-based solar cells; A hole transport layer is fabricated on the front side of the silicon substrate cell; A perovskite layer is prepared on the hole transport layer, wherein the perovskite layer is prepared by the method for preparing a perovskite layer as described in any one of claims 6-8; An electron transport layer is fabricated on the perovskite layer; A positive electrode and a negative electrode are fabricated on the electron transport layer to obtain the perovskite tandem solar cell.
14. The method for preparing a perovskite tandem solar cell according to claim 13, characterized in that, A hole modification layer is also prepared between the hole transport layer and the perovskite layer, and a passivation layer is also prepared between the perovskite layer and the electron transport layer. A buffer layer is also prepared on the side of the electron transport layer away from the silicon substrate cell. A second transparent conductive layer is also provided on the side of the buffer layer away from the electron transport layer, and an anti-reflection layer is also provided on the side of the second transparent conductive layer away from the silicon substrate cell.
15. The method for preparing a perovskite tandem solar cell according to claim 14, characterized in that, The hole transport layer, the hole modification layer, the passivation layer, the electron transport layer, and / or the buffer layer are fabricated using a slot coating method.
16. The method for preparing a perovskite tandem solar cell according to claim 15, characterized in that, The hole transport layer is prepared as follows: An aqueous solution of nickel oxide nanocrystals is dissolved in a volatile solvent to obtain a nickel oxide nanocrystal solution. The nickel oxide nanocrystal solution is then coated to form a wet film of the hole transport layer. Subsequently, an airflow with a temperature of 50°C to 70°C and a pressure of 0.8 MPa to 1.2 MPa is blown towards the surface of the wet film of the hole transport layer to obtain the hole transport layer. The volatile solvent is one or more of ethanol, acetonitrile, and isopropanol; and / or... The electron transport layer is prepared as follows: C60 is dissolved in chlorobenzene, and ethanol is added to obtain a C60 solution. The C60 solution is then coated to form a wet electron transport layer film. Subsequently, an airflow with a temperature of 40°C to 60°C and a pressure of 0.6 MPa to 1 MPa is blown towards the surface of the wet electron transport layer film to obtain the electron transport layer; and / or, The method for preparing the hole-modified layer is as follows: 2PACz is dissolved in ethanol to obtain a 2PACz solution, then the 2PACz solution is coated to form a wet film of the hole-modified layer, and then an airflow with a temperature of 40℃~50℃ and a pressure of 0.2 MPa~0.5 MPa is blown towards the surface of the wet film of the hole-modified layer to obtain the hole-modified layer; and / or, A passivation layer is further prepared between the perovskite layer and the electron transport layer. The passivation layer is prepared as follows: 2-thiophene ethylamine bromide is dissolved in isopropanol to obtain a 2-thiophene ethylamine bromide solution; then, the 2-thiophene ethylamine bromide solution is coated to form a wet passivation film; subsequently, an airflow with a temperature of 50℃~60℃ and a pressure of 0.4MPa~0.6MPa is blown towards the surface of the wet passivation film to obtain the passivation layer; and / or, The buffer layer is prepared as follows: a tin dioxide hydrocolloid solution is dissolved in a mixed solvent of water and ethanol to obtain a tin dioxide solution. The tin dioxide solution is then coated to form a wet buffer film. Subsequently, an airflow with a temperature of 50°C to 70°C and a wind pressure of 0.5 MPa to 1 MPa is blown toward the surface of the wet buffer film to obtain the buffer layer.
17. The method for preparing a perovskite tandem solar cell according to claim 16, characterized in that, During the preparation of the hole transport layer, the concentration of the nickel oxide nanocrystal solution is 10 mg / mL to 15 mg / mL, the slit spacing is 50 μm to 80 μm, the coating speed is 7 mm / s to 14 mm / s, and the thickness of the wet film of the hole transport layer is 2 μm to 5 μm; and / or, During the preparation of the electron transport layer, the concentration of the C60 solution is 0.8 mg / ml to 2.0 mg / ml, the slit spacing is 30 μm to 70 μm, the coating speed is 7 mm / s to 14 mm / s, and the thickness of the wet film of the electron transport layer is 4 μm to 7 μm; and / or, During the preparation of the hole-modified layer, the concentration of the 2PACz solution is 0.1 mg / ml to 0.5 mg / ml, the slit spacing is 15 μm to 25 μm, the coating speed is 10 mm / s to 20 mm / s, and the thickness of the passivation layer wet film is 1 μm to 3 μm; and / or, During the preparation of the passivation layer, the concentration of the 2-thiophene ethylamine bromide solution is 0.8 mg / ml to 2.0 mg / ml, the slit spacing is 20 μm to 40 μm, the coating speed is 15 mm / s to 25 mm / s, and the thickness of the wet passivation layer is 1 μm to 4 μm; and / or, During the preparation of the buffer layer, the concentration of the tin dioxide hydrocolloid solution is 1.5%~5%, the slit spacing is 50 μm~80 μm, the coating speed is 7 mm / s~14 mm / s, and the thickness of the passivation layer wet film is 1 μm~5 μm.
Citation Information
Patent Citations
In-site crystallization preparation method for high-viscosity liquid film creepage-suppression of suede uniform perovskite film