Light emitting diode epitaxial wafer and preparation method thereof, and light emitting diode

CN117423786BActive Publication Date: 2026-11-24JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311549338.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-20
Publication Date
2026-11-24
Estimated Expiration
2043-11-20

AI Technical Summary

Technical Problem

然而,Si衬底与GaN外延层薄膜之间存在较大的晶格失配及热失配,会在外延层中引入大量的位错、缺陷和应力,严重的甚至会造成外延片表面的粗化以及开裂等现象

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117423786B_ABST
    Figure CN117423786B_ABST
Patent Text Reader

Abstract

This invention discloses a light-emitting diode epitaxial wafer and its fabrication method, and the light-emitting diode itself, relating to the field of semiconductor optoelectronic devices. The light-emitting diode epitaxial wafer includes a silicon substrate and, sequentially disposed on the silicon substrate, a composite buffer layer, an intrinsic GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, a P-type GaN layer, and an ohmic contact layer. The composite buffer layer includes sequentially stacked B... a Al 1‑a N layer, Sc x B y Al 1‑x‑y N-layer and Mg-doped B b Ga 1‑b N layers; where a is 0.3–0.6, x is 0–0.25, y is 0.3–0.5, b is 0–0.3, and the Mg doping concentration is <8 × 10⁻⁶. 17 cm ‑3 By implementing this invention, the luminous efficiency of light-emitting diodes can be improved and their anti-static capability can be enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor optoelectronic devices, and more particularly to a light-emitting diode epitaxial wafer and its fabrication method, and a light-emitting diode. Background Technology

[0002] Currently, compared to traditional light sources, GaN-based light-emitting diodes (LEDs) are widely used in various fields such as white light lighting, full-color displays, indicator lights, LCD backlights, and biomedicine due to their advantages of high efficiency, low price, and long lifespan. Considering cost and technological maturity, the epitaxial growth of GaN-based LEDs is often carried out on heterogeneous substrates such as sapphire, SiC, and Si. Currently, most LED device fabrication is concentrated on sapphire or SiC substrates, but both substrates have their limitations. Sapphire substrates are difficult to use for large-size epitaxy (8-12 inches, etc.), and their poor heat dissipation and peeling difficulties limit their large-scale application in high-power LEDs. SiC substrates are expensive, which to some extent limits their large-scale application and industrialization. Si is the most mature and widely used semiconductor material in terms of fabrication technology. High-quality, low-cost, and large-size (4-12 inches) Si substrates are readily available, showing significant market potential. Furthermore, compared to the most widely used sapphire substrate, Si substrates have higher electrical and thermal conductivity and are easier to peel off, making them ideal for manufacturing high-power LED devices. However, there is a significant lattice and thermal mismatch between the Si substrate and the GaN epitaxial layer, which introduces numerous dislocations, defects, and stresses into the epitaxial layer, potentially causing surface roughening and cracking. In addition, defects in the underlying layer extend upwards into the multi-quantum-well active region, forming non-radiative recombination centers, leading to reduced luminous efficacy and decreased antistatic properties of the LED. Moreover, direct GaN growth on a Si substrate results in a reaction between Si and Ga atoms, forming "Ga remelting," which creates large voids on the epitaxial surface.

[0003] To alleviate the above phenomenon, the industry generally uses a high-low temperature AlN buffer layer in the GaN epitaxial process on Si substrates. Although this method can prevent the "remelting" phenomenon between the Si substrate and the GaN epitaxial layer, the simple AlN buffer layer cannot reduce the lattice mismatch between the Si substrate and the GaN epitaxial layer, resulting in a high density of defect dislocations in the epitaxial layer. These defects and dislocations not only affect the crystal quality of the GaN epitaxial layer, causing surface roughening and cracks in the epitaxial wafer, but also affect the luminous efficiency of the active region and reduce the antistatic capability of the LED chip after extending upwards. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide an epitaxial wafer for a light-emitting diode and a method for preparing the same, which can improve the luminous efficiency of the light-emitting diode and enhance its antistatic capability.

[0005] Another technical problem to be solved by the present invention is to provide a light-emitting diode with high luminous efficiency and high anti-static capability.

[0006] To address the aforementioned problems, this invention discloses a light-emitting diode epitaxial wafer, comprising a silicon substrate and, sequentially disposed on the silicon substrate, a composite buffer layer, an intrinsic GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, a P-type GaN layer, and an ohmic contact layer. The composite buffer layer comprises sequentially stacked B... a Al 1-a N layer, Sc x B y Al 1-x-y N-layer and Mg-doped B b Ga 1-b N layers;

[0007] Where a is 0.3–0.6, x is 0–0.25, y is 0.3–0.5, b is 0–0.3, and the doping concentration of Mg is <8 × 10⁻⁶. 17 cm -3 .

[0008] As an improvement to the above technical solution, along the epitaxial growth direction, the B a Al 1-a The proportion of component B in layer N gradually increases.

[0009] As an improvement to the above technical solution, along the epitaxial growth direction, the Sc x B y Al 1-x-y The proportion of Sc component in the N layer gradually increases.

[0010] As an improvement to the above technical solution, the Mg doped with B b Ga 1-b In the N-layer, the Mg doping concentration is 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 .

[0011] As an improvement to the above technical solution, the B a Al 1-a The thickness of the N layer is 30nm to 60nm, and the Sc x B y Al 1-x-y The thickness of the N layer is 20 nm to 30 nm, and the Mg-doped B b Ga1-b The thickness of the N layer is 10nm to 20nm.

[0012] As an improvement to the above technical solution, the composite buffer layer further includes Sc α B β Al 1-α-β N layers, the Sc α B β Al 1-α-β Layer N is located in the Sc x B y Al 1-x-y Above layer N, where α is 0.25 and β is 0.3–0.5, the Sc α B β Al 1-α-β The thickness of the N layer is 20nm to 30nm.

[0013] Accordingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes:

[0014] A silicon substrate is provided, on which a composite buffer layer, an intrinsic GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, a P-type GaN layer, and an ohmic contact layer are sequentially grown, wherein the composite buffer layer comprises sequentially stacked B... a Al 1-a N layer, Sc x B y Al 1-x-y N-layer and Mg-doped B b Ga 1-b N layers;

[0015] Where a is 0.3–0.6, x is 0–0.25, y is 0.3–0.5, b is 0–0.3, and the doping concentration of Mg is <8 × 10⁻⁶. 17 cm -3 .

[0016] As an improvement to the above technical solution, the B a Al 1-a The growth temperature of the N layer is 800℃~850℃, and the growth pressure is 100 torr~150 torr.

[0017] The Sc x B y Al 1-x-y The growth temperature of the N layer is 820℃~870℃, and the growth pressure is 100 torr~150 torr;

[0018] The Mg-doped B b Ga 1-bThe growth temperature of the N layer is 850℃~900℃, and the growth pressure is 100 torr~150 torr.

[0019] As an improvement to the above technical solution, the composite buffer layer further includes Sc α B β Al 1-α-β N layers, the Sc α B β Al 1-α-β Layer N is located in the Sc x B y Al 1-x-y Above layer N, the Sc α B β Al 1-α-β The growth temperature of the N layer is 820℃~870℃, and the growth pressure is 100 torr~150 torr.

[0020] Accordingly, the present invention also discloses a light-emitting diode, which includes the above-mentioned light-emitting diode epitaxial wafer.

[0021] Implementing this invention has the following beneficial effects:

[0022] 1. In the epitaxial wafer of the light-emitting diode of the present invention, the composite buffer layer comprises B layers stacked sequentially. a Al 1-a N layer, Sc x B y Al 1-x-y N-layer and Mg-doped B b Ga 1-b N-layer. First, the introduction of boron atoms in the composite buffer layer can reduce the lattice mismatch with the silicon substrate, achieving a higher potential barrier to block and fill defects in the silicon substrate. Secondly, it can replace some al atoms, improving the bonding between atomic layers within the composite buffer layer, making it denser, preventing the "Ga remelting" phenomenon in the silicon substrate, improving surface flatness, and enhancing the luminous efficiency and antistatic properties of the epitaxial wafer. Secondly, Sc... x B y Al 1-x-y Introducing Sc components into the N layer further reduces defect and dislocation density. Furthermore, Sc atoms are comparable to Ga atoms, which can reduce lattice mismatch with GaN materials and improve lattice quality. Finally, Mg is doped with B. b Ga 1-b Introducing Mg components into the N layer can provide nuclei for the intrinsic GaN layer and promote the three-dimensional growth of the intrinsic GaN layer.

[0023] 2. In the epitaxial wafer of the light-emitting diode of the present invention, B a Al 1-a The proportion of component B in layer N gradually increases along the epitaxial growth direction, further reducing the proportion of B.a Al 1-a The lattice mismatch between the N-layer and the silicon substrate improves lattice quality and increases the luminous efficiency of the diode.

[0024] 3. In the epitaxial wafer of the light-emitting diode of the present invention, Sc x B y Al 1-x-y The proportion of Sc component in the N layer gradually increases along the epitaxial growth direction, further reducing B. a Al 1-a N-layer and Mg-doped B b Ga 1-b Lattice mismatch in the N-layer.

[0025] 4. In the epitaxial wafer of the light-emitting diode of the present invention, the composite buffer layer further includes Sc. α B β Al 1-α-β N layers, Sc α B β Al 1-α-β N layer is located at Sc x B y Al 1-x-y Above layer N, where α is constant at 0.25, Sc is reduced. x B y Al 1-x-y N-layer and Mg-doped B b Ga 1-b Lattice mismatch in the N-layer reduces defect density. Attached Figure Description

[0026] Figure 1 This is a schematic diagram of the structure of a light-emitting diode epitaxial wafer in one embodiment of the present invention;

[0027] Figure 2 This is a schematic diagram of the composite buffer layer in one embodiment of the present invention;

[0028] Figure 3 This is a schematic diagram of the composite buffer layer in another embodiment of the present invention;

[0029] Figure 4 This is a flowchart of a method for preparing an epitaxial wafer for a light-emitting diode according to an embodiment of the present invention. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.

[0031] refer to Figures 1-2The present invention discloses a light-emitting diode epitaxial wafer, comprising a silicon substrate 1 and a composite buffer layer 2, an intrinsic GaN layer 3, an N-type GaN layer 4, a stress relief layer 5, a multiple quantum well layer 6, an electron blocking layer 7, a P-type GaN layer 8, and an ohmic contact layer 9 sequentially disposed on the silicon substrate 1.

[0032] Among them, the composite buffer layer 2 includes B layers stacked sequentially. a Al 1-a N layer 21, Sc x B y Al 1-x-y N-layer 22 and Mg-doped B b Ga 1-b N layer 23. First, the introduction of B atoms in the composite buffer layer 2 can, on the one hand, reduce the lattice mismatch with the silicon substrate 1, achieve a higher potential barrier, and block and fill the defects extending from the silicon substrate 1; on the other hand, it can replace some Al atoms, improve the bonding between atomic layers within the composite buffer layer 2, making the composite buffer layer 2 denser, preventing the "Ga remelting" phenomenon of the silicon substrate 1, improving surface flatness, and improving the luminous efficiency and antistatic ability of the epitaxial wafer; secondly, Sc x B y Al 1-x-y The introduction of Sc components into the N-layer 22 further reduces defect and dislocation density. Furthermore, the Sc atoms are comparable to Ga atoms, which can reduce lattice mismatch with GaN materials and improve lattice quality. Finally, Mg is doped with B. b Ga 1-b Introducing Mg components into the N-layer 23 provides nuclei for the intrinsic GaN layer 3, promoting its three-dimensional growth. In summary, the composite buffer layer 2 of this invention achieves the blocking, filling, and annihilation of crystal defects, improving the surface flatness of the epitaxial wafer and enhancing the luminous efficacy and antistatic capability of the diode.

[0033] Among them, B a Al 1-a In layer N21, a is 0.3–0.6, and the proportion of B component within this range can achieve a high potential barrier without causing a decrease in lattice quality. For example, a can be 0.35, 0.4, 0.45, 0.5, or 0.55, but is not limited thereto. Preferably, in one embodiment of the invention, along the epitaxial growth direction, B... a Al 1-a In layer N, the proportion of component B gradually increases, further reducing the proportion of B. a Al 1-a The lattice mismatch between the N-layer 21 and the silicon substrate 1 improves the lattice quality and enhances the luminous efficiency of the diode.

[0034] Among them, B a Al 1-aThe thickness of layer N21 is 25nm to 65nm. Within this thickness range, good surface flatness can be achieved. Preferably, B a Al 1-a The thickness of the N layer 21 is 30nm to 60nm, with examples of 40nm, 45nm, 50nm or 55nm, but not limited to these.

[0035] Among them, Sc x B y Al 1-x-y In layer N22, x is 0–0.25 and y is 0.3–0.5. The proportions of Sc and B components within this range can achieve high lattice quality and reduce defect and dislocation density. For example, x can be 0.12, 0.15, 0.18, 0.2, or 0.22, and y can be 0.35, 0.4, or 0.45, but are not limited thereto. Preferably, in one embodiment of the invention, along the epitaxial growth direction, Sc... x B y Al 1-x-y In layer N22, the proportion of Sc component gradually increases, further reducing B. a Al 1-a N-layer 21 and Mg-doped B b Ga 1- b Lattice mismatch in N-layer 23.

[0036] Among them, Sc x B y Al 1-x-y The thickness of the N layer 22 is 15nm to 35nm, preferably 20nm to 30nm, and exemplary are 22nm, 25nm or 28nm, but not limited thereto.

[0037] Among them, Mg doped with B b Ga 1-b In the N-layer 23, the b content is 0–0.3%, indicating a relatively small proportion of boron, which can reduce lattice mismatch with the intrinsic GaN layer 3. Examples of b values ​​are 0.1, 0.15, 0.2, or 0.25, but these are not limited to. Mg doped with boron... b Ga 1-b The Mg doping concentration in layer 23 is < 8 × 10⁻⁶. 17 cm -3 To avoid a decrease in lattice quality, the preferred doping concentration of Mg is 5 × 10⁻⁶. 16 cm -3 ~5×10 17 cm -3 A further preferred value is 1×10 17 cm -3 ~5×10 17 cm -3 An example is 2×1017 cm -3 3×10 17 cm -3 Or 4×10 17 cm -3 However, it is not limited to this.

[0038] Among them, Mg doped with B b Ga 1-b The thickness of the N layer 23 is 5nm to 25nm, preferably 10nm to 20nm, and exemplary are 12nm, 15nm or 18nm, but not limited thereto.

[0039] Preferably, in one embodiment of the present invention, reference is made to... Figure 3 The composite buffer layer 2 also includes Sc α B β Al 1-α-β Nth floor 24, Sc α B β Al 1-α-β N layer 24 is located in Sc x B y Al 1-x-y Above layer N (23), where α is constant at 0.25, and Sc is reduced. x B y Al 1-x-y N-layer 22 and Mg-doped B b Ga 1-b The lattice mismatch of N-layer 23 reduces the defect density.

[0040] Specifically, β is 0.3 to 0.5, with examples of 0.35, 0.4, or 0.45, but is not limited thereto. α B β Al 1-α-β The thickness of the N layer 24 is 20nm to 30nm, with 22nm, 25nm or 28nm being exemplary, but not limited to these.

[0041] The thickness of the intrinsic GaN layer 3 is 2.6 μm to 4 μm, with exemplary thicknesses of 2.8 μm, 3 μm, 3.2 μm, 3.4 μm, 3.6 μm or 3.8 μm, but not limited thereto.

[0042] The N-type GaN layer 4 is doped with Si, but is not limited to Si. The doping concentration of the N-type GaN layer 4 is 3.5 × 10⁻⁶. 18 cm -3 ~1.5×10 19 cm -3 The thickness of the N-type GaN layer 4 is 1.3 μm to 2.5 μm, with exemplary thicknesses of 1.4 μm, 1.6 μm, 1.8 μm or 2 μm, but not limited thereto.

[0043] The stress relief layer 5 has a periodic structure with 4 to 8 periods. Each period consists of sequentially stacked InGaN and Si-doped GaN layers. The Si-doped GaN has a doping concentration of 3.2 × 10⁻⁶. 17 cm -3 ~6.5×10 17 cm -3 The thickness of a single InGaN layer is 3nm to 6nm, and the thickness of a single Si-doped GaN layer is 6nm to 10nm.

[0044] Among them, the multi-quantum well layer 6 consists of alternating stacked InGaN quantum well layers and GaN quantum barrier layers, with a period number of 6 to 12. The In composition in the InGaN quantum well layer is 0.25 to 0.36, the thickness of a single InGaN quantum well layer is 2 nm to 5 nm, and the thickness of a single GaN quantum barrier layer is 8 nm to 20 nm.

[0045] The electron blocking layer 7 is an AlGaN layer, but is not limited to it. The thickness of the electron blocking layer 7 is 20 nm to 110 nm, and the proportion of Al component is 0.45 to 0.65.

[0046] The p-type GaN layer 8 is doped with Mg, but is not limited to this. The Mg doping concentration in the p-type GaN layer 8 is 6.5 × 10⁸. 18 cm -3 ~2.5×10 19 cm -3 The thickness of the p-type GaN layer 8 is 50nm to 200nm.

[0047] Among them, the ohmic contact layer 9 is a P-type InGaN layer, and the P-type dopant is Mg, but not limited to this. The Mg doping concentration is 1.5 × 10⁻⁶. 19 cm -3 ~3.5×10 19 cm -3 The doping concentration of the In component is 1.1 × 10⁻⁶. 2 cm -3 ~8×10 2 cm -3 The thickness of the ohmic contact layer 9 is 5nm to 20nm.

[0048] Accordingly, refer to Figure 4 The present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes the following steps:

[0049] S101: Provides a silicon substrate;

[0050] S102: Growing a composite buffer layer on a silicon substrate;

[0051] Specifically, in one embodiment of the present invention, S103 includes:

[0052] (I) Growth of B on a silicon substrate a Al 1-a N layers;

[0053] Specifically, growing B in MOCVD a Al 1-a The N layer is grown at a temperature of 800℃~850℃ and a growth pressure of 100 torr~150 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 is used as the carrier gas, TEB is introduced as the B source, and TMAl is introduced as the Al source.

[0054] (II) In B a Al 1-a Sc grows on layer N x B y Al 1-x-y N layers;

[0055] Specifically, growing Sc in MOCVD x B y Al 1-x-y The N layer is grown at a temperature of 820℃~870℃ and a growth pressure of 100 torr~150 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 is introduced as the carrier gas, TEB is introduced as the B source, TMAl is introduced as the Al source, and Sc(TMHD)3 is introduced as the Sc source.

[0056] (III) In Sc x B y Al 1-x-y Sc grows on layer N α B β Al 1-α-β N layers;

[0057] Specifically, growing Sc in MOCVD α B β Al 1-α-β The N layer is grown at a temperature of 820℃~870℃ and a growth pressure of 100 torr~150 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source; N2 is used as the carrier gas, TEB is introduced as the B source, TMAl is introduced as the Al source, and Sc(TMHD)3 is introduced as the Sc source.

[0058] (Ⅳ) In Sc α B β Al 1-α-β Mg-doped B grows on N layer b Ga 1-b N layers;

[0059] Specifically, Mg-doped B is grown in MOCVD. b Ga 1-b The N-layer was grown at a temperature of 850℃ to 900℃ and a pressure of 100 torr to 150 torr. During growth, NH3 was introduced as the N source, TEB as the B source, TMGa as the Ga source, and CP2Mg as the Mg source in the MOCVD reaction chamber. A mixture of N2 and H2 was used as the carrier gas, with a volume ratio of N2 to H2 of 1:1 to 1:3.

[0060] S103: Intrinsic GaN layer is grown on the composite buffer layer;

[0061] Specifically, intrinsic GaN layers were grown in MOCVD at a temperature of 1100℃ to 1150℃ and a pressure of 200 torr to 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source; H2 and N2 were used as carrier gases, and TMGa was introduced as the Ga source.

[0062] S104: An N-type GaN layer is grown on an intrinsic GaN layer;

[0063] Specifically, an N-type GaN layer is grown in MOCVD at a temperature of 1150℃ to 1200℃ and a pressure of 100 torr to 200 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, and SiH4 is introduced as the N-type doping source; H2 and N2 are used as carrier gases, and TMGa is introduced as the Ga source.

[0064] S105: A stress-relieving layer is grown on an N-type GaN layer;

[0065] Specifically, InGaN and Si-doped GaN layers are periodically grown in MOCVD to form stress-relieving layers. The InGaN layer is grown at a temperature of 750℃–850℃ and a growth pressure of 100 torr–200 torr. During growth, NH3 is introduced as the N source, N2 as the carrier gas, TEGa as the Ga source, and TMI as the In source in the MOCVD reaction chamber. The Si-doped GaN layer is grown at a temperature of 850℃–880℃ and a growth pressure of 100 torr–200 torr. During growth, NH3 is introduced as the N source, SiH4 as the Si source, N2 as the carrier gas, and TEGa as the Ga source in the MOCVD reaction chamber.

[0066] S106: A multi-quantum well layer is grown on the stress-relief layer;

[0067] Specifically, InGaN quantum well layers and GaN quantum barrier layers are periodically grown in MOCVD to form multiple quantum well layers. The InGaN quantum well layer is grown at a temperature of 710℃–750℃ and a growth pressure of 100 torr–150 torr. During growth, NH3 is introduced as the N source, N2 as the carrier gas, TEGa as the Ga source, and TMI as the In source in the MOCVD reaction chamber. The GaN quantum barrier layer is grown at a temperature of 850℃–900℃ and a growth pressure of 100 torr–200 torr. During growth, NH3 is introduced as the N source, H2 and N2 as the carrier gases, and TEGa as the Ga source in the MOCVD reaction chamber.

[0068] S107: An electron blocking layer is grown on a multi-quantum-well layer;

[0069] Specifically, an AlGaN layer is grown in MOCVD as an electron blocking layer. The growth temperature is 900℃~980℃, and the growth pressure is 150 torr~200 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMAl as the Al source, and TMGa as the Ga source.

[0070] S108: A P-type GaN layer is grown on an electron blocking layer;

[0071] Specifically, a P-type GaN layer is grown in MOCVD at a temperature of 920℃ to 1000℃ and a pressure of 300 torr to 500 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, and CP2Mg is introduced as the P-type doping source; H2 and N2 are used as carrier gases, and TMGa is introduced as the Ga source.

[0072] S109: An ohmic contact layer is grown on a p-type GaN layer;

[0073] Specifically, an ohmic contact layer is grown in MOCVD at a temperature of 850℃ to 950℃ and a pressure of 100 torr to 200 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as an N source, CP2Mg as a P-type dopant source, TMGa as a Ga source, and TMIn as an In source, with H2 and N2 as carrier gases.

[0074] The present invention will be further described below with reference to specific embodiments:

[0075] Example 1

[0076] This embodiment provides a light-emitting diode epitaxial wafer, referenced... Figures 1-2 , Figure 4It includes a silicon substrate 1 and a composite buffer layer 2, an intrinsic GaN layer 3, an N-type GaN layer 4, a stress relief layer 5, a multiple quantum well layer 6, an electron blocking layer 7, a P-type GaN layer 8, and an ohmic contact layer 9 sequentially disposed on the silicon substrate 1.

[0077] Among them, the composite buffer layer 2 includes B layers stacked sequentially. a Al 1-a N layer 21, Sc x B y Al 1-x-y N-layer 22 and Mg-doped B b Ga 1-b Layer N is 23, where a is 0.45, x is 0.15, y is 0.4, b is 0.15, and Mg is doped with B. b Ga 1-b The Mg doping concentration in layer 23 is 5 × 10⁻⁶. 16 cm -3 B a Al 1-a The thickness of layer N21 is 65nm, Sc x B y Al 1-x-y The thickness of the N-layer 22 is 35 nm, and it is Mg-doped with B. b Ga 1-b The thickness of layer N23 is 25nm.

[0078] The intrinsic GaN layer 3 has a thickness of 2.6 μm. The N-type GaN layer 4 has a thickness of 1.6 μm and is doped with Si at a doping concentration of 1 × 10⁻⁶. 19 cm -3 .

[0079] The stress relief layer 5 has a periodic structure with 6 periods, each period consisting of sequentially stacked InGaN and Si-doped GaN layers. The Si-doped GaN layer has a doping concentration of 4.5 × 10⁻⁶. 17 cm -3 The thickness of a single InGaN layer is 4 nm, and the thickness of a single Si-doped GaN layer is 8 nm.

[0080] Among them, the multi-quantum well layer 6 is a periodic structure with 10 periods. Each period consists of InGaN quantum well layers and GaN quantum barrier layers stacked sequentially. The thickness of a single InGaN quantum well layer is 3 nm, and the thickness of a single GaN quantum barrier layer is 10 nm.

[0081] Among them, electron blocking layer 7 is an AlGaN layer with a thickness of 60 nm and an Al composition of 0.55%. The p-type GaN layer 8 is doped with Mg at a doping concentration of 8 × 10⁻⁶. 18 cm -3The thickness of the p-type GaN layer 8 is 85 nm. The ohmic contact layer 9 is a p-type InGaN layer, with Mg as the p-type dopant and a Mg doping concentration of 2 × 10⁻⁶. 19 cm -3 The doping concentration of the In component is 5 × 10⁻⁶. 2 cm -3 The thickness of the ohmic contact layer 9 is 10 nm.

[0082] The method for fabricating an epitaxial wafer for a light-emitting diode in this embodiment includes the following steps:

[0083] (1) Provide a silicon substrate;

[0084] (2) A composite buffer layer is grown on a silicon substrate;

[0085] The growth of the composite buffer layer includes the following steps:

[0086] (I) Growth of B on a silicon substrate a Al 1-a N layers;

[0087] Specifically, growing B in MOCVD a Al 1-a The N layer was grown at a temperature of 820℃ and a pressure of 120 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 was used as the carrier gas, TEB was introduced as the B source, and TMAl was introduced as the Al source.

[0088] (II) In B a Al 1-a Sc grows on layer N x B y Al 1-x-y N layers;

[0089] Specifically, growing Sc in MOCVD x B y Al 1-x-y The N layer was grown at a temperature of 840℃ and a pressure of 120 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TEB as the B source, TMAl as the Al source, and Sc(TMHD)3 as the Sc source.

[0090] (III) In Sc x B y Al 1-x-y Mg-doped B grows on N layer b Ga 1-b N layers;

[0091] Specifically, Mg-doped B is grown in MOCVD. b Ga1-b The N layer was grown at a temperature of 870℃ and a pressure of 120 torr. During growth, NH3 was introduced as the N source, TEB as the B source, TMGa as the Ga source, and CP2Mg as the Mg source in the MOCVD reaction chamber. A mixture of N2 and H2 was used as the carrier gas, with a volume ratio of N2 to H2 of 1:2.

[0092] (3) An intrinsic GaN layer is grown on the composite buffer layer;

[0093] Intrinsic GaN layers were grown in MOCVD at a temperature of 1120℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 were introduced as the carrier gas, and TMGa was introduced as the Ga source.

[0094] (4) Growing an N-type GaN layer on the intrinsic GaN layer;

[0095] In this process, an N-type GaN layer was grown in MOCVD at a temperature of 1160℃ and a pressure of 150 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gas, TMGa was introduced as the Ga source, and SiH4 was introduced as the N-type doping source.

[0096] (5) A stress-relieving layer is grown on the N-type GaN layer;

[0097] In this process, InGaN and Si-doped GaN layers are periodically grown in MOCVD to form stress-relieving layers. The InGaN layer is grown at 800℃ and 150 torr at a pressure of 150 torr. During growth, NH3 is introduced as the N source, N2 as the carrier gas, TEGa as the Ga source, and TMI as the In source in the MOCVD reaction chamber. The Si-doped GaN layer is grown at 860℃ and 150 torr at a pressure of 150 torr. During growth, NH3 is introduced as the N source, SiH4 as the Si source, H2 as the carrier gas, and TEGa as the Ga source in the MOCVD reaction chamber.

[0098] (6) Grow a multi-quantum well layer on the stress relief layer;

[0099] In this process, InGaN quantum well layers and GaN quantum barrier layers are periodically grown in MOCVD to form multiple quantum well layers. The InGaN quantum well layers are grown at a temperature of 730℃ and a growth pressure of 120 torr. During growth, NH3 is introduced as the N source, N2 as the carrier gas, TEGa as the Ga source, and TMIn as the In source in the MOCVD reaction chamber. The GaN quantum barrier layers are grown at a temperature of 880℃ and a growth pressure of 150 torr. During growth, NH3 is introduced as the N source, H2 and N2 as the carrier gases, and TEGa as the Ga source in the MOCVD reaction chamber.

[0100] (7) Grow an electron blocking layer on a multi-quantum-well layer;

[0101] In this process, an AlGaN layer was grown in MOCVD as an electron blocking layer at a growth temperature of 950℃ and a growth pressure of 180 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMAl as the Al source, and TMGa as the Ga source.

[0102] (8) Grow a P-type GaN layer on the electron blocking layer;

[0103] In this process, a P-type GaN layer was grown in MOCVD at a temperature of 950℃ and a pressure of 400 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, and CP2Mg was introduced as the P-type doping source; H2 and N2 were used as carrier gases, and TMGa was introduced as the Ga source.

[0104] (9) Growing an ohmic contact layer on a p-type GaN layer;

[0105] Specifically, an ohmic contact layer was grown in MOCVD at a temperature of 900℃ and a pressure of 150 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as an N source, CP2Mg as a P-type dopant source, TMGa as a Ga source, and TMIn as an In source, with H2 and N2 as carrier gases.

[0106] Example 2

[0107] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that B a Al 1-a The thickness of layer N21 is 45nm, Sc x B y Al 1-x-y The thickness of the N-layer 22 is 25 nm, and it is Mg-doped with B. b Ga 1-b The thickness of layer 23 (N) is 15 nm, and the doping concentration of Mg is 3 × 10⁻⁶.17 cm -3 Everything else is the same as in Example 1.

[0108] Example 3

[0109] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 2 in that, along the epitaxial growth direction, B a Al 1-a The proportion of component B in layer N21 gradually increases from 0.3 to 0.6. The rest is the same as in Example 2.

[0110] Example 4

[0111] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 3 in that, along the epitaxial growth direction, Sc x B y Al 1-x-y The proportion of the Sc component in layer N22 gradually increases from 0 to 0.25. Everything else is the same as in Example 3.

[0112] Example 5

[0113] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 4 in that, with reference to... Figure 3 The composite buffer layer 2 also includes Sc α B β Al 1-α-β Nth floor 24, Sc α B β Al 1-α-β N layer 24 is located in Sc x B y Al 1-x-y Above layer N (23), where α is constant at 0.25, β is 0.4, and Sc α B β Al 1-α-β The thickness of layer N24 is 25 nm. Correspondingly, in the fabrication method, Sc is grown in MOCVD. α B β Al 1-α-β The N-layer was grown at a temperature of 840°C and a growth pressure of 120 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source; N2 was used as the carrier gas, TEB was introduced as the B source, TMAl was introduced as the Al source, and Sc(TMHD)3 was introduced as the Sc source. All other aspects were the same as in Example 4.

[0114] Comparative Example 1

[0115] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the composite buffer layer 2 is an AlN layer with a thickness of 120 nm. Accordingly, in the fabrication method, the AlN layer is grown using magnetron sputtering (PVD) at a growth temperature of 550°C and a power of 4000 W. During growth, Ar is used as the sputtering gas, N2 as the precursor, and Al as the sputtering target. A small amount of O2 is introduced to adjust the crystal quality. All other aspects are the same as in Example 1.

[0116] Comparative Example 2

[0117] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the composite buffer layer 2 does not include Sc. x B y Al 1-x-y N-layer 22 and Mg-doped B b Ga 1-b Layer N, 23. Accordingly, the preparation method does not include the steps for preparing the above two layers. Everything else is the same as in Example 1.

[0118] Comparative Example 3

[0119] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the composite buffer layer 2 does not include Sc. x B y Al 1-x-y Layer N, 22. Accordingly, the preparation method does not include the step of preparing this layer. Everything else is the same as in Example 1.

[0120] Comparative Example 4

[0121] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that Mg is doped with B. b Ga 1-b The Mg doping concentration in layer 23 is 1×10⁻⁶. 18 cm -3 Everything else is the same as in Example 1.

[0122] The epitaxial wafers of the light-emitting diodes obtained in Examples 1 to 5 and Comparative Examples 1 to 4 were tested. The specific test methods are as follows:

[0123] (1) The epitaxial wafer was fabricated into a chip with a size of 10mil×24mil, and its luminous brightness was tested under a current of 120mA;

[0124] (2) Antistatic capability test: The antistatic performance of the base chip was tested using an electrostatic meter under the HBM (Human Body Discharge Model) model. The percentage of chips that could withstand 6000V reverse static electricity was tested.

[0125] The specific results are as follows:

[0126] Luminous intensity (120mA) / mW Antistatic capability (-6000V) Example 1 197.65 97.58% Example 2 197.93 97.95% Example 3 198.14 98.22% Example 4 198.65 98.59% Example 5 199.78 99.84% Comparative Example 1 195.63 94.52% Comparative Example 2 196.59 95.31% Comparative Example 3 196.77 95.72% Comparative Example 4 196.96 96.24%

[0127] As can be seen from the table, when the traditional light-emitting diode structure (Comparative Example 1) is changed to the composite buffer layer structure of the present invention, the luminous brightness increases from 195.63mW to 197.65mW, and the antistatic capability increases from 94.52% to 97.58%, indicating that the composite transition layer of the present invention can improve luminous efficiency and antistatic capability.

[0128] Furthermore, a comparison between Example 1 and Comparative Examples 2 to 4 shows that when the composite buffer layer structure in this invention is changed, it is difficult to effectively improve the brightness and enhance the antistatic capability.

[0129] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A light-emitting diode epitaxial wafer, characterized in that, The system includes a silicon substrate and, sequentially disposed on the silicon substrate, a composite buffer layer, an intrinsic GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, a P-type GaN layer, and an ohmic contact layer. The composite buffer layer includes sequentially stacked B... a Al 1-a N layer, Sc x B y Al 1-x-y N layer, Sc α B β Al 1-α-β N-layer and Mg-doped B b Ga 1-b N layers; Wherein, the B a Al 1-a The thickness of the N layer is 30nm~60nm, and a is 0.3~0.6; The Sc x B y Al 1-x-y The thickness of the N layer is 20nm~30nm, x is 0~0.25, and y is 0.3~0.5; The Sc α B β Al 1-α-β The thickness of the N layer is 20nm~30nm, α is 0.25, and β is 0.3~0.5; The Mg-doped B b Ga 1-b The thickness of the N layer is 10 nm to 20 nm, the b value is 0 to 0.3, and the Mg doping concentration is < 8 × 10⁻⁶. 17 cm -3 .

2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, Along the epitaxial growth direction, the B a Al 1-a The proportion of component B in layer N gradually increases.

3. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, Along the epitaxial growth direction, the Sc x B y Al 1-x-y The proportion of Sc component in the N layer gradually increases.

4. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The Mg-doped B b Ga 1-b In the N-layer, the Mg doping concentration is 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 .

5. A method for preparing a light-emitting diode epitaxial wafer, used to prepare a light-emitting diode epitaxial wafer as described in any one of claims 1 to 4, characterized in that, include: A silicon substrate is provided on which a composite buffer layer, an intrinsic GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, an electron blocking layer, a P-type GaN layer and an ohmic contact layer are sequentially grown. The composite buffer layer comprises B layers stacked sequentially. a Al 1-a N layer, Sc x B y Al 1-x-y N layer, Sc α B β Al 1-α-β N-layer and Mg-doped B b Ga 1-b N layers; Wherein, the B a Al 1-a The thickness of the N layer is 30nm~60nm, and a is 0.3~0.6; The Sc x B y Al 1-x-y The thickness of the N layer is 20nm~30nm, x is 0~0.25, and y is 0.3~0.5; The Sc α B β Al 1-α-β The thickness of the N layer is 20nm~30nm, α is 0.25, and β is 0.3~0.5; The Mg-doped B b Ga 1-b The thickness of the N layer is 10 nm to 20 nm, the b value is 0 to 0.3, and the Mg doping concentration is < 8 × 10⁻⁶. 17 cm -3 .

6. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The B a Al 1-a The growth temperature of the N layer is 800℃~850℃, and the growth pressure is 100 torr~150 torr. The Sc x B y Al 1-x-y The growth temperature of the N layer is 820℃~870℃, and the growth pressure is 100 torr~150 torr. The Mg-doped B b Ga 1-b The growth temperature of the N layer is 850℃~900℃, and the growth pressure is 100 torr~150 torr.

7. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 5 or 6, characterized in that, The Sc α B β Al 1-α-β The growth temperature of the N layer is 820℃~870℃, and the growth pressure is 100 torr~150 torr.

8. A light-emitting diode, characterized in that, Includes the light-emitting diode epitaxial wafer as described in any one of claims 1 to 4.

Citation Information

Patent Citations

  • Light-emitting diode epitaxial wafer, preparation method thereof and light-emitting diode

    CN116190517A

  • Light-emitting diode chip manufacturing method and light-emitting diode chip

    JP2018029110A