Positive electrode material, electrochemical device comprising the same, and electronic device

By doping Al and coating B on the surface of a lithium cobalt oxide matrix, synergistic first and second regions are formed, solving the problem of reduced stability of lithium-ion batteries under high voltage and improving cycle stability and cycle performance under high voltage.

CN117413384BActive Publication Date: 2026-11-20NINGDE AMPEREX TECHNOLOGY LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380012127.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2026-11-20
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

The stability of the cathode material in lithium-ion batteries decreases under high voltage, leading to a severe decline in cycle life.

Method used

Al is doped onto the surface of a lithium cobalt oxide matrix, and boron is coated onto the surface to form a first region and a second region. These regions work synergistically to stabilize the material structure, repair surface defect sites, and suppress side reactions and transition metal dissolution.

Benefits of technology

It significantly improves the cycling stability of cathode materials under high voltage, enhances the energy density and cycling performance of electrochemical devices, and extends the battery life and service life of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117413384B_ABST
    Figure CN117413384B_ABST
Patent Text Reader

Abstract

The application provides a positive electrode material, an electrochemical device containing the positive electrode material and an electronic device, and the positive electrode material comprises a substrate, a first region and a second region, wherein the first region is located on the surface of the substrate, and the second region is located on the surface of the first region; the substrate and the first region comprise a lithium cobalt oxide with a P63mc structure, the first region contains an Al element, and the second region contains a B element. The positive electrode material has good cycle stability at a high voltage, so that the electrochemical device has a high energy density and good cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery technology, and in particular to a cathode material, an electrochemical device comprising the cathode material, and an electronic device. Background Technology

[0002] Lithium-ion batteries have advantages such as high energy density, high operating voltage, low self-discharge rate, small size, and light weight, and are widely used in various fields such as portable electronic devices, drones, and electric vehicles. To meet the demand for long battery life, the operating voltage of lithium-ion batteries has been continuously increased. However, at high voltages, the stability of the cathode material decreases, leading to a significant reduction in the cycle life of lithium-ion batteries. Summary of the Invention

[0003] In view of this, the purpose of this application is to provide a positive electrode material, an electrochemical device comprising the positive electrode material, and an electronic device, so as to improve the cycle stability of the electrochemical device under high voltage.

[0004] A first aspect of this application provides a cathode material comprising a substrate, a first region, and a second region, wherein the first region is located on the surface of the substrate, and the second region is located on the surface of the first region; the substrate and the first region comprise lithium cobalt oxide with a P63mc structure, the first region contains Al, and the second region contains B. By doping the surface of the P63mc structured lithium cobalt oxide substrate with Al, the surface structure of the material can be stabilized; simultaneously, introducing B (boron) to coat the surface of the Al-doped first region can repair defect sites (such as pits and / or gaps) on the surface of the cathode material, suppressing side reactions between the cathode material and the electrolyte, and inhibiting the dissolution of transition metal elements. Therefore, the first and second regions work synergistically to significantly improve the cycle stability of the cathode material under high voltage.

[0005] In some implementations, the molar ratio n of Al to Co in the first region is... Al / n Co 0 <n Al / n Co ≤0.1. In some implementations, 0.001 ≤ n Al / n Co ≤0.01. At this point, Al can be uniformly doped into Co sites, better stabilizing the surface structure of the cathode material and thus improving the cycling stability of the cathode material under high voltage.

[0006] In some implementations, the molar ratio m of element B to element Co in the cathode material is... B / m Co 0 <m B / m Co≤0.05. In some implementations, 0.002≤m B / m Co ≤0.02. At this temperature, element B can better repair defect sites on the surface of the cathode material, suppress side reactions between the cathode material and the electrolyte, and inhibit the dissolution of transition metal elements, thereby improving the cycle stability of the cathode material under high voltage.

[0007] In some embodiments, the matrix includes elements M, Q, and Co, wherein element M includes at least one of Na, K, or Ca, and element Q includes at least one of Al, Mg, Ti, La, Y, Zr, Fe, Mn, Ni, Nb, Mo, W, Ta, Zn, Cr, W, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, or Cu, and the molar ratio x of element M to element Co in the matrix is... M / x Co 0 < x M / x Co ≤0.015, the molar ratio x of Q to Co in the matrix Q / x Co 0 < x Q / x Co ≤0.1.

[0008] In some implementations, the second region is an amorphous structure.

[0009] In some implementations, the second region includes a B-containing oxide.

[0010] In some implementations, the surface of the first region has pits and / or crevices, and the surface of the pits and / or crevices contains the second region. Element B tends to accumulate at the defect sites on the surface of the first region, forming an amorphous coating structure, thereby repairing the defect sites on the surface of the first region, suppressing side reactions between the cathode material and the electrolyte, and thus improving the cycle stability of the cathode material under high voltage.

[0011] In some implementations, the specific surface area of ​​the cathode material is 0.1 m². 2 / g to 1.0m 2 / g. In some implementations, the Dv50 of the cathode material is from 5 μm to 25 μm.

[0012] In some implementations, the general formula for the cathode material is Li. x M y Co 1-z R z O 2±q T qM includes at least one of Na, K, or Ca; R includes at least one of Al, Mg, Ti, La, Y, Zr, Fe, Mn, Ni, Nb, Mo, W, Ta, Zn, Cr, W, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, B, or Cu; and T is a halogen, wherein 0.6 ≤ x ≤ 1.05, 0 ≤ y ≤ 0.03, and 0 <z≤0.15,0≤q≤0.2。

[0013] A second aspect of this application provides an electrochemical device comprising the cathode material of any of the foregoing embodiments. The cathode material provided by this application exhibits good cycle stability at high voltages, thereby providing the electrochemical device with high energy density and good cycle performance.

[0014] A third aspect of this application provides an electronic device that includes the electrochemical device in any of the foregoing embodiments. The electrochemical device provided by this application has high energy density and good cycle performance, thus providing the electronic device with long battery life and extended operating time. Attached Figure Description

[0015] The accompanying drawings, which are provided to further illustrate this application and form part of this application, illustrate exemplary embodiments of this application and are used to explain this application, but do not constitute an undue limitation of this application.

[0016] Figure 1 This is a scanning electron microscope image of the cathode material in Comparative Example 1 of this application;

[0017] Figure 2 This is a scanning electron microscope image of the cathode material in Comparative Example 2 of this application;

[0018] Figure 3 Energy dispersive spectroscopy (EDS) analysis of the cathode material in Comparative Example 2 of this application;

[0019] Figure 4 This is a scanning electron microscope image of the positive electrode material in Embodiment 1 of this application;

[0020] Figure 5 These are cycle performance diagrams for various embodiments of this application;

[0021] Figure 6 The diagram shows the cyclic performance of each comparative example in this application. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided with reference to the accompanying drawings and embodiments. Obviously, the described embodiments are merely some embodiments of this application, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments in this application are within the scope of protection of this application.

[0023] It should be noted that, in the specific embodiments of this application, lithium-ion batteries are used as an example of electrochemical devices to explain this application, but the electrochemical devices of this application are not limited to lithium-ion batteries.

[0024] The first aspect of this application provides a positive electrode material, comprising a substrate, a first region, and a second region, wherein the first region is located on the surface of the substrate, and the second region is located on the surface of the first region; the substrate and the first region comprise lithium cobalt oxide with a P63mc structure, the first region contains Al, and the second region contains B. The inventors of this application have discovered that the surface of the P63mc structure lithium cobalt oxide is prone to defect sites (such as pits and / or gaps), and these defect sites exhibit significant side reactions with the electrolyte, easily leading to electrolyte decomposition and dissolution of transition metal elements, deteriorating the interface between the positive and negative electrode materials, and causing rapid capacity decay of the battery. Al… 3+ radius and Co 3+ Proximity and easy uniform doping at Co sites, along with Al doping on the surface of the P63mc lithium cobalt oxide matrix, improve the performance of Li... + The transmission is not significantly affected, and due to Al 3 + Lacking electrochemical activity and not participating in reactions during charge and discharge, it plays a role in stabilizing the surface structure of the cathode material. Simultaneously, the introduction of boron (B) repairs defect sites on the cathode material surface, suppressing side reactions between the cathode material and the electrolyte, as well as the dissolution of transition metal elements. Therefore, the synergistic effect of the first and second regions can suppress interfacial side reactions and Co dissolution without deteriorating the kinetic performance of the cathode material or sacrificing specific capacity, thereby significantly improving the cycle stability of the cathode material under high voltage.

[0025] In some embodiments, the molar ratio n of Al element to Co element in the first region is... Al / n Co 0 <n Al / n Co ≤0.1. For example, n Al / n Co The range is 0.001, 0.005, 0.01, 0.02, 0.04, 0.06, 0.08, 0.1, or any two of the above values. In some embodiments, 0.001 ≤ nAl / n Co ≤0.01. By controlling the molar ratio of Al to Co in the first region within the above range, Al can be uniformly doped at Co sites, better stabilizing the surface structure of the cathode material and thus improving the cycle stability of the cathode material under high voltage.

[0026] In some embodiments, the molar ratio m of element B to element Co in the cathode material is... B / m Co 0 <m B / m Co ≤0.05. For example, m B / m Co The range is 0.002, 0.005, 0.008, 0.01, 0.02, 0.04, 0.05, or any two of the above values. In some embodiments, 0.002 ≤ m B / m Co ≤0.02. By controlling the molar ratio of B to Co in the cathode material within the above range, trace amounts of B can better repair defect sites on the surface of the cathode material, suppress side reactions between the cathode material and the electrolyte, and inhibit the dissolution of transition metal elements, thereby improving the cycle stability of the cathode material under high voltage.

[0027] In some embodiments, the matrix includes elements M, Q, and Co. Element M includes at least one of Na, K, or Ca, and element Q includes at least one of Al, Mg, Ti, La, Y, Zr, Fe, Mn, Ni, Nb, Mo, W, Ta, Zn, Cr, W, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, or Cu. The molar ratio x of element M to element Co in the matrix is... M / x Co 0 < x M / x Co ≤0.015, the molar ratio x of Q to Co in the matrix Q / x Co 0 < x Q / x Co ≤0.1.

[0028] In some embodiments, the second region is an amorphous structure.

[0029] In some embodiments, the second region includes a B-containing oxide.

[0030] In some embodiments, the surface of the first region has pits and / or crevices, and the surface of the pits and / or crevices contains the second region. Element B tends to accumulate at defect sites on the surface of the first region, forming an amorphous coating structure, thereby repairing the defect sites on the surface of the first region, suppressing side reactions between the cathode material and the electrolyte, and thus improving the cycle stability of the cathode material under high voltage.

[0031] In some embodiments, the specific surface area of ​​the cathode material is 0.1 m². 2 / g to 1.0m 2 / g. For example, the specific surface area of ​​the cathode material is 0.1m². 2 / g, 0.2m 2 / g, 0.3m 2 / g, 0.4m 2 / g, 0.5m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g, 1.0m 2 / g or a range of any two of the above values. In some embodiments, the Dv50 of the cathode material is from 5 μm to 25 μm. Exemplarily, the Dv50 of the cathode material is 5 μm, 10 μm, 15 μm, 20 μm, 25 μm or a range of any two of the above values.

[0032] In some embodiments, the general formula of the positive electrode material is Li x M y Co 1-z R z O 2±q T q M includes at least one of Na, K, or Ca; R includes at least one of Al, Mg, Ti, La, Y, Zr, Fe, Mn, Ni, Nb, Mo, W, Ta, Zn, Cr, W, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, B, or Cu; and T is a halogen, wherein 0.6 ≤ x ≤ 1.05, 0 ≤ y ≤ 0.03, and 0 <z≤0.15,0≤q≤0.2。

[0033] This application does not impose any particular restrictions on the preparation method of the cathode material, as long as it can achieve the purpose of this application. For example, the preparation method of the cathode material may include, but is not limited to, the following steps: (1) Weigh sodium cobaltate and alumina, ball mill and mix them evenly, place the ball-milled mixture in a muffle furnace for heat treatment to obtain solid powder, grind the obtained solid powder thoroughly and sieve it to obtain Al-doped sodium cobaltate; (2) Add lithium to an organic solvent, stir until completely dissolved, add Al-doped sodium cobaltate while stirring under heating conditions, and continue stirring for a period of time, filter, and place in a vacuum environment until completely dry, grind the obtained solid powder thoroughly and sieve it to obtain P63mc structure-doped lithium cobaltate; (3) Weigh P63mc structure-doped lithium cobaltate and boric acid, ball mill and mix them evenly, place the ball-milled mixture in a muffle furnace for heat treatment to obtain solid powder, grind the obtained solid powder thoroughly and sieve it to obtain the finished cathode material.

[0034] This application does not impose any particular restrictions on the preparation method of sodium cobaltate, as long as it achieves the purpose of this application. For example, sodium cobaltate can be prepared by high-temperature solid-state sintering or wet synthesis. This application does not impose any particular restrictions on the lithium compound, as long as it achieves the purpose of this application. For example, the lithium compound can be lithium chloride, lithium bromide, or lithium iodide. This application does not impose any particular restrictions on the organic solvent, as long as it achieves the purpose of this application. For example, the organic solvent can be anhydrous methanol, ethylene glycol, or cyclohexane. This application does not impose any particular restrictions on the heat treatment temperature in step (1), the heating temperature in step (2), and the heat treatment temperature in step (3), as long as it achieves the purpose of this application. For example, the heat treatment temperature in step (1) can be 800°C to 1000°C, the heating temperature in step (2) can be 50°C to 180°C, and the heat treatment temperature in step (3) can be 150°C to 250°C.

[0035] A second aspect of this application provides an electrochemical device comprising the cathode material of any of the foregoing embodiments. The cathode material provided by this application exhibits good cycle stability at high voltages, thereby providing the electrochemical device with high energy density and good cycle performance.

[0036] The electrochemical device of this application includes a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode comprises a positive current collector and a positive active material layer. This application does not impose any particular limitation on the positive current collector, as long as it achieves the purpose of this application. For example, the positive current collector may comprise aluminum foil, aluminum alloy foil, or a composite current collector. In this application, there are no particular limitations on the thickness of the positive current collector and the positive active material layer, as long as they achieve the purpose of this application. For example, the thickness of the positive current collector is 5 μm to 20 μm. The thickness of the single-sided positive active material layer is 30 μm to 120 μm. In this application, the positive active material layer may be disposed on one surface in the thickness direction of the positive current collector, or on two surfaces in the thickness direction of the positive current collector. Optionally, the positive active material layer may also include a conductive agent and a binder. This application does not impose any particular limitation on the type of binder in the positive electrode active material layer, as long as it can achieve the purpose of this application. For example, the binder may include, but is not limited to, at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polytetrafluoroethylene, or polyhexafluoropropylene. This application does not impose any particular limitation on the type of conductive agent in the positive electrode active material layer, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fiber, Ketjen black, graphene, metallic materials, or conductive polymers. The aforementioned metallic materials may include, but are not limited to, metal powder and / or metal fibers. Specifically, the metal may include, but is not limited to, at least one of copper, nickel, aluminum, or silver. The aforementioned conductive polymers may include, but are not limited to, at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene, or polypyrrole. This application does not impose any particular limitation on the mass ratio of the positive electrode active material, conductive agent, and binder in the positive electrode active material layer. Those skilled in the art can select according to actual needs, as long as the purpose of this application can be achieved.

[0037] This application does not impose any particular limitation on the negative electrode sheet, as long as it achieves the purpose of this application. For example, the negative electrode sheet includes a negative current collector and a negative active material layer. This application does not impose any particular limitation on the negative current collector, as long as it achieves the purpose of this application. For example, the negative current collector may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, or copper foam, etc. The negative active material layer of this application includes a negative active material. This application does not impose any particular limitation on the type of negative active material, as long as it achieves the purpose of this application. For example, the negative active material may include at least one of natural graphite, artificial graphite, mesophase microcarbon spheres (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composites, silicon-oxygen composites, Li-Al alloys, or lithium metal. In this application, there is no particular limitation on the thickness of the negative current collector and the negative active material layer, as long as it achieves the purpose of this application. For example, the thickness of the negative current collector is 6 μm to 10 μm, and the thickness of the negative active material layer is 30 μm to 130 μm. Optionally, the negative electrode active material layer may further include at least one of a conductive agent, a thickener, and a binder. This application does not impose any particular limitation on the types of conductive agents, thickeners, and binders in the negative electrode active material layer, as long as the purpose of this application is achieved. This application also does not impose any particular limitation on the mass ratio of the negative electrode active material, conductive agent, thickener, and binder in the negative electrode active material layer, as long as the purpose of this application is achieved.

[0038] This application does not impose any particular limitation on the diaphragm, as long as it can achieve the purpose of this application. For example, the diaphragm may include a substrate layer and a surface treatment layer. The substrate layer may be a nonwoven fabric, membrane, or composite membrane with a porous structure, and the material of the substrate layer may include, but is not limited to, at least one of polyethylene, polypropylene, polyethylene terephthalate, or polyimide. Optionally, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane may be used. Optionally, a surface treatment layer may be provided on at least one surface of the substrate layer, and the surface treatment layer may be an adhesive layer or a heat-resistant layer.

[0039] The heat-resistant layer may include, but is not limited to, inorganic particles and binders. This application does not impose any particular limitation on the inorganic particles, as long as they achieve the purpose of this application. For example, they may include, but are not limited to, at least one of alumina, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. This application does not impose any particular limitation on the binder. For example, it may include, but is not limited to, at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, acrylate polymers, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polytetrafluoroethylene, or polyhexafluoropropylene. The adhesive layer contains a binder, and the binder material may include, but is not limited to, at least one of polyamide, polyacrylonitrile, acrylate polymers, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, or vinylidene fluoride-hexafluoropropylene copolymer.

[0040] In this application, the electrochemical device further includes an electrolyte, which comprises a lithium salt and a non-aqueous solvent. The lithium salt may include at least one selected from LiPF6, LiBF4, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalato)borate (LiBOB), or lithium difluoroborate. This application does not impose any particular limitation on the concentration of the lithium salt in the electrolyte, as long as it achieves the purpose of this application. For example, the concentration of the lithium salt in the electrolyte is from 0.9 mol / L to 1.5 mol / L. This application does not impose any particular limitation on the non-aqueous solvent, as long as it achieves the purpose of this application, such as including but not limited to at least one selected from carbonate compounds, carboxylic acid ester compounds, or ether compounds. The aforementioned carbonate compounds may include, but are not limited to, at least one selected from chain carbonate compounds or cyclic carbonate compounds. The aforementioned chain carbonate compounds may include, but are not limited to, at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), or methyl ethyl carbonate (MEC). The aforementioned cyclic carbonates may include, but are not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), or butenyl carbonate (BC). The aforementioned carboxylic acid ester compounds may include, but are not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valproic acid lactone, or caprolactone. The aforementioned ether compounds may include, but are not limited to, at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran, or tetrahydrofuran.

[0041] The electrochemical device described in this application is not particularly limited and may include any device in which an electrochemical reaction occurs. In one embodiment of this application, the electrochemical device may include, but is not limited to, a lithium-ion secondary battery, a lithium polymer secondary battery, or a lithium-ion polymer secondary battery. In one embodiment, the electrode assembly structure includes a wound structure or a stacked structure.

[0042] A third aspect of this application provides an electronic device comprising the electrochemical device described in any of the foregoing embodiments. Therefore, it has a longer battery life and service life.

[0043] The electronic device described in this application is not particularly limited and can be any electronic device known in the prior art. For example, the electronic device may include, but is not limited to: laptop computers, pen input computers, mobile computers, e-book players, portable telephones, portable fax machines, portable copiers, portable printers, stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini CDs, transceivers, electronic notebooks, calculators, memory cards, portable recorders, radios, backup power supplies, motors, automobiles, motorcycles, electric bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, household large-capacity batteries, and lithium-ion capacitors.

[0044] Example

[0045] The embodiments and comparative examples provided below illustrate the implementation of this application in more detail. Various tests and evaluations were conducted according to the methods described below. Furthermore, unless otherwise specified, "parts" and "%" are quality standards.

[0046] Test methods and equipment:

[0047] Scanning electron microscopy and energy dispersive spectroscopy analysis:

[0048] The cathode material was made into a sample and tested using a scanning electron microscope (SEM) and an energy dispersive spectroscopy (EDS) instrument to observe the surface morphology and elemental distribution of the cathode material.

[0049] in, Figure 1 Here is a scanning electron microscope image of the cathode material in Comparative Example 1; Figure 2 Here is a scanning electron microscope image of the cathode material in Comparative Example 2; Figure 3 For the energy dispersive spectroscopy analysis of the cathode material in Comparative Example 2, it can be seen from the figure that Al element is uniformly doped on the surface of the lithium cobalt oxide matrix with P63mc structure. Figure 4 This is a scanning electron microscope image of the cathode material in Embodiment 1 of this application, for comparison. Figure 1 and Figure 2 , Figure 4The number of pits and gaps on the surface of the cathode material is relatively reduced.

[0050] Testing of elemental composition, content, and crystal structure of the cathode material matrix, first region, and second region:

[0051] The positive electrode sheet was transferred into the chamber of a scanning electron microscope (SEM) equipped with a focused ion beam (model: FEI Vion Plasma FIB) to prepare a sample suitable for analysis using a transmission scanning electron microscope (STEM, model: FEI Titan3 G2 60-300). The sample surface was protected with Pt and processed using a Ga ion beam, with a sample thickness not exceeding 100 nm. The sample was then cleaned using a low-voltage mode to remove any residual surface material. The sample was observed under STEM, and the crystal structure of the positive electrode matrix, the first region, and the second region was determined by electron diffraction analysis. Data was acquired using X-ray energy dispersive spectroscopy (EDS) at an appropriate magnification to obtain the elemental types and contents in the positive electrode matrix, the first region, and the second region. Data was collected from at least three different locations, and the average value was taken as the final result to obtain the molar ratio n of Al to Co in the first region. Al / n Co .

[0052] Testing of elemental content in cathode materials:

[0053] The cathode material sample was digested in aqua regia, and the contents of Li, B, and Co elements in the cathode material were determined by inductively coupled plasma optical emission spectrometry (ICP-OES). The molar ratio X of Li to Co elements in the cathode material was then calculated. Li / X Co And the molar ratio m of element B to element Co B / m Co .

[0054] Cyclic capacity retention test:

[0055] The lithium-ion coin cells of each embodiment and comparative example were subjected to charge-discharge cycles using a battery tester (Land CT2001A), and the cycle capacity retention rate was calculated.

[0056] In an environment of 25℃, the first charge and discharge were performed. The capacitor was charged to 4.6V under a constant current of 0.5C, and then charged to 50μA under a constant voltage. Then it was discharged to 3V under a constant current of 0.5C. This is one cycle. The discharge capacity of the first cycle was recorded. The above cycle was repeated, and the discharge capacity of the 80th and 120th cycles was recorded.

[0057] Capacity retention rate after 80 cycles = Discharge capacity of the 80th cycle / Discharge capacity of the first cycle × 100%.

[0058] Capacity retention rate after 120 cycles = Discharge capacity after 120 cycles / Discharge capacity after the first cycle × 100%.

[0059] Mass specific capacity = discharge capacity / mass of cathode material.

[0060] Figure 5 and Figure 6 The diagram shows the cyclic performance of various embodiments and comparative examples of this application.

[0061] Example 1

[0062] <Preparation of cathode materials>

[0063] (1) 19.98g of sodium cobaltate and 0.02g of alumina were ball-milled and mixed evenly. The ball-milled mixture was placed in a muffle furnace and heat-treated at 900℃ for 24h. The resulting solid powder was thoroughly ground and sieved to obtain doped sodium cobaltate.

[0064] (2) Dissolve 42.4 g of lithium chloride in 100 mL of anhydrous methanol, add 10.7 g of doped sodium cobaltate to the solution, react for 72 h under water bath heating at 65 °C, filter, wash three times with anhydrous methanol, and dry under vacuum at 90 °C for 8 h to obtain doped lithium cobaltate powder with P63mc structure.

[0065] (3) 19.995g of doped lithium cobalt oxide and 0.005g of boric acid were ball-milled and mixed evenly. The ball-milled mixture was placed in a muffle furnace and heat-treated at 200℃ for 8h to obtain the finished cathode material.

[0066] <Preparation of the positive electrode>

[0067] The above-mentioned positive electrode material, conductive carbon black, and binder polyvinylidene fluoride were mixed in a mass ratio of 90:5:5, and N-methylpyrrolidone was added as a solvent. The mixture was stirred evenly under vacuum to obtain a positive electrode slurry with a solid content of 70 wt%. Aluminum foil was used as the current collector, and the positive electrode slurry was coated onto the aluminum foil at a coating weight of 12.0 mg / cm². 2 After drying, cold pressing, and cutting, the positive electrode sheet is obtained.

[0068] <Preparation of Electrolyte>

[0069] In a dry argon-atmospheric glove box, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1:1 to obtain an organic solvent. Lithium salt LiPF6 was then added to the organic solvent, dissolved, and mixed thoroughly to obtain the electrolyte. The mass concentration of LiPF6 in the electrolyte was 12.5%.

[0070] <Preparation of the diaphragm>

[0071] A porous PE film with a thickness of 7μm was used.

[0072] <Preparation of Lithium-ion Button Batteries>

[0073] The positive electrode sheet is punched into a circular piece with a diameter of 1.4 cm, and then packed into the battery case in sequence with the separator and the negative lithium sheet. The electrolyte is injected, and the battery is packaged on a packaging machine to obtain a lithium-ion button battery.

[0074] Example 2

[0075] Except for the fact that the mass of sodium cobaltate is 19.99g and the mass of aluminum oxide is 0.01g, everything else is the same as in Example 1.

[0076] Example 3

[0077] Except for the fact that the mass of sodium cobaltate is 19.96g and the mass of aluminum oxide is 0.04g, everything else is the same as in Example 1.

[0078] Example 4

[0079] Except for the fact that the mass of the doped lithium cobalt oxide is 19.99g and the mass of boric acid is 0.01g, everything else is the same as in Example 1.

[0080] Example 5

[0081] Except for the fact that the mass of the doped lithium cobalt oxide is 19.98g and the mass of boric acid is 0.02g, everything else is the same as in Example 1.

[0082] Example 6

[0083] Except that the lithium compound is lithium bromide and the mass of lithium bromide is 86.9g, everything else is the same as in Example 1.

[0084] Example 7

[0085] Except that the lithium compound is lithium iodide and the mass of lithium iodide is 133.9g, everything else is the same as in Example 1.

[0086] Example 8

[0087] Except that the organic solvent is ethylene glycol and the heating conditions are 150°C oil bath heating, everything else is the same as in Example 1.

[0088] Example 9

[0089] Except for the use of cyclohexane as the organic solvent and the heating conditions of 180°C oil bath heating, everything else is the same as in Example 1.

[0090] Comparative Example 1

[0091] Except for the steps in <Preparation of Cathode Material> for preparing the cathode material, the rest is the same as in Example 1:

[0092] 42.4 g of lithium chloride was dissolved in 100 mL of anhydrous methanol. 10.7 g of sodium cobalt oxide was added to the solution, and the mixture was reacted at 65 °C in a water bath for 72 h. The mixture was then filtered, washed three times with anhydrous methanol, and dried under vacuum at 90 °C for 8 h to obtain lithium cobalt oxide powder with a P63mc structure.

[0093] Comparative Example 2

[0094] Except for the steps in <Preparation of Cathode Material> for preparing the cathode material, the rest is the same as in Example 1:

[0095] (1) 19.96g of sodium cobaltate and 0.04g of alumina were ball-milled and mixed evenly. The ball-milled mixture was placed in a muffle furnace and heat-treated at 900℃ for 24h to obtain sodium cobaltate powder.

[0096] (2) Dissolve 42.4 g of lithium chloride in 100 mL of anhydrous methanol, add 10.7 g of doped sodium cobaltate to the solution, react for 72 h under water bath heating at 65 °C, filter, wash three times with anhydrous methanol, and dry under vacuum at 90 °C for 8 h to obtain doped lithium cobaltate powder with P63mc structure.

[0097] Comparative Example 3

[0098] Except for the steps in <Preparation of Cathode Material> for preparing the cathode material, the rest is the same as in Example 1:

[0099] (1) Dissolve 42.4 g of lithium chloride in 100 mL of anhydrous methanol, add 10.7 g of sodium cobalt oxide to the solution, react for 72 h under water bath heating at 65 °C, filter, wash three times with anhydrous methanol, and dry under vacuum at 90 °C for 8 h to obtain lithium cobalt oxide powder with P63mc structure.

[0100] (2) 19.96g of lithium cobalt oxide and 0.04g of boric acid were ball-milled and mixed evenly. The ball-milled mixture was placed in a muffle furnace and heat-treated at 200℃ for 8 hours to obtain the finished cathode material.

[0101] The preparation and performance parameters of each embodiment and comparative example are shown in Table 1.

[0102] Table 1

[0103]

[0104]

[0105] Note: " / " in Table 1 indicates that the corresponding parameter or substance does not exist.

[0106] from Figure 1 As can be seen from Comparative Example 1, the surface of the P63mc structure lithium cobalt oxide without Al doping and B coating has a large number of pits and gaps, resulting in significant side reactions with the electrolyte. This leads to electrolyte decomposition and dissolution of transition metal elements, deteriorating the interface between the positive and negative electrode materials and causing a low cycle capacity retention rate of the lithium-ion battery. Figure 4 It can be seen that the surface of lithium cobalt oxide with a P63mc structure doped with Al and coated with B has a correspondingly reduced number of pits and crevices. The presence of B at the locations of these pits and crevices forms a second region with an amorphous structure, which can suppress side reactions between the cathode material and the electrolyte, resulting in a higher cycle capacity retention rate for the lithium-ion battery. Furthermore, from... Figure 5 and Figure 6 It can be seen that after 90 cycles, the specific capacity of the lithium-ion battery in Comparative Example 1 is less than 180 mAh / g, and the cycle capacity retention rate is significantly lower than that in Examples 1 to 9.

[0107] from Figure 2 It can be seen that, even within the substrate and the first region, the surface of the cathode material still contains numerous pits and gaps. Figure 5 and Figure 6 It can be seen that after 140 cycles, the specific capacity of the lithium-ion battery in Comparative Example 2 is less than 180 mAh / g, and the cycle capacity retention rate is significantly lower than that in Examples 1 to 9.

[0108] A comparison of Examples 1 to 9 with Comparative Example 3 shows that although Comparative Example 3 can maintain a high capacity retention rate, the surface of the cathode material in Comparative Example 3 needs to be coated with a large amount of boron, which reduces conductivity and is detrimental to electron transport and capacity utilization during the charging and discharging process of the cathode material. This results in significant electrochemical polarization, affecting the kinetic performance and capacity utilization of the cathode material. Figure 5 and Figure 6 It can be seen that the specific capacity of the lithium-ion battery in Comparative Example 3 is consistently lower than that of the lithium-ion batteries in Examples 1 to 9 as the number of cycle cycles increases. The presence of Al element affects the specific capacity of Li. + The transmission was not significantly affected, Al 3+ radius and Co 3+ Al is close to Co sites and can be easily and uniformly doped. Since Al has no electrochemical activity, it does not participate in the reaction during charging and discharging, which can play a role in stabilizing the structure. As a result, the cycle capacity retention rate of the corresponding cathode material is relatively high.

[0109] From Examples 1 to 9 and Figure 5As can be seen, with the increase of cycle number, the specific capacity of Examples 1 to 9 all decrease slowly, with a high cycle capacity retention rate and good cycle stability, thereby improving the cycle performance of the lithium-ion battery. Therefore, the synergistic effect of the first and second regions can suppress interfacial side reactions and Co dissolution without deteriorating the kinetic performance of the cathode material or losing specific capacity, significantly improving the cycle stability of the cathode material under high voltage, thereby improving the energy density and cycle performance of the lithium-ion battery.

[0110] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A cathode material, comprising a substrate, a first region, and a second region, wherein, The first region is located on the surface of the substrate, and the second region is located on the surface of the first region; The substrate and the first region comprise lithium cobalt oxide having a P63mc structure; The first region contains doped Al elements; the molar ratio n of Al elements to Co elements in the first region is... Al / n Co For 0.001≤n Al / n Co ≤0.01; The matrix includes elements M, Q, and Co, wherein element M includes at least one of Na, K, or Ca, and element Q includes at least one of Mg, Ti, La, Y, Zr, Fe, Mn, Ni, Nb, Mo, W, Ta, Zn, Cr, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, or Cu. The second region includes B oxides; The second region has an amorphous structure.

2. The cathode material according to claim 1, wherein, The molar ratio m of element B to element Co in the cathode material B / m Co 0 <m B / m Co ≤0.

05.

3. The cathode material according to claim 2, wherein, The molar ratio m of element B to element Co in the cathode material B / m Co 0.002≤m B / m Co ≤0.

02.

4. The cathode material according to claim 1, wherein, The molar ratio x of element M to element Co in the matrix M / x Co 0 < x M / x Co ≤0.015, the molar ratio x of Q element to Co element in the matrix. Q / x Co 0 < x Q / x Co ≤0.

1.

5. The cathode material according to claim 1, wherein, The surface of the first region has pits and / or gaps, and the surface of the pits and / or gaps has the second region.

6. The cathode material according to claim 1, wherein, The cathode material satisfies at least one of the following conditions: (1) The specific surface area of ​​the positive electrode material is 0.1 m². 2 / g to 1.0m 2 / g; (2) The Dv50 of the positive electrode material is 5 μm to 25 μm.

7. The cathode material according to claim 1, wherein, The general formula of the cathode material is Li x M y Co 1-z R z O 2±q T q M includes at least one of Na, K, or Ca; R includes at least one of Al, Mg, Ti, La, Y, Zr, Fe, Mn, Ni, Nb, Mo, W, Ta, Zn, Cr, Sn, V, Ce, Sr, Ge, Ga, Pb, Ba, B, or Cu; T is a halogen; and 0.6 ≤ x ≤ 1.05, 0 < y ≤ 0.03, 0 <z≤0.15,0≤q≤0.2。 8. An electrochemical device comprising a positive electrode, said positive electrode comprising a positive active material layer, wherein, The positive electrode active material layer comprises the positive electrode material according to any one of claims 1-7.

9. An electronic device comprising the electrochemical device of claim 8.

Citation Information

Patent Citations

  • Lithium cobalt oxide positive electrode material, preparation method, positive plate and battery

    CN114975954A

  • Positive electrode active material, lithium ion secondary battery and vehicle

    WO2022096989A1