Low-voltage fire-resistant cable and method of manufacture

By using mica tape, glass fiber rope, and specific additives to blend with polypropylene resin in low-voltage cables, the problem of poor compatibility between polypropylene and flame retardants was solved, and the high efficiency, toughness, and oxidation resistance of the cables were improved.

CN117423494BActive Publication Date: 2026-11-24贵州安众成电线电缆有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311446740.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-02
Publication Date
2026-11-24
Estimated Expiration
2043-11-02

AI Technical Summary

Technical Problem

Existing low-voltage cable materials, such as polypropylene, have poor compatibility with flame retardants, resulting in high production costs and insufficient toughness, making it difficult to meet the high demands of the cable industry.

Method used

Mica tape is used as the insulation layer, glass fiber rope is used as the filler, and the protective sleeve is prepared by melt blending with polypropylene resin through specific additives. The additives include N,N'-dicyclohexyl terephthalamide, HPN-20E, black phosphorus and lubricant, forming a polymer compound to improve flame retardancy and toughness.

Benefits of technology

It improves the flame retardancy, toughness, and oxidation resistance of cables, reduces production costs, and has significant fire resistance and smoke suppression effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a low-voltage fire-resistant cable and its preparation method, belonging to the field of cable technology. From the inside out, it consists of a conductor, an insulation layer, a filler, and a protective sheath. The insulation layer uses mica tape, which imparts significant fire resistance to the cable. The filler is glass fiber rope, which improves the cable's flame retardancy and flexibility to a certain extent. The protective sheath is prepared by melt blending polypropylene resin, additives, nucleating agents, black phosphorus, and lubricant in a mass ratio of 100:5-15:0.1-0.2:1:0.2-0.4. The nucleating agent enhances the cable's impact resistance. Black phosphorus works synergistically with the additives to strengthen the cable's flame retardancy. The addition of additives further improves the cable's flame retardancy and impact resistance, and also imparts excellent oxidation resistance. Therefore, the resulting cable possesses stable and significant flame retardancy, toughness, oxidation resistance, and a certain degree of smoke suppression, making it of significant application value in the cable industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of cable technology, specifically relating to a low-voltage fireproof cable and its preparation method. Background Technology

[0002] Cables can be classified into high-voltage cables and low-voltage cables according to voltage. Generally, 220V and 380V are considered low-voltage, while 35kV and above are considered high-voltage, mainly used for power transmission. Low-voltage cables are widely used in nuclear power plants for power transmission, data and signal communication, and instrument control. Common cable materials include PVC (polyvinyl chloride), PE (polyethylene), PP (polypropylene), rubber, and mica tape. Among them, polypropylene has excellent mechanical strength, the highest softening temperature among thermoplastic resins, good low-temperature resistance, aging resistance, and abrasion resistance, and also has high volume resistivity and dielectric strength. It is recyclable and reusable, making it a very high-quality cable material.

[0003] When using polypropylene (PP) as a low-voltage cable material, flame-retardant modification is unavoidable. PP has an oxygen index of 18, making it highly flammable; it continues to burn after the flame is removed, releasing a petroleum fumes. A fire in this case poses a significant threat to life and property. Current research on flame-retardant modification of PP is extensive, typically involving blending PP with flame retardants and other functional agents. This method is simple, convenient, and easy to produce. However, it doesn't consider the compatibility issues between PP and these agents. PP often has poor compatibility with these modifying agents, hindering their full performance and often requiring large amounts of these agents, increasing production costs. Furthermore, while PP has a high elastic modulus, its toughness and low-temperature toughness are poor, making it prone to brittle fracture. Improving its toughness is necessary to meet the higher demands of the cable industry. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a low-voltage fireproof cable and its preparation method.

[0005] The objective of this invention can be achieved through the following technical solutions: A low-voltage fireproof cable consists of conductors, insulation layer, filler, and protective sheath arranged sequentially from the inside out.

[0006] Furthermore, the insulating layer is mica tape.

[0007] Mica tape is an excellent fire-resistant and insulating material that can maintain the normal operation of the line for a period of time at high temperatures, giving the cable significant fire resistance.

[0008] Furthermore, the filler is glass fiber rope.

[0009] Fiberglass rope itself has certain flame-retardant and fire-resistant functions. By filling the gaps in the cabling, the overall fire resistance of the cable can be further improved, while ensuring a reasonable cabling gap, so that the cable has a certain degree of flexibility.

[0010] Furthermore, the protective sleeve is prepared by the following steps: The polypropylene resin was dried in an oven for 12 hours. The dried polypropylene resin, additives, nucleating agents, black phosphorus and lubricant were stirred and mixed evenly, added to a twin-screw extruder, melt-blended, extruded and injection molded to obtain a protective sleeve.

[0011] Furthermore, the nucleating agent is obtained by mixing N,N'-dicyclohexyl terephthalamide and HPN-20E in a mass ratio of 1:1.

[0012] Furthermore, the lubricant is one of calcium stearate, zinc stearate, and oleamide.

[0013] Furthermore, the mass ratio of the polypropylene resin, additives, nucleating agent, black phosphorus, and lubricant is 100:5-15:0.1-0.2:1:0.2-0.4.

[0014] The resulting protective sleeve uses both α and β nucleating agents, which gives it better low-temperature impact resistance. In addition, black phosphorus, as a new type of two-dimensional material, not only has characteristic size effect and thermal stability, but also imparts certain flame-retardant properties to the protective sleeve. Finally, the lubricant can promote the uniform dispersion of various reagents in polypropylene and better exert their performance.

[0015] Furthermore, the additive is prepared by the following steps: S1. First, the end-double-bond polyethylene was vacuum dried at 40°C for 1 hour. Then, nitrogen gas was introduced into a three-necked flask equipped with a stirring reflux device, toluene was injected, and after stirring until fully dissolved, 3-mercaptopropanol and azobisisobutyronitrile were added. The mixture was refluxed at 85°C for 4 hours. The polymer was washed with anhydrous methanol, filtered, and vacuum dried at 40°C for 12 hours to obtain intermediate 1. The ratio of end-double-bond polyethylene, toluene, 3-mercaptopropanol, and azobisisobutyronitrile was 0.1 mol: 100 mL: 9.2 g: 0.2 g. In the presence of azobisisobutyronitrile (AIBN), the terminal unsaturated carbon-carbon double bonds of terminally double-bonded polyethylene undergo a click reaction with 3-mercaptopropanol to yield intermediate 1. The reaction process is shown below:

[0016] S2. In a three-necked flask equipped with a stirring reflux apparatus, intermediate 1, methylphosphonic dichloro, toluene, and triethylamine were mixed and stirred until homogeneous. The mixture was then slowly heated to 88°C and refluxed for 4 hours. After the reaction was complete, the triethylamine hydrochloride was removed by filtration, and some of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (using a chloroform / methanol mixture as the eluent, with a volume ratio of 3:1). The eluent was removed by rotary evaporation to obtain intermediate 2. The ratio of intermediate 1, methylphosphonic dichloro, toluene, and triethylamine was 0.1 mol: 15.2 g: 150 mL: 30 mL. Intermediate 1 undergoes an esterification reaction with methylphosphonic dichloride. By controlling the molar ratio of the two to be close to 1:1 and with a slight excess of methylphosphonic dichloride, only one -Cl group on the methylphosphonic dichloride participates in the reaction. Triethylamine removes the hydrogen chloride generated in the reaction to obtain intermediate 2. The specific reaction process is shown below:

[0017] S3. In a three-necked flask equipped with a stirrer, 1,3-bis(aminopropane)tetramethyldisiloxane, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, DCC (dicyclohexylcarbodiimide, a dehydrating agent), and toluene were mixed and stirred until homogeneous. The mixture was then reacted in a 60°C water bath for 75 min. After the reaction was completed, part of the solvent was removed by rotary evaporation, and then purified by column chromatography (using a mixed solvent of benzene and diethyl ether in a volume ratio of 3:7). The eluent was removed by rotary evaporation to obtain intermediate 3. The ratio of the amounts of 1,3-bis(aminopropane)tetramethyldisiloxane, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, DCC, and toluene was 28.5 g: 27.8 g: 20.6 g: 150 mL. The amino group of 1,3-bis(aminopropane)tetramethyldisiloxane reacts with the carboxyl group of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid via an amidation reaction. This reaction can occur under relatively mild conditions with the aid of a dehydrating agent. By controlling the molar ratio of the two to approximately 1:1 and with a slight excess of 1,3-bis(aminopropane)tetramethyldisiloxane, ensuring that only one NH₂ atom from 1,3-bis(aminopropane)tetramethyldisiloxane participates in the reaction, intermediate 3 is obtained. The specific reaction process is shown below:

[0018] S4. At room temperature and under nitrogen protection, intermediates 2, 3, tetrahydrofuran, and triethylamine were mixed and stirred thoroughly in a three-necked flask equipped with a stirrer for reflux. The reaction temperature was controlled at 75°C, and the mixture was refluxed for 6 hours. After the reaction was completed, triethylamine hydrochloride was removed by filtration, and some of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (using a mixed solvent of benzene and diethyl ether in a volume ratio of 2:5). The eluent was removed by rotary evaporation to obtain the auxiliary agent. The ratio of intermediates 2, 3, tetrahydrofuran, and triethylamine was 0.1 mol: 50.8 g: 200 mL: 50 mL. Intermediate 2 and intermediate 3 undergo nucleophilic substitution, and triethylamine removes the hydrogen chloride generated in the reaction to obtain the auxiliary agent; the specific reaction process is shown below:

[0019] The obtained additive molecules are high molecular weight compounds, mainly composed of polyethylene molecular chains. Compared with small molecular weight flame retardants, high molecular weight compounds have the advantages of being more heat-resistant and more stable. Furthermore, polyethylene molecular chains have high compatibility with polypropylene, allowing the additive to be more evenly distributed within the polypropylene, thus maximizing its performance. In addition, the high flexibility of polyethylene molecular chains, interwoven between polypropylene molecular chains, also contributes to the toughening effect of PP, improving the toughness of the protective case. Moreover, the additive molecules also contain PN flame retardant components, -Si-O-Si- segments, and hindered phenolic structures. The PN flame retardant component is an excellent halogen-free flame retardant, possessing the synergistic flame retardant effect of phosphorus and nitrogen-based flame retardants, endowing the protective case with environmentally friendly and highly efficient flame retardant properties. The -Si-O-Si- segments are good flame retardant and smoke-suppressing components, further enhancing the flame retardant performance of the additive and also providing a certain degree of smoke suppression. Finally, the hindered phenol has excellent antioxidant capabilities, giving the protective case significant antioxidant properties.

[0020] It should be added that the additives are also phosphorus-containing flame retardants, which can work synergistically with black phosphorus to jointly enhance the flame retardant performance of the protective case.

[0021] The beneficial effects of this invention are: The cable of this invention comprises a conductor, an insulation layer, a filler, and a protective sheath. The insulation layer uses mica tape, which imparts significant fire resistance to the cable. The filler, made of glass fiber rope, enhances the cable's flame retardancy and flexibility to a certain extent. The protective sheath is prepared by melt blending polypropylene resin, additives, nucleating agents, black phosphorus, and lubricants. The nucleating agent improves the cable's impact resistance. Black phosphorus works synergistically with the additives to enhance the cable's flame retardancy. The addition of additives further improves the cable's flame retardancy and impact resistance, and also imparts excellent oxidation resistance and a certain degree of smoke suppression. Furthermore, the additives have good compatibility with polypropylene, allowing their performance to be fully realized. Therefore, the resulting cable possesses stable and significant flame retardancy, toughness, oxidation resistance, and a certain degree of smoke suppression, making it of significant application value in the cable industry. Detailed Implementation

[0022] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention. Example

[0023] Preparation aids S1. First, 39g of end-double-bond polyethylene was vacuum dried at 40℃ for 1h. Then, nitrogen gas was introduced into a three-necked flask equipped with a stirring reflux device, and 100mL of toluene was injected. After stirring until fully dissolved, 9.2g of 3-mercaptopropanol and 0.2g of azobisisobutyronitrile were added, and the mixture was refluxed at 85℃ for 4h. The polymer was washed with anhydrous methanol, filtered, and vacuum dried at 40℃ for 12h to obtain intermediate 1. S2. In a three-necked flask equipped with a stirring reflux apparatus, 48.1 g of intermediate 1, 15.2 g of methylphosphonic dichloride, 150 mL of toluene, and 30 mL of triethylamine were mixed and stirred until homogeneous. The mixture was then slowly heated to 88 °C and refluxed for 4 h. After the reaction was complete, the triethylamine hydrochloride was removed by filtration, and some of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (using a chloroform / methanol mixture as the eluent, with a volume ratio of 3:1). The eluent was removed by rotary evaporation to obtain intermediate 2. S3. In a three-necked flask equipped with a stirrer, 28.5 g of 1,3-bis(aminopropane)tetramethyldisiloxane, 27.8 g of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, 20.6 g of DCC and 150 mL of toluene were mixed and stirred until homogeneous. The mixture was then placed in a water bath at 60 °C and reacted for 75 min. After the reaction was completed, part of the solvent was removed by rotary evaporation, and then purified by column chromatography (using a mixed solvent of benzene and diethyl ether in a volume ratio of 3:7 as the eluent). The eluent was removed by rotary evaporation to obtain intermediate 3. S4. At room temperature and under nitrogen protection, 57.7 g of intermediate 2, 50.8 g of intermediate 3, 200 mL of tetrahydrofuran, and 50 mL of triethylamine were mixed and stirred until homogeneous in a three-necked flask equipped with a stirrer and reflux. The reaction temperature was controlled at 75 °C, and the mixture was refluxed for 6 h. After the reaction was completed, the triethylamine hydrochloride was removed by filtration, and part of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (using a mixed solvent of benzene and diethyl ether in a volume ratio of 2:5). The eluent was removed by rotary evaporation to obtain the auxiliary agent. Example

[0024] Preparation aids S1. First, 78g of end-double-bond polyethylene was vacuum dried at 40℃ for 1h. Then, nitrogen gas was introduced into a three-necked flask equipped with a stirring reflux device, and 200mL of toluene was injected. After stirring until fully dissolved, 18.4g of 3-mercaptopropanol and 0.4g of azobisisobutyronitrile were added, and the mixture was refluxed at 85℃ for 4h. The polymer was washed with anhydrous methanol, filtered, and vacuum dried at 40℃ for 12h to obtain intermediate 1. S2. In a three-necked flask equipped with a stirring reflux apparatus, 96.2 g of intermediate 1, 30.4 g of methylphosphonic dichloride, 300 mL of toluene, and 60 mL of triethylamine were mixed and stirred until homogeneous. The mixture was then slowly heated to 88 °C and refluxed for 4 h. After the reaction was complete, the triethylamine hydrochloride was removed by filtration, and some of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (using a chloroform / methanol mixture as the eluent, with a volume ratio of 3:1). The eluent was removed by rotary evaporation to obtain intermediate 2. S3. In a three-necked flask equipped with a stirrer, 57 g of 1,3-bis(aminopropane)tetramethyldisiloxane, 55.6 g of 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, 41.2 g of DCC and 300 mL of toluene were mixed and stirred until homogeneous. The mixture was then placed in a water bath at 60 °C and reacted for 75 min. After the reaction was completed, part of the solvent was removed by rotary evaporation, and then purified by column chromatography (using a mixed solvent of benzene and diethyl ether in a volume ratio of 3:7 as the eluent). The eluent was removed by rotary evaporation to obtain intermediate 3. S4. At room temperature and under nitrogen protection, 115.4 g of intermediate 2, 101.6 g of intermediate 3, 400 mL of tetrahydrofuran, and 100 mL of triethylamine were mixed and stirred until homogeneous in a three-necked flask equipped with a stirrer and reflux. The reaction temperature was controlled at 75 °C, and the mixture was refluxed for 6 h. After the reaction was completed, the triethylamine hydrochloride was removed by filtration, and part of the solvent was removed by rotary evaporation. The mixture was then purified by column chromatography (using a mixed solvent of benzene and diethyl ether in a volume ratio of 2:5). The eluent was removed by rotary evaporation to obtain the auxiliary agent. Example

[0025] Preparation of protective sleeve materials 100g of polypropylene resin was dried in an oven for 12 hours. The dried polypropylene resin, 5g of additives, 0.05g of N,N'-dicyclohexyl terephthalamide, 0.05g of HPN-20E, 1g of black phosphorus and 0.2g of calcium stearate were stirred and mixed evenly, and then added to a twin-screw extruder for melt blending and extrusion to obtain the protective sleeve material. Example

[0026] Preparation of protective sleeve materials 100g of polypropylene resin was dried in an oven for 12 hours. The dried polypropylene resin, 10g of additives, 0.1g of N,N'-dicyclohexyl terephthalamide, 0.1g of HPN-20E, 1g of black phosphorus and 0.3g of zinc stearate were stirred and mixed evenly, and then added to a twin-screw extruder for melt blending and extrusion to obtain the protective sleeve material. Example

[0027] Preparation of protective sleeve materials 100g of polypropylene resin was dried in an oven for 12 hours. The dried polypropylene resin, 15g of additives, 0.1g of N,N'-dicyclohexyl terephthalamide, 0.1g of HPN-20E, 1g of black phosphorus and 0.4g of oleamide were stirred and mixed evenly, and then added to a twin-screw extruder for melt blending and extrusion to obtain the protective sleeve material.

[0028] Comparative Example 1 The additives in the example were replaced with an equal mass of flame retardant Doher-6000-2 produced by Dongguan Daer New Material Technology Co., Ltd., and the remaining steps were the same.

[0029] Comparative Example 2 Ordinary polypropylene is used as the protective sleeve material without adding any reagents.

[0030] The protective sleeve materials of Examples 3-5 and Comparative Examples 1-2 were made into corresponding test shapes according to different test standards, and the following performance tests were conducted: The oxidation induction time was determined using the national standard GB / T 19466.6-2009 "Differential Scanning Calorimetry for Plastics"; The impact strength at 25℃ and 0℃ was determined according to the national standard GB / T 1043.1-2008 "Determination of Impact Properties of Plastic Simply Supported Beams"; The smoke density was determined according to the national standard GB / T 8323.2-2008 "Plastic Smoke Generation - Part 2: Test Method for Determination of Smoke Density by Single Chamber Method"; The limiting oxygen index was determined according to the national standard GB / T 2406-2008 "Test Method for Burning Performance of Plastics"; The measurement results are shown in the table below: Test Project Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 Oxidation induction time / min 28 31 35 21 18 <![CDATA[Impact strength, 25℃ / kJ·m -2 > 98.4 99.5 101.4 86.4 72.7 <![CDATA[Impact strength, 0℃ / kJ·m -2 > 89.5 93.7 94.9 80.1 60.4 Smoke density 272 264 251 292 317 Limiting oxygen index / % 31 32 34 30 18 As shown in the table above, in Examples 3-5, the performance of each component improved as the amount of additives gradually increased. In addition, the amount of nucleating agent significantly improved the low-temperature toughness of the cable. Therefore, the resulting cable has stable and significant flame retardancy, toughness, oxidation resistance and a certain degree of smoke suppression, which is of great significance in the field of cables.

[0031] In the description of this specification, the references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0032] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.

Claims

1. A method for manufacturing a low-voltage fire-resistant cable, wherein the cable comprises, from the inside out, conductors, insulation layer, filler, and protective sheath, characterized in that, The protective sleeve is made by melt blending polypropylene resin, additives, nucleating agents, black phosphorus, and lubricants. The auxiliary agent is prepared through the following steps: S1. First, the end-double bond polyethylene was vacuum dried at 40°C for 1 hour. Under nitrogen conditions, toluene was injected and stirred until fully dissolved. Then, 3-mercaptopropanol and azobisisobutyronitrile were added, and the mixture was refluxed at 85°C for 4 hours. The polymer was washed with anhydrous methanol, filtered, and vacuum dried at 40°C for 12 hours to obtain intermediate 1. S2. Mix intermediate 1, methylphosphonic dichloro, toluene and triethylamine evenly, reflux at 88°C for 4 hours, filter, rotary evaporate, purify by column chromatography, and rotary evaporate again to obtain intermediate 2. S3. Mix 1,3-bis(aminopropane)tetramethyldisil ether, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, DCC and toluene until homogeneous, and react in a 60°C water bath for 75 min. Then, evaporate by rotary evaporation, purify by column chromatography, and evaporate by rotary evaporation to obtain intermediate 3. S4. At room temperature and under nitrogen protection, intermediate 2, intermediate 3, tetrahydrofuran and triethylamine were mixed and stirred evenly, and refluxed at 75°C for 6 hours. After filtration, rotary evaporation, column chromatography purification, and rotary evaporation, the auxiliary agent was obtained.

2. The method for preparing a low-voltage fire-resistant cable according to claim 1, characterized in that, In step S1, the ratio of the amounts of terminal double-bonded polyethylene, toluene, 3-mercaptopropanol, and azobisisobutyronitrile is 39g:100mL:9.2g:0.2g.

3. The method for preparing a low-voltage fire-resistant cable according to claim 1, characterized in that, In step S2, the ratio of intermediate 1, methylphosphonodichloro, toluene, and triethylamine is 0.1 mol: 15.2 g: 150 mL: 30 mL.

4. The method for preparing a low-voltage fire-resistant cable according to claim 1, characterized in that, In step S3, the ratio of 1,3-bis(aminopropane)tetramethyldisiloxane, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, DCC, and toluene is 28.5 g: 27.8 g: 20.6 g: 150 mL.

5. The method for preparing a low-voltage fire-resistant cable according to claim 1, characterized in that, In step S4, the ratio of intermediate 2, intermediate 3, tetrahydrofuran, and triethylamine is 0.1 mol: 50.8 g: 200 mL: 50 mL.

6. The method for preparing a low-voltage fire-resistant cable according to claim 1, characterized in that, The nucleating agent was obtained by mixing N,N'-dicyclohexyl terephthalamide and HPN-20E in a mass ratio of 1:

1.

7. The method for preparing a low-voltage fire-resistant cable according to claim 1, characterized in that, The lubricant is one of calcium stearate, zinc stearate, or oleamide.

8. The method for preparing a low-voltage fire-resistant cable according to claim 1, characterized in that, The mass ratio of polypropylene resin, additives, nucleating agent, black phosphorus, and lubricant is 100:5-15:0.1-0.2:1:0.2-0.

4.

9. A low-voltage fire-resistant cable, characterized in that, Prepared according to the method according to any one of claims 1-8.

Citation Information

Patent Citations

  • Flame-resistant thermoplastic elastomer resin composition and application thereof

    JP2010229390A

  • Coating material

    JP2011256236A