Method for determining automatic welding heat input threshold of gas shielded flux cored wire
By acquiring test data of pipe materials and weld metal, and optimizing the heat input threshold, the impact toughness and CTOD fracture toughness of the circumferential weld and heat-affected zone in the automatic welding of X80 pipeline steel pipes with gas-shielded flux-cored wire were solved, ensuring the quality performance of the circumferential weld joint and improving the welding technology level.
Patent Information
- Application Number
- CN202210808642.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-07-11
AI Technical Summary
In the automatic welding process of gas-shielded flux-cored wire for X80 pipeline steel pipes, there are problems such as low impact toughness and unqualified CTOD fracture toughness in the circumferential weld and heat-affected zone. Furthermore, the mechanical properties of the circumferential weld joints produced by gas-shielded flux-cored wires from different manufacturers vary greatly and are sensitive to changes in circumferential weld heat input.
By acquiring test data of pipe materials and weld metal, the ranges of the first, second, and third heat input thresholds are determined. Combining standard requirements and classical models, the heat input thresholds are optimized. Using composite grooves and specific welding parameters, thermal simulation specimens are prepared, and microstructure and performance test data are obtained. The intersection of the three is then calculated to determine the heat input threshold for automatic welding of gas-shielded flux-cored wire.
It improves the impact toughness and CTOD fracture toughness of circumferential welds, ensuring that the quality and performance of circumferential welded joints meet engineering requirements, optimizes the traditional heat input threshold, and enhances the level of welding technology.
Smart Images

Figure CN117415505B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of pipeline steel pipe welding technology, and in particular to a method for determining the automatic welding heat input threshold of gas shielded flux-cored welding wire. Background Technology
[0002] Gas-shielded flux-cored wire automatic welding is one of the current field circumferential welding processes for large-diameter X80 pipeline steel pipes. This method has the characteristics of good field operability, strong field adaptability, and less susceptibility to incomplete fusion defects. It has good field adaptability for pipeline welding construction in different terrains and at joints and other locations.
[0003] However, during the circumferential welding process evaluation of the gas-shielded flux-cored welding wire for X80 pipelines, problems were found in the circumferential weld and heat-affected zone, such as low impact toughness and unqualified CTOD fracture toughness. In addition, the mechanical properties of the circumferential weld joints of gas-shielded flux-cored welding wires produced by different manufacturers also vary greatly, and they are quite sensitive to changes in the heat input of the circumferential weld.
[0004] Therefore, it is urgent to determine the heat input threshold range for on-site circumferential welding based on the gas-shielded flux-cored automatic welding process, typical X80 pipe, and gas-shielded flux-cored welding wire combination. This will guide the on-site welding construction of X80 pipe gas-shielded flux-cored automatic welding, improve the impact toughness and CTOD fracture toughness of the circumferential weld, and ensure that the quality performance of the circumferential weld joint meets the engineering requirements. Summary of the Invention
[0005] In view of the above problems, the present invention is proposed to provide a method for determining the automatic welding heat input threshold of gas-shielded flux-cored welding wire to overcome or at least partially solve the above problems.
[0006] The first aspect of this invention provides a method for determining the automatic welding heat input threshold of gas-shielded flux-cored welding wire, the method comprising:
[0007] Acquire heat-affected zone test data of the pipe, and determine the first heat input threshold range based on the heat-affected zone test data;
[0008] Obtain test data of the first weld metal, and determine the second heat input threshold range based on the test data of the first weld metal;
[0009] The test data of the second weld metal is obtained, and the third heat input threshold range is determined based on the test data of the second weld metal, wherein the second weld metal is obtained by welding the pipe under different welding heat input conditions;
[0010] The automatic welding heat input threshold of the gas-shielded flux-cored wire is determined based on the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range.
[0011] The first weld metal is a thermal simulation specimen specifically prepared for welding simulation experiments, and its preparation method is as follows:
[0012] During welding, a composite bevel is used, the preheating temperature is 80-100℃, the interpass temperature is controlled at 60-80℃, the number of welding passes is 3, and the thickness of the last pass should be greater than 7mm.
[0013] Optionally, heat-affected zone test data of the pipe is acquired, and a first heat input threshold range is determined based on the heat-affected zone test data, including:
[0014] Obtain tissue test data and performance test data of the heat-affected zone;
[0015] Based on the tissue test data and performance test data of the heat-affected zone, the range of the first heat input threshold is determined.
[0016] Optionally, the tissue test data and performance test data of the heat-affected zone are obtained, including:
[0017] Obtain microstructure test data of the heat-affected zone under different cooling rates. The microstructure test data of the heat-affected zone includes: changes in microstructure transformation temperature, phase ratio, and Vickers hardness of the heat-affected zone.
[0018] The performance test data of the heat-affected zone under different cooling rates are obtained. The performance test data of the heat-affected zone includes the changes in tensile properties, CVN, CTOD, and transition temperature of the heat-affected zone.
[0019] Optionally, the first heat input threshold range is determined based on the tissue test data and performance test data of the heat-affected zone, including:
[0020] Based on the tissue and performance test data of the heat-affected zone under different cooling rates, and in conjunction with standard requirements, the first cooling rate range was optimally selected.
[0021] The first heat input threshold range is determined based on the first cooling rate range.
[0022] Optionally, acquiring test data of the first weld metal and determining a second heat input threshold range based on the test data of the first weld metal includes:
[0023] Obtain the microstructure and performance test data of the first weld metal;
[0024] The second heat input threshold range is determined based on the microstructure and performance test data of the first weld metal.
[0025] Optionally, the microstructure test data and performance test data of the first weld metal are obtained, including:
[0026] Obtain test data on the continuous cooling structure of the first weld metal, which includes: changes in the microstructure transformation temperature, phase ratio, and Vickers hardness of the first weld metal.
[0027] Obtain test data on the continuous cooling performance of the first weld metal, which includes: tensile properties, CVN, CTOD, and changes in transformation temperature of the first weld metal.
[0028] Optionally, the second heat input threshold range is determined based on the microstructure test data and performance test data of the first weld metal, including:
[0029] Based on the test data of continuous cooling structure and continuous cooling performance of the first weld metal, and in conjunction with the standard requirements, the second cooling rate range is optimally obtained;
[0030] The second heat input threshold range is determined based on the second cooling rate range.
[0031] Optionally, test data of the second weld metal is acquired, and a third heat input threshold range is determined based on the test data of the second weld metal, including:
[0032] The microstructure test data of the second weld metal under different heat input conditions are obtained. The microstructure test data of the second weld metal under different heat input conditions include: changes in the microstructure transformation temperature, phase ratio, and Vickers hardness of the second weld metal.
[0033] The performance test data of the second weld metal under different heat input conditions are obtained. The performance test data of the second weld metal under different heat input conditions include: tensile properties, CVN, CTOD, and transformation temperature change data of the second weld metal.
[0034] The third heat input threshold range is determined based on the microstructure and performance test data of the second weld metal.
[0035] Optionally, the third heat input threshold range is determined based on the microstructure test data and performance test data of the second weld metal, including:
[0036] Based on the test data of the second weld metal under different heat input conditions and the test data of continuous cooling performance, combined with the standard requirements, the third cooling rate range was optimally obtained;
[0037] The third heat input threshold range is determined based on the third cooling rate range.
[0038] Optionally, the automatic welding heat input threshold of the gas-shielded flux-cored welding wire is determined based on the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range, including:
[0039] Find the intersection of the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range, and determine the intersection as the automatic welding heat input threshold of the gas-shielded flux-cored wire.
[0040] The method for determining the heat input threshold of gas-shielded flux-cored welding wire provided by this invention first obtains the microstructure and performance test data of the heat-affected zone of the pipe, and determines a first heat input threshold range based on the microstructure and performance test data of the heat-affected zone; then, based on thermal simulation tests, tests are conducted on the prepared first weld metal to obtain test data of the first weld metal. Finally, based on the test data of the first weld metal, a second heat input threshold range is determined.
[0041] The transformation law of the microstructure and properties of the prepared second weld metal under continuous cooling was experimentally investigated to obtain experimental data of the second weld metal. Based on the experimental data of the second weld metal, the third heat input threshold range was determined. Finally, based on the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range, the heat input threshold for automatic welding of gas-shielded flux-cored wire was determined.
[0042] This invention, through physical simulation, performance testing, and microstructure analysis, reveals the continuous cooling microstructure and property transformation (SWCCT, SHCCT) patterns of circumferential welded joints under different chemical compositions (carbon equivalent Pcm) of X80 pipes and different gas-shielded flux-cored welding wire combinations. Based on the heat input threshold determined by this pattern, the traditional heat input threshold is optimized, improving the impact toughness and CTOD fracture toughness of the circumferential weld, thereby ensuring that the quality and performance of the circumferential welded joint meet engineering requirements and demonstrating good practicality. Attached Figure Description
[0043] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0044] Figure 1 This is a flowchart of a method for determining the automatic welding heat input threshold of a gas-shielded flux-cored welding wire according to an embodiment of the present invention;
[0045] Figure 2 This is a schematic diagram showing the number and sequence of welding passes for the first weld metal in an embodiment of the present invention;
[0046] Figure 3 This is a schematic diagram showing the number and sequence of welding passes for the second weld metal in an embodiment of the present invention;
[0047] Figure 4 This is a block diagram of a device for determining the automatic welding heat input threshold of gas-shielded flux-cored welding wire according to an embodiment of the present invention. Detailed Implementation
[0048] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0049] The inventors discovered that in the circumferential welding process evaluation of X80 gas-shielded flux-cored welding wire, the circumferential weld and heat-affected zone have problems such as low impact toughness and unqualified CTOD fracture toughness. In addition, the inventors also found that the mechanical properties of the circumferential weld joints of gas-shielded flux-cored welding wires produced by different manufacturers are also quite different, and are quite sensitive to changes in circumferential welding heat input.
[0050] Further research by the inventors revealed that the weld microstructure determines the performance of the circumferential weld joint. The base material, welding materials, and welding process all significantly influence the microstructure of the weld joint. Abnormal microstructures in the weld joint (martensite, coarse bainite, coarse / chain MA, Widmanstätten structure, grain boundary precipitation, etc.), columnar grains in the weld, and excessive growth of the microstructure in the fusion zone and coarse-grained zone can all lead to performance degradation.
[0051] However, systematic research is currently lacking in the typical microstructure characteristics, grain size, inclusions, second-phase precipitation, crystal segregation, microscopic defects, and microstructure identification of pipe circumferential weld joints. This is particularly true for high-grade pipeline steels, such as X80 steel pipes, where the microstructure characteristics and identification techniques for circumferential weld joints are still incomplete. Therefore, using traditionally obtained heat input thresholds as welding parameters results in weld metals with low impact toughness and substandard CTOD fracture toughness in the circumferential weld and heat-affected zone, failing to meet the quality performance requirements of circumferential weld joints.
[0052] In response to the problems discovered in the above research, the inventors have creatively proposed a method for determining the automatic welding heat input threshold of gas-shielded flux-cored welding wire according to the present invention. The determination method of the present invention will be described in detail below.
[0053] Reference Figure 1 The flowchart illustrates a method for determining the automatic welding heat input threshold of gas-shielded flux-cored welding wire according to an embodiment of the present invention, specifically including:
[0054] Step 101: Obtain the heat-affected zone test data of the pipe and determine the first heat input threshold range based on the heat-affected zone test data.
[0055] Generally, pipes contain typical chemical components, and different types of chemical components result in different properties between pipes. The method for determining the automatic welding heat input threshold of gas-shielded flux-cored welding wire proposed in this invention is applicable to pipes composed of all types of chemical components.
[0056] Pipes of any chemical composition can be selected for welding heat-affected zone (HAZ) simulation tests to obtain HAZ test data. Based on this data, the first heat input threshold range can be determined. A preferred method is as follows:
[0057] The welding heat-affected zone (HAZ) simulation test can obtain multiple HAZ test data. Among them, the required test data are: HAZ microstructure test data and HAZ performance test data. These two test data will affect the heat input threshold range of the HAZ of the pipe. After obtaining them, the heat input threshold range of the HAZ, i.e., the first heat input threshold range, is determined based on the HAZ microstructure test data and performance test data.
[0058] To more accurately determine the range of the first heat input threshold, microstructure test data of the heat-affected zone under different cooling rates and performance test data of the heat-affected zone under different cooling rates can be obtained. In this embodiment of the invention, the microstructure test data of the heat-affected zone includes: changes in the microstructure transformation temperature, phase ratio, and Vickers hardness of the heat-affected zone; the performance test data of the heat-affected zone includes: changes in the tensile properties, CVN, CTOD, and transformation temperature of the heat-affected zone.
[0059] After obtaining microstructure and performance test data of the heat-affected zone under different cooling rates, and combining this with standard requirements, the optimal first cooling rate range is obtained. In this embodiment of the invention, the standard requirements can be any currently known test item standard requirements, without specific limitations.
[0060] Finally, the first heat input threshold range can be determined based on the first cooling rate range. A preferred method is to convert the cooling rate into a heat input value using the classic Rykalin-3D model, thus determining the first heat input threshold range based on the first cooling rate range.
[0061] Step 102: Obtain the test data of the first weld metal, and determine the second heat input threshold range based on the test data of the first weld metal. The first weld metal is a heat simulation specimen specially prepared for welding simulation test. Its preparation method is as follows: during welding, a composite groove is adopted, the preheating temperature is 80-100℃, the interpass temperature is controlled at 60-80℃, the number of welding passes is 3 layers, and the thickness of the last filler pass is greater than 7mm.
[0062] After obtaining the first heat input threshold range, the first weld metal is prepared. In this embodiment of the invention, the first weld metal is a thermal simulation specimen specifically prepared for welding simulation experiments. This thermal simulation specimen differs from traditional thermal simulation specimens in that it is prepared using the following method: during welding, a composite bevel is used, the preheating temperature is 80-100℃, the interpass temperature is controlled at 60-80℃, the number of welding passes is 3, and the thickness of the last pass is greater than 7mm. For example, refer to... Figure 2 The diagram shows the number and sequence of welding passes for the first weld metal. Figure 2 The horizontal 2 and 9 indicate that the blunt edge thickness is 2mm and the lower bevel height is 9mm, respectively. The vertical 1, 2, and 3 indicate the number of welding passes, respectively. The angle 10° is the upper bevel angle and the angle 30° is the lower bevel angle.
[0063] After the first weld metal is prepared, a simulation test is conducted to obtain the test data of the first weld metal. Then, based on the test data of the first weld metal, the range of the second heat input threshold is determined. Similar to the heat-affected zone method in step 101, a preferred method is:
[0064] The simulation test of the first weld metal can obtain multiple test data, among which the required test data are: microstructure test data and performance test data of the first weld metal. These two test data will affect the heat input threshold range of the first weld metal of the pipe. After obtaining them, the heat input threshold range of the first weld metal, i.e., the second heat input threshold range, is determined based on the microstructure test data and performance test data of the first weld metal.
[0065] To more accurately determine the range of the second heat input threshold, continuous cooling microstructure test data and continuous cooling performance test data of the first weld metal can be obtained. In this embodiment of the invention, the continuous cooling microstructure test data of the first weld metal includes: changes in the microstructure transformation temperature, phase ratio, and Vickers hardness of the first weld metal; the continuous cooling performance test data of the first weld metal includes: changes in the tensile properties, CVN, CTOD, and transformation temperature of the first weld metal.
[0066] After obtaining the test data of continuous cooling structure and continuous cooling performance of the first weld metal, and combining the aforementioned standard requirements, the second cooling rate range is optimally obtained.
[0067] Finally, the second heat input threshold range can be determined based on the second cooling rate range. A preferred method is the same as obtaining the first heat input threshold range: by using the classic Rykalin-3D model, the cooling rate is converted into a heat input value, and the second heat input threshold range can be determined based on the second cooling rate range.
[0068] Step 103: Obtain test data of the second weld metal, and determine the third heat input threshold range based on the test data of the second weld metal. The second weld metal is obtained by welding the pipe under different welding heat input conditions.
[0069] After obtaining the second heat input threshold range, the second weld metal is prepared. In this embodiment of the invention, the second weld metal is the weld metal obtained by welding the pipe under different welding heat input conditions. This weld metal can be prepared using traditional welding methods. For example, the preparation method can be: a single-sided V-groove with a groove angle of 22°, a blunt edge of 1.6 mm, and a butt joint gap of 3.0 mm. Specifically, the root weld and hot weld use BOEHLER EMK 6 welding material, with a shielding gas of 100% Ar and a welding material diameter of 2.4 mm. The filler and capping welds use AWS A5.29E91T1-K2MJH4 gas-shielded flux-cored welding wire with a wire diameter of 1.2 mm and a shielding gas of 80% Ar + 20% CO2%. Welding is performed using six heat inputs: 0.5 kJ / mm, 0.8 kJ / mm, 1.2 kJ / mm, 1.8 kJ / mm, 2.4 kJ / mm, and 3.0 kJ / mm, respectively, to obtain the second weld metal. For example, refer to... Figure 3 The diagram shows the number and sequence of welding passes for the second weld metal. Figure 3 The numbers 1-9 represent the number of weld passes. First, perform one root pass (corresponding to number 1), then one heat pass (corresponding to number 2), and finally three filler passes. Figure 3 Filler layers 1, 2, and 3 (corresponding to numbers 3, 5, and 6), and finally, a cover layer is welded. Figure 3 The middle cover layer corresponds to the number 8.
[0070] After the second weld metal is prepared, a simulation test is conducted to obtain the test data of the second weld metal. Then, based on the test data of the second weld metal, the range of the third heat input threshold is determined. Similar to the heat-affected zone in step 101 and the first weld metal in step 102, a preferred method is:
[0071] The simulation test of the second weld metal can obtain multiple test data. Among them, the test data that needs to be obtained are: the microstructure test data and the performance test data of the second weld metal. These two test data will affect the heat input threshold range of the second weld metal of the pipe. After obtaining them, the heat input threshold range of the second weld metal, that is, the third heat input threshold range, is determined based on the microstructure test data and the performance test data of the second weld metal.
[0072] To more accurately determine the range of the third heat input threshold, microstructure test data and performance test data of the second weld metal under different heat input conditions can be obtained. In this embodiment of the invention, the microstructure test data of the second weld metal under different heat input conditions includes: changes in the microstructure transformation temperature, phase ratio, and Vickers hardness of the second weld metal; the performance test data of the second weld metal under different heat input conditions includes: changes in the tensile properties, CVN, CTOD, and transformation temperature of the second weld metal.
[0073] After obtaining test data on the organization and continuous cooling performance under different heat input conditions of the second weld metal, and combining the aforementioned standard requirements, the third cooling rate range was optimally obtained.
[0074] Finally, the third heat input threshold range can be determined based on the third cooling rate range. A preferred method is the same as obtaining the first and second heat input threshold ranges: by using the classic Rykalin-3D model, the cooling rate is converted into a heat input value, and the third heat input threshold range can be determined based on the third cooling rate range.
[0075] Step 104: Determine the automatic welding heat input threshold for gas-shielded flux-cored wire based on the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range.
[0076] After obtaining the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range through steps 101 to 103 respectively, the automatic welding heat input threshold for gas-shielded flux-cored wire can be determined. A preferred method is to find the intersection of the first, second, and third heat input threshold ranges and use this intersection as the automatic welding heat input threshold for gas-shielded flux-cored wire.
[0077] It should be noted that the intersection of the first, second, and third heat input threshold ranges may be a specific value or a range, rather than a single value. However, regardless of whether it is a specific value or a range, the heat input threshold obtained by this invention for automatic welding of gas-shielded flux-cored wire is more accurate than the heat input threshold range obtained by current traditional methods. This method can provide important technical basis for determining welding process parameters for different combinations of base materials, welding materials, and welding methods, guiding welding construction in pipeline engineering, improving on-site welding technology, and has significant application value and practical significance.
[0078] Using the above method, the continuous cooling microstructure and property transformation (SWCCT, SHCCT) laws of circumferential welded joints under different chemical compositions (carbon equivalent Pcm) of X80 pipes and different gas-shielded flux-cored welding wire combinations can be obtained. Based on the heat input threshold determined by this law, the current traditional heat input threshold is optimized, improving the impact toughness and CTOD fracture toughness of the circumferential weld, thereby ensuring that the quality performance of the circumferential welded joint meets engineering requirements and has good practicality.
[0079] To better illustrate the method for determining the automatic welding heat input threshold of the gas-shielded flux-cored wire of the present invention, a specific example is given below.
[0080] A typical alloy composition X80 steel pipe with a diameter of 1219 mm and a wall thickness of 22 mm was selected. A Gleeble-3500 thermal simulation testing machine was used to conduct simulation tests on its weld heat-affected zone. The study investigated the changes in weld metal microstructure (microstructure transformation temperature, phase ratio, Vickers hardness) and properties (tensile properties, CVN, CTOD, transformation temperature) under different cooling rates. Experimental data were obtained, and based on the standard indicators of each test item, an optimal cooling rate range was determined. This optimal cooling rate range was then converted into a heat input range (i.e., the first heat input threshold range) using the classical model Rykalin-3D.
[0081] Preparation of the first weld metal: During welding, a composite groove is used, the preheating temperature is 80-100℃, the interpass temperature is controlled at 60-80℃, the number of welding passes is 3, and the thickness of the last pass should be greater than 7mm.
[0082] Simulation experiments were conducted on the prepared first weld metal to study the microstructure transformation (microstructure transformation temperature, phase ratio, Vickers hardness) and property transformation (tensile properties, CVN, CTOD, transformation temperature) of the first weld metal under different cooling rates. Based on the various test standard indicators, an optimal cooling rate range was determined. This optimal cooling rate range was then converted into a heat input range (i.e., the second heat input threshold range) using the classical model Rykalin-3D.
[0083] The second weld metal was prepared based on different welding heat inputs: the groove type was a single-sided V-groove with a groove angle of 22°, a blunt edge of 1.6 mm, and a butt joint gap of 3.0 mm. Root pass and hot pass welding used BOEHLER EMK6 welding consumables with a 100% Ar shielding gas and a welding consumable diameter of 2.4 mm. The filler and cap pass used AWS A5.29E91T1-K2MJH4 gas-shielded flux-cored welding wire with a diameter of 1.2 mm and a shielding gas of 80% Ar + 20% CO2. Welding was performed using six heat inputs: 0.5 kJ / mm, 0.8 kJ / mm, 1.2 kJ / mm, 1.8 kJ / mm, 2.4 kJ / mm, and 3.0 kJ / mm.
[0084] Microstructure analysis, tensile properties, CVN, CTOD, and transformation temperature were conducted on the second weld metal (the same tests as for the first weld metal). Based on the standard indicators of each test item, an optimal cooling rate range was determined. This optimal cooling rate range was then converted into a heat input range (i.e., the third heat input threshold range) using the classical model Rykalin-3D.
[0085] By combining the three heat input ranges determined by the above three methods, the intersection of the three heat input ranges is taken to determine the heat input threshold range corresponding to the optimal automatic welding performance of gas-shielded flux-cored wire for X80 steel pipe, which is the heat input threshold for automatic welding of gas-shielded flux-cored wire.
[0086] Finally, to verify the effectiveness of the method for determining the automatic welding heat input threshold of gas-shielded flux-cored wire, an actual welding process test was conducted on the automatic welding process of X80 steel pipe using gas-shielded flux-cored wire to verify the determined automatic welding heat input threshold. The results showed that the tensile properties, CVN, and CTOD values of the weld metal all met the relevant standard requirements.
[0087] Based on the above-described method for determining the automatic welding heat input threshold of gas-shielded flux-cored wire, this embodiment of the invention also provides a device for determining the automatic welding heat input threshold of gas-shielded flux-cored wire. (Refer to...) Figure 4 The diagram shows a block diagram of an automatic welding heat input threshold determination device for gas-shielded flux-cored welding wire according to an embodiment of the present invention.
[0088] The determining device includes:
[0089] The first threshold module 410 is used to acquire heat-affected zone test data of the pipe and determine the first heat input threshold range based on the heat-affected zone test data.
[0090] The second threshold module 420 is used to acquire test data of the first weld metal and determine the second heat input threshold range based on the test data of the first weld metal.
[0091] The third threshold module 430 is used to acquire test data of the second weld metal and determine the third heat input threshold range based on the test data of the second weld metal, wherein the second weld metal is obtained by welding the pipe under different welding heat input conditions;
[0092] The input threshold determination module 440 is used to determine the automatic welding heat input threshold of the gas shielded flux-cored welding wire based on the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range.
[0093] The first weld metal is a thermal simulation specimen specifically prepared for welding simulation experiments, and its preparation method is as follows:
[0094] During welding, a composite bevel is used, the preheating temperature is 80-100℃, the interpass temperature is controlled at 60-80℃, the number of welding passes is 3, and the thickness of the last pass should be greater than 7mm.
[0095] Optionally, the module 410 for determining the first threshold includes:
[0096] The first acquisition unit is used to acquire tissue test data and performance test data of the heat-affected zone;
[0097] A first threshold unit is determined to determine the range of the first heat input threshold based on tissue test data and performance test data of the heat-affected zone.
[0098] Optionally, the first acquisition unit is specifically used for:
[0099] Obtain microstructure test data of the heat-affected zone under different cooling rates. The microstructure test data of the heat-affected zone includes: changes in microstructure transformation temperature, phase ratio, and Vickers hardness of the heat-affected zone.
[0100] The performance test data of the heat-affected zone under different cooling rates are obtained. The performance test data of the heat-affected zone includes the changes in tensile properties, CVN, CTOD, and transition temperature of the heat-affected zone.
[0101] Optionally, the unit for determining the first threshold is specifically used for:
[0102] Based on the tissue and performance test data of the heat-affected zone under different cooling rates, and in conjunction with standard requirements, the first cooling rate range was optimally selected.
[0103] The first heat input threshold range is determined based on the first cooling rate range.
[0104] Optionally, the second threshold determination module 420 includes:
[0105] The second acquisition unit is used to acquire the microstructure test data and performance test data of the first weld metal;
[0106] A second threshold unit is determined to determine the range of the second heat input threshold based on the microstructure test data and performance test data of the first weld metal.
[0107] Optionally, the second acquisition unit is specifically used for:
[0108] Obtain test data on the continuous cooling structure of the first weld metal, which includes: changes in the microstructure transformation temperature, phase ratio, and Vickers hardness of the first weld metal.
[0109] Obtain test data on the continuous cooling performance of the first weld metal, which includes: tensile properties, CVN, CTOD, and changes in transformation temperature of the first weld metal.
[0110] Optionally, the determination of the second threshold unit is specifically used for:
[0111] Based on the test data of continuous cooling structure and continuous cooling performance of the first weld metal, and in conjunction with the standard requirements, the second cooling rate range is optimally obtained;
[0112] The second heat input threshold range is determined based on the second cooling rate range.
[0113] Optionally, the module 430 for determining the third threshold includes:
[0114] The microstructure data acquisition unit is used to acquire microstructure test data of the second weld metal under different heat input conditions. The microstructure test data of the second weld metal under different heat input conditions includes: changes in the microstructure transformation temperature, phase ratio, and Vickers hardness of the second weld metal.
[0115] The performance data acquisition unit is used to acquire performance test data of the second weld metal under different heat input conditions. The performance test data of the second weld metal under different heat input conditions includes: tensile properties, CVN, CTOD, and transformation temperature variation data of the second weld metal.
[0116] A third threshold unit is determined to determine the third heat input threshold range based on the microstructure test data and performance test data of the second weld metal.
[0117] Optionally, the method for determining the third threshold unit is specifically used for:
[0118] Based on the test data of the second weld metal under different heat input conditions and the test data of continuous cooling performance, combined with the standard requirements, the third cooling rate range was optimally obtained;
[0119] The third heat input threshold range is determined based on the third cooling rate range.
[0120] Optionally, the input threshold determination module 440 is specifically used for:
[0121] Find the intersection of the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range, and determine the intersection as the automatic welding heat input threshold of the gas-shielded flux-cored wire.
[0122] Through the above examples, the method for determining the heat input threshold of the gas-shielded flux-cored welding wire of the present invention first obtains the microstructure and performance test data of the heat-affected zone of the pipe, and determines a first heat input threshold range based on the microstructure and performance test data of the heat-affected zone; then, based on thermal simulation tests, tests are conducted on the prepared first weld metal to obtain test data of the first weld metal. Finally, based on the test data of the first weld metal, a second heat input threshold range is determined.
[0123] The transformation law of the microstructure and properties of the prepared second weld metal under continuous cooling was experimentally investigated to obtain experimental data of the second weld metal. Based on the experimental data of the second weld metal, the third heat input threshold range was determined. Finally, based on the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range, the heat input threshold for automatic welding of gas-shielded flux-cored wire was determined.
[0124] This invention, through physical simulation, performance testing, and microstructure analysis, reveals the continuous cooling microstructure and property transformation (SWCCT, SHCCT) patterns of circumferential welded joints under different chemical compositions (carbon equivalent Pcm) of X80 pipes and different gas-shielded flux-cored welding wire combinations. Based on the heat input threshold determined by this pattern, the traditional heat input threshold is optimized, improving the impact toughness and CTOD fracture toughness of the circumferential weld, thereby ensuring that the quality and performance of the circumferential welded joint meet engineering requirements and demonstrating good practicality.
[0125] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes that element.
[0126] The embodiments of the present invention have been described above with reference to the accompanying drawings. However, the present invention is not limited to the specific embodiments described above. The specific embodiments described above are merely illustrative and not restrictive. Those skilled in the art can make many other forms under the guidance of the present invention without departing from the spirit and scope of the claims. All of these forms are within the protection scope of the present invention.
Claims
1. A method for determining the automatic welding heat input threshold of gas-shielded flux-cored welding wire, characterized in that, The determination method includes: Acquire heat-affected zone test data of the pipe, and determine the first heat input threshold range based on the heat-affected zone test data; Obtain test data of the first weld metal, and determine the second heat input threshold range based on the test data of the first weld metal; The test data of the second weld metal is obtained, and the third heat input threshold range is determined based on the test data of the second weld metal, wherein the second weld metal is obtained by welding the pipe under different welding heat input conditions; The automatic welding heat input threshold of the gas-shielded flux-cored wire is determined based on the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range. The first weld metal is a thermal simulation specimen prepared for welding simulation experiments, and its preparation method is as follows: During welding, a composite bevel is used, the preheating temperature is 80-100℃, the interpass temperature is controlled at 60-80℃, the number of welding passes is 3, and the thickness of the last pass filler should be greater than 7mm. The process includes acquiring heat-affected zone (HAZ) test data for the pipe and determining a first heat input threshold range based on the HAZ test data, including: Obtain tissue test data and performance test data of the heat-affected zone; Based on the tissue and performance test data of the heat-affected zone under different cooling rates, and in conjunction with standard requirements, the first cooling rate range is obtained; The first heat input threshold range is determined based on the first cooling rate range; The process includes acquiring test data of the first weld metal and determining the second heat input threshold range based on the test data of the first weld metal, including: Obtain the microstructure and performance test data of the first weld metal; Based on the continuous cooling structure test data and continuous cooling performance test data of the first weld metal, and in conjunction with the standard requirements, the second cooling rate range is obtained; The second heat input threshold range is determined based on the second cooling rate range; The process includes acquiring test data of the second weld metal and determining the third heat input threshold range based on the test data of the second weld metal, including: Obtain microstructure test data and performance test data of the second weld metal under different heat input conditions; Based on the microstructure test data and performance test data under different heat input conditions of the second weld metal, and in conjunction with the standard requirements, the third cooling rate range is obtained; The third heat input threshold range is determined based on the third cooling rate range; The determination of the automatic welding heat input threshold for gas-shielded flux-cored welding wire based on the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range includes: Find the intersection of the first heat input threshold range, the second heat input threshold range, and the third heat input threshold range, and determine the intersection as the automatic welding heat input threshold of the gas-shielded flux-cored wire.
2. The determination method according to claim 1, characterized in that, Obtain tissue test data and performance test data of the heat-affected zone, including: Obtain microstructure test data of the heat-affected zone under different cooling rates. The microstructure test data of the heat-affected zone includes: changes in microstructure transformation temperature, phase ratio, and Vickers hardness of the heat-affected zone. The performance test data of the heat-affected zone under different cooling rates are obtained. The performance test data of the heat-affected zone includes the changes in tensile properties, CVN, CTOD, and transition temperature of the heat-affected zone.
3. The determination method according to claim 1, characterized in that, Obtain the microstructure and performance test data of the first weld metal, including: Obtain test data on the continuous cooling structure of the first weld metal, which includes: changes in the microstructure transformation temperature, phase ratio, and Vickers hardness of the first weld metal. Obtain test data on the continuous cooling performance of the first weld metal, which includes: tensile properties, CVN, CTOD, and changes in transformation temperature of the first weld metal.
4. The determination method according to claim 1, characterized in that, The microstructure test data of the second weld metal under different heat input conditions include: changes in the microstructure transformation temperature, phase ratio, and Vickers hardness of the second weld metal; The performance test data of the second weld metal under different heat input conditions include: tensile properties, CVN, CTOD, and transformation temperature variation data of the second weld metal.
Citation Information
Patent Citations
Preparation method of crack-arresting steel welded joint
CN109128447A
Low-carbon microalloyed steel high-heat-input weldability evaluation method based on flux-cored wire
CN113732551A