Transparent conductive layer and preparation method thereof, LED chip
By combining laser annealing controlled by a laser mask with BOE etching solution and RTA annealing, the problem of residual ITO material in the through-hole of the transparent conductive layer was solved, thus improving the light extraction efficiency of the LED chip.
Patent Information
- Application Number
- CN202311403993.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-27
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-10-27
AI Technical Summary
In existing technologies, etching processes cannot completely remove the ITO material inside the vias of the transparent conductive layer, resulting in low light extraction efficiency of the chip.
A laser mask is used to control laser annealing to form crystalline regions. Amorphous regions are then removed using BOE etching solution to form transparent conductive layer vias. The crystal structure is then improved by RTA annealing to prepare the transparent conductive layer.
It achieves precise removal of the through-holes in the transparent conductive layer, avoids material residue, and improves the light extraction efficiency of the LED chip.
Smart Images

Figure CN117423784B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor device technology, specifically to a transparent conductive layer and its preparation method, and an LED chip. Background Technology
[0002] A typical upright high-efficiency light-emitting diode (LED) usually consists of an epitaxial structure and a chip structure. The epitaxial structure typically includes N-type semiconductors, quantum wells, and P-type semiconductors, while the chip structure, from bottom to top, includes a current blocking layer, a transparent conductive layer, an electrode layer, and a passivation layer. However, the transparent conductive layer is usually made of ITO (indium tin oxide), which absorbs light to some extent, reducing the chip's light extraction efficiency.
[0003] Based on the transparent conductive layer made of ITO, existing technologies typically create transparent conductive layer vias on the transparent conductive layer to reduce light obstruction and improve light emission efficiency. Currently, when creating transparent conductive layer vias, an etching process is used to remove part of the material of the transparent conductive layer to form the vias. However, in the etching process, it is common for some transparent conductive layer vias to not be completely removed, leaving some ITO material inside, or even creating blind vias.
[0004] Therefore, in the existing technology, the etching process cannot completely remove some of the ITO material to form a complete transparent conductive layer via. As a result, when the chip uses a transparent conductive layer with such a via, the light extraction efficiency of the chip cannot be improved. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a transparent conductive layer and its preparation method, as well as an LED chip, to solve the problem that the etching process in the prior art cannot completely remove some of the ITO material to form a well-formed transparent conductive layer via, resulting in the chip's light extraction efficiency not being significantly improved when using a transparent conductive layer with such vias.
[0006] A first aspect of the present invention is to provide a method for preparing a transparent conductive layer, the method comprising: An LED wafer is provided, the LED wafer comprising a substrate, and an N-type semiconductor layer, a light-emitting layer, a P-type semiconductor layer and a current blocking layer sequentially stacked on the substrate; A transparent conductive material is deposited on the P-type semiconductor layer to obtain an initial transparent conductive layer covering the current blocking layer. A laser mask is provided, the laser mask including a non-transparent area and a plurality of transparent areas formed in the non-transparent area at intervals; The laser device is controlled to irradiate the laser mask. The laser passes through the light-transmitting area and performs laser annealing on at least a portion of the area on the initial transparent conductive layer that is projected onto the current blocking layer and other areas thereon, thereby forming the crystal region of the initial transparent conductive layer. The LED wafer is immersed in BOE etching solution to etch away the amorphous region of the initial transparent conductive layer, thereby forming a plurality of transparent conductive layer vias that expose the surface of the P-type semiconductor layer on the initial transparent conductive layer. The target transparent conductive layer is obtained.
[0007] According to one aspect of the above technical solution, the step of controlling a laser device to irradiate a laser towards the laser mask, the laser passing through the light-transmitting area, and performing laser annealing on at least a portion of the area of the initial transparent conductive layer that is orthogonally projected onto the current-blocking layer and other areas thereon, to form the crystalline region of the initial transparent conductive layer, specifically includes: The laser device is controlled to emit a parallel laser beam, and part of the laser beam will pass through the light-transmitting area of the laser mask to act on at least a portion of the initial transparent conductive layer. Laser irradiation is applied to the initial transparent conductive layer to achieve laser annealing of at least a portion of the initial transparent conductive layer, so as to form a crystal region under high temperature. Among them, at least a portion of the region is the region on the initial transparent conductive layer that is orthogonally projected onto the current blocking layer, and at least a portion of the region outside of that region.
[0008] According to one aspect of the above technical solution, after the step of forming a plurality of transparent conductive layer vias exposing the surface of the P-type semiconductor layer on the initial transparent conductive layer, the preparation method further includes: The LED wafer is subjected to RTA annealing.
[0009] According to one aspect of the above technical solution, when performing RTA annealing on the LED wafer, 1-5 sccm of O2 is introduced into the reaction chamber, and the annealing temperature is controlled at 500-600℃.
[0010] According to one aspect of the above technical solution, the step of performing RTA annealing on the LED wafer specifically includes: Nitrogen gas is introduced into the equipment cavity of the RTA annealing equipment to clean the equipment cavity and remove air and impurity gases; The temperature inside the control equipment cavity is raised to 500-600℃, while oxygen is introduced into the equipment cavity at 1-5 sccm. The LED wafer is placed into the equipment cavity for annealing, and the annealing time is 2-6 minutes. Nitrogen gas is introduced into the equipment cavity again, and the wafer is removed to complete the annealing process.
[0011] According to one aspect of the above technical solution, the laser mask also includes a non-transparent area connected to the transparent area, the non-transparent area being circular in shape with a diameter of 4-12μm.
[0012] According to one aspect of the above technical solution, the BOE etching solution is prepared by mixing a 49% HF aqueous solution and a 40% NH4F aqueous solution in a volume ratio of (0.5-2):(5-8), and the solution temperature is controlled at less than 10°C.
[0013] A second aspect of the present invention is to provide a transparent conductive layer, which is prepared by the preparation method described in the above technical solution, and the transparent conductive layer has a plurality of spaced transparent conductive layer vias.
[0014] According to one aspect of the above technical solution, the vias in the transparent conductive layer are located in the area outside the region corresponding to the orthographic projection of the current blocking layer on the transparent conductive layer, and the distribution density of the vias in the transparent conductive layer outside the region corresponding to the orthographic projection is 1 / 6-1 / 3.
[0015] A third aspect of the present invention is to provide an LED chip, the LED chip including the transparent conductive layer described in the above technical solution, the transparent conductive layer being disposed on the P-type semiconductor layer and covering the current blocking layer.
[0016] Compared with existing technologies, the advantages of using the transparent conductive layer and its preparation method, as well as the LED chip, as shown in this invention are as follows: In the fabrication of the transparent conductive layer, a transparent conductive material is deposited on a P-type semiconductor layer to obtain an initial transparent conductive layer that is located on the P-type semiconductor layer and covers the current blocking layer. Then, by providing a laser mask, when the laser device irradiates the initial transparent conductive layer, the laser mask selectively blocks or guides the laser, achieving laser annealing of the initial transparent conductive layer to form crystalline regions, while the unirradiated areas remain amorphous regions. Then, the layer is immersed in a BOE etching solution, which reacts with the amorphous regions of the initial transparent conductive layer to remove at least a portion of the material, forming vias in the transparent conductive layer to obtain the target transparent conductive layer. In this invention, the removal of the amorphous regions of the transparent conductive material is relatively simple and efficient, the material removal is relatively precise, and material residue is not easily left. The vias in the transparent conductive layer have a good morphology. Using this transparent conductive layer can effectively improve the light extraction efficiency of LED chips. Attached Figure Description
[0017] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1This is a schematic diagram of a method for preparing a transparent conductive layer according to an embodiment of the present invention; Figure 2 This is a schematic diagram of the structure of an LED wafer before the preparation of the transparent conductive layer in one embodiment of the present invention; Figure 3 This is a schematic diagram of the structure of a transparent conductive layer fabricated on an LED wafer in one embodiment of the present invention; Figure 4 This is a schematic diagram of the structure of the transparent conductive layer in one embodiment of the present invention; Figure 5 This is a schematic diagram of the structure of a laser mask in one embodiment of the present invention; Explanation of symbols in the attached drawings: N-type semiconductor layer 10, P-type semiconductor layer 20, current blocking layer 30, transparent conductive layer 40, transparent conductive layer via 41, laser mask 50, non-transparent area 51, and transparent area 5252. Detailed Implementation
[0018] To make the objectives, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Several embodiments of the present invention are shown in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that the disclosure of the present invention will be more thorough and complete.
[0019] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0021] A first aspect of the present invention is to provide a method for preparing a transparent conductive layer, the method comprising: An LED wafer is provided, the LED wafer comprising a substrate, and an N-type semiconductor layer, a light-emitting layer, a P-type semiconductor layer and a current blocking layer sequentially stacked on the substrate; A transparent conductive material is deposited on the P-type semiconductor layer to obtain an initial transparent conductive layer covering the current blocking layer. A laser mask is provided, the laser mask including a non-transparent area and a plurality of transparent areas formed in the non-transparent area at intervals; The laser device is controlled to irradiate the laser mask. The laser passes through the light-transmitting area and performs laser annealing on at least a portion of the area on the initial transparent conductive layer that is projected onto the current blocking layer and other areas thereon, thereby forming the crystal region of the initial transparent conductive layer. The LED wafer is immersed in BOE etching solution to etch away the amorphous region of the initial transparent conductive layer, thereby forming a plurality of transparent conductive layer vias that expose the surface of the P-type semiconductor layer on the initial transparent conductive layer. The target transparent conductive layer is obtained.
[0022] Further, the step of controlling a laser device to irradiate a laser towards the laser mask, the laser passing through the light-transmitting area, and performing laser annealing on at least a portion of the area of the initial transparent conductive layer that is orthogonally projected onto the current-blocking layer, and other areas thereon, to form the crystalline region of the initial transparent conductive layer, specifically includes: The laser device is controlled to emit a parallel laser beam, and part of the laser beam will pass through the light-transmitting area of the laser mask to act on at least a portion of the initial transparent conductive layer. Laser irradiation is applied to the initial transparent conductive layer to achieve laser annealing of at least a portion of the initial transparent conductive layer, so as to form a crystal region under high temperature. Among them, at least a portion of the region is the region on the initial transparent conductive layer that is orthogonally projected onto the current blocking layer, and at least a portion of the region outside of that region.
[0023] Furthermore, after the step of forming a plurality of transparent conductive layer vias exposing the surface of the P-type semiconductor layer on the initial transparent conductive layer, the fabrication method further includes: The LED wafer is subjected to RTA annealing.
[0024] Furthermore, during the RTA annealing process of the LED wafer, 1-5 sccm of O2 is introduced into the reaction chamber, and the annealing temperature is controlled at 500-600℃.
[0025] Furthermore, the step of performing RTA annealing on the LED wafer specifically includes: Nitrogen gas is introduced into the equipment cavity of the RTA annealing equipment to clean the equipment cavity and remove air and impurity gases; The temperature inside the control equipment cavity is raised to 500-600℃, while oxygen is introduced into the equipment cavity at 1-5 sccm. The LED wafer is placed into the equipment cavity for annealing, and the annealing time is 2-6 minutes. Nitrogen gas is introduced into the equipment cavity again, and the wafer is removed to complete the annealing process.
[0026] Furthermore, the laser mask also includes a non-transparent area connected to the transparent area, the non-transparent area being circular in shape with a diameter of 4-12 μm.
[0027] Furthermore, the BOE etching solution is prepared by mixing a 49% HF aqueous solution and a 40% NH4F aqueous solution in a volume ratio of (0.5-2):(5-8), and the solution temperature is controlled at less than 10°C.
[0028] A second aspect of the present invention is to provide a transparent conductive layer, which is prepared by the preparation method described in the above technical solution, and the transparent conductive layer has a plurality of spaced transparent conductive layer vias.
[0029] Furthermore, the vias in the transparent conductive layer are located in the region outside the area corresponding to the orthographic projection of the current blocking layer on the transparent conductive layer, and the distribution density of the vias in the transparent conductive layer outside the orthographic projection region is [value missing].
[0030] A third aspect of the present invention is to provide an LED chip, the LED chip including the transparent conductive layer described in the above technical solution, the transparent conductive layer being disposed on the P-type semiconductor layer and covering the current blocking layer.
[0031] Compared with existing technologies, the advantages of using the transparent conductive layer and its preparation method, as well as the LED chip, as shown in this invention are as follows: In the fabrication of the transparent conductive layer, a transparent conductive material is deposited on a P-type semiconductor layer to obtain an initial transparent conductive layer that is located on the P-type semiconductor layer and covers the current blocking layer. Then, by providing a laser mask, when the laser device irradiates the initial transparent conductive layer, the laser mask selectively blocks or guides the laser, achieving laser annealing of the initial transparent conductive layer to form crystalline regions, while the unirradiated areas remain amorphous regions. Then, the layer is immersed in a BOE etching solution, which reacts with the amorphous regions of the initial transparent conductive layer to remove at least a portion of the material, forming vias in the transparent conductive layer to obtain the target transparent conductive layer. In this invention, the removal of the amorphous regions of the transparent conductive material is relatively simple and efficient, the material removal is relatively precise, and material residue is not easily left. The vias in the transparent conductive layer have a good morphology. Using this transparent conductive layer can effectively improve the light extraction efficiency of LED chips.
[0032] Example 1 Please see Figures 1-5The first embodiment of the present invention provides a method for preparing a transparent conductive layer 40, the method comprising steps S1-S6: Step S1: Provide an LED wafer, the LED wafer including a substrate, and an N-type semiconductor layer 10, a light-emitting layer, a P-type semiconductor layer 20 and a current blocking layer 30 sequentially stacked on the substrate.
[0033] In this embodiment, the LED wafer is a front-mounted LED, which includes a substrate and an N-type semiconductor layer 10, a light-emitting layer, and a P-type semiconductor layer 20 sequentially stacked on the substrate.
[0034] Since this embodiment requires the fabrication of a transparent conductive layer 40 for light emission and conduction, and in the prior art the transparent conductive layer 40 is usually disposed on the P-type semiconductor layer 20 and covers the current blocking layer 30, this embodiment is no exception. Therefore, the LED wafer also includes a current blocking layer 30 disposed on the P-type semiconductor layer 20, so as to block and guide the current through the current blocking layer 30 and prevent the current from accumulating under the electrodes of the LED chip.
[0035] Step S2: A transparent conductive material is deposited on the P-type semiconductor layer 20 to obtain an initial transparent conductive layer 40 covering the current blocking layer 30.
[0036] In this embodiment, the transparent conductive material is ITO, i.e., indium tin oxide. Indium tin oxide is deposited on the P-type semiconductor layer 20. When depositing indium tin oxide, the current blocking layer 30 located on the P-type semiconductor layer 20 needs to be covered to obtain the transparent conductive layer 40 located on the P-type semiconductor layer 20 and the current blocking layer 30.
[0037] Since the transparent conductive layer 40 is a semi-finished product, the transparent conductive layer 40 deposited in the current step in this embodiment is referred to as the initial transparent conductive layer 40.
[0038] The initial transparent conductive layer 40 has a thickness of 250 Å and is made using a coating device. That is, the initial transparent conductive layer 40 is a film structure with a thickness of 250 Å and is an amorphous structure.
[0039] Step S3: Provide a laser mask 50, the laser mask 50 including a non-transparent area 51 and a plurality of transparent areas 52 formed in the non-transparent area 51 at intervals.
[0040] It should be noted that the main body of the laser mask 50 is the non-transparent area 51, through which the laser cannot pass or which has a significant weakening effect on the laser energy, while the transparent area 52 formed between the non-transparent areas 51 allows the laser to pass through and irradiate.
[0041] In this embodiment, on the laser mask 50, only a specific area within the non-transparent area 51 has multiple spaced transparent areas 52, thereby achieving precise control of the laser-acting part through the positional distribution of the multiple transparent areas 52.
[0042] Specifically, on the laser mask 50, the area corresponding to the outline of the current blocking layer 30 is the light-transmitting area 52, and outside this area, a plurality of light-transmitting areas 52 are formed in the non-light-transmitting area 51.
[0043] More specifically, the laser mask 50 is used to selectively block and guide the laser emitted by the laser device. The laser can pass through the light-transmitting area 52 to act on other components, but cannot pass through the non-light-transmitting area 51 to act on other components.
[0044] Step S4: Control the laser device to irradiate the laser towards the laser mask 50. The laser passes through the light-transmitting area 52 and performs laser annealing on at least a portion of the area on the initial transparent conductive layer 40 that is orthogonally projected onto the current blocking layer 30 and other areas thereon, forming the crystal region of the initial transparent conductive layer 40.
[0045] First, it should be noted that the laser emitted by the laser device is a pulsed laser with a power of 400W.
[0046] In this embodiment, before controlling the laser device to irradiate the laser towards the laser mask 50, the laser mask 50 should be placed between the laser head of the laser device and the initial transparent conductive layer 40, and the laser mask 50 and the initial transparent conductive layer 40 should be aligned using alignment marks. Then, the laser device is controlled to irradiate a parallel laser beam. Part of the laser beam will pass through the light-transmitting area 52 to act on at least a portion of the initial transparent conductive layer 40, while part of the laser beam will be blocked by the non-light-transmitting area 51 and will not be able to pass through the laser mask 50 and thus will not be able to act on the initial transparent conductive layer 40.
[0047] Specifically, after the laser passes through the light-transmitting area 52 of the laser mask 50, the laser will irradiate the initial transparent conductive layer 40, achieving laser annealing of at least a portion of the initial transparent conductive layer 40. Under high temperature, this portion will form a crystalline region, while the portion of the initial transparent conductive layer 40 that is not irradiated by the laser remains an amorphous region.
[0048] Step S5: Immerse the LED wafer in BOE etching solution to etch away the amorphous region of the initial transparent conductive layer 40, so as to form a plurality of transparent conductive layer vias 41 on the initial transparent conductive layer 40 that expose the surface of the P-type semiconductor layer 20.
[0049] In this embodiment, before immersing the LED wafer in the BOE etching solution, a crystalline region and an amorphous region have already been formed on the transparent conductive layer 40 according to the region division. When immersing the LED in the BOE etching solution, the BOE etching solution will only act on the amorphous region of the initial transparent conductive layer 40, thereby removing at least part of the ITO material from the initial transparent conductive layer 40. This forms a plurality of transparent conductive layer vias 41 on the initial transparent conductive layer 40, and the transparent conductive layer vias 41 can expose the surface of the P-type semiconductor layer 20, so that the light emitted from the epitaxial layer can be emitted outward through the transparent conductive layer vias 41.
[0050] Specifically, the BOE etching solution is prepared by mixing two aqueous solutions, specifically including a 49% HF aqueous solution and a 40% NH4F aqueous solution with a volume ratio of 1:6. This BOE etching solution can react violently with the ITO material, thereby etching at least a portion of the initial transparent conductive layer 40 to form a plurality of spaced transparent conductive layer vias 41.
[0051] Furthermore, the multiple transparent conductive layer vias 41 are uniformly distributed in the area outside the region corresponding to the orthographic projection of the current blocking layer 30 on the initial transparent conductive layer 40, which greatly reduces the obstruction of light, and the uniformly arranged transparent conductive layer vias 41 can effectively control the light path.
[0052] Step S6, the target transparent conductive layer 40 is obtained.
[0053] It should be noted that the target transparent conductive layer 40 is the transparent conductive layer 40 after the transparent conductive layer via 41 is formed, which is the target state of the transparent conductive layer 40.
[0054] The advantages of using the method for preparing the transparent conductive layer 40 shown in this embodiment are as follows: In the fabrication of the transparent conductive layer 40, a transparent conductive material is deposited on the P-type semiconductor layer 20 to obtain an initial transparent conductive layer 40 that is located on the P-type semiconductor layer 20 and covers the current blocking layer 30. Then, a laser mask 50 is provided. When the laser device irradiates the initial transparent conductive layer 40, the laser mask 50 selectively blocks or guides the laser, thereby achieving laser annealing of the initial transparent conductive layer 40 to form a crystalline region. The unirradiated region remains an amorphous region. Then, the initial transparent conductive layer 40 is immersed in a BOE etching solution. The BOE etching solution reacts with the amorphous region of the initial transparent conductive layer 40 to remove at least a portion of the material, forming a transparent conductive layer via 41 to obtain the target transparent conductive layer 40. In this embodiment, the removal of the amorphous region of the transparent conductive material is relatively simple and efficient, the material removal is relatively precise, and material residue is not easily left. The morphology of the transparent conductive layer via 41 is good. Using this transparent conductive layer 40 can effectively improve the light extraction efficiency of the LED chip.
[0055] Example 2 The second embodiment of the present invention also provides a method for preparing a transparent conductive layer. The preparation method shown in this embodiment is basically known from the preparation method shown in the first embodiment, except that: In this embodiment, after the step of immersing the LED wafer in BOE etching solution to form multiple spaced transparent conductive layer vias on the initial transparent conductive layer, the method further includes: The LED wafer is subjected to RTA annealing.
[0056] During the RTA annealing process of the LED wafer, 1-5 sccm of O2 is introduced into the reaction chamber, and the annealing temperature is controlled at 500-600℃.
[0057] Specifically, the RTA annealing process for LED wafers includes: Nitrogen gas is introduced into the equipment cavity of the RTA annealing equipment to clean the equipment cavity and remove air and impurity gases; The temperature inside the control equipment cavity is raised to 500-600℃, while oxygen is introduced into the equipment cavity at 1-5 sccm. The LED wafer is placed into the equipment cavity for annealing, and the annealing time is 2-6 minutes. Nitrogen gas is introduced into the equipment cavity again, and the wafer is removed to complete the annealing process.
[0058] In this embodiment, after laser annealing to form crystalline regions in at least a portion of the transparent conductive layer, and etching the amorphous regions of the transparent conductive layer using BOE etching solution, the transparent conductive layer after forming the vias is subjected to high-temperature oxygen annealing, i.e., RTA annealing. The purpose is to anneal the transparent conductive layer again using high temperature and oxygen, so that the crystalline structure within the transparent conductive layer is more complete. At the same time, the oxidizing ability of oxygen is used to make the light-absorbing ions more fully oxidized, thereby reducing the absorption of light and improving the light extraction efficiency.
[0059] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0060] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this patent should be determined by the appended claims.
Claims
1. A method for preparing a transparent conductive layer, characterized in that, The preparation method includes: An LED wafer is provided, the LED wafer comprising a substrate, and an N-type semiconductor layer, a light-emitting layer, a P-type semiconductor layer and a current blocking layer sequentially stacked on the substrate; A transparent conductive material is deposited on the P-type semiconductor layer to obtain an initial transparent conductive layer covering the current blocking layer. A laser mask is provided, the laser mask including a non-transparent area and a plurality of transparent areas formed in the non-transparent area at intervals; The laser device is controlled to irradiate the laser mask. The laser passes through the light-transmitting area and performs laser annealing on at least a portion of the area on the initial transparent conductive layer that is projected onto the current blocking layer and other areas thereon, thereby forming the crystal region of the initial transparent conductive layer. The LED wafer is immersed in BOE etching solution to etch away the amorphous region of the initial transparent conductive layer, thereby forming a plurality of transparent conductive layer vias that expose the surface of the P-type semiconductor layer on the initial transparent conductive layer. The target transparent conductive layer is obtained.
2. The method for preparing the transparent conductive layer according to claim 1, characterized in that, The step of controlling a laser device to irradiate a laser towards the laser mask, the laser passing through the light-transmitting area, and performing laser annealing on at least a portion of the initial transparent conductive layer, including the area projected onto the current-blocking layer and other areas, to form the crystalline region of the initial transparent conductive layer, specifically includes: The laser device is controlled to emit a parallel laser beam, and part of the laser beam will pass through the light-transmitting area of the laser mask to act on at least a portion of the initial transparent conductive layer. Laser irradiation is applied to the initial transparent conductive layer to achieve laser annealing of at least a portion of the initial transparent conductive layer, so as to form a crystal region under high temperature. Among them, at least a portion of the region is the region on the initial transparent conductive layer that is orthogonally projected onto the current blocking layer, and at least a portion of the region outside of that region.
3. The method for preparing the transparent conductive layer according to claim 1, characterized in that, After the step of forming a plurality of transparent conductive layer vias exposing the surface of the P-type semiconductor layer on the initial transparent conductive layer, the fabrication method further includes: The LED wafer is subjected to RTA annealing.
4. The method for preparing the transparent conductive layer according to claim 3, characterized in that, During the RTA annealing process of the LED wafer, 1-5 sccm of O2 is introduced into the reaction chamber, and the annealing temperature is controlled at 500-600℃.
5. The method for preparing the transparent conductive layer according to claim 4, characterized in that, The step of performing RTA annealing on the LED wafer specifically includes: Nitrogen gas is introduced into the equipment cavity of the RTA annealing equipment to clean the equipment cavity and remove air and impurity gases; The temperature inside the control equipment cavity is raised to 500-600℃, while oxygen is introduced into the equipment cavity at 1-5 sccm. The LED wafer is placed into the equipment cavity for annealing, and the annealing time is 2-6 minutes. Nitrogen gas is introduced into the equipment cavity again, and the wafer is removed to complete the annealing process.
6. The method for preparing a transparent conductive layer according to claim 1, characterized in that, The laser mask also includes a non-transparent area connected to the transparent area. The non-transparent area is circular in shape and has a diameter of 4-12 μm.
7. The method for preparing a transparent conductive layer according to claim 1, characterized in that, The BOE etching solution is prepared by mixing 49% HF aqueous solution and 40% NH4F aqueous solution in a volume ratio of (0.5-2):(5-8), and the solution temperature is controlled at less than 10°C.
8. A transparent conductive layer, characterized in that, The transparent conductive layer is prepared by the preparation method according to any one of claims 1-7, and the transparent conductive layer has a plurality of spaced transparent conductive layer vias.
9. The transparent conductive layer according to claim 8, characterized in that, The vias in the transparent conductive layer are located in the area outside the region corresponding to the orthographic projection of the current blocking layer on the transparent conductive layer, and the distribution density of the vias outside the region corresponding to the orthographic projection is 1 / 6-1 / 3.
10. An LED chip, characterized in that, The LED chip includes the transparent conductive layer as described in claim 8 or 9, wherein the transparent conductive layer is disposed on the P-type semiconductor layer and covers the current blocking layer.
Citation Information
Patent Citations
Wafer-level package structure of light emitting diode and manufacturing method thereof
CN102024897A
Light emitting diode having vertical electrodestructure, manufacturing method of the same andetching method of sapphire substrate