Ionically conductive solid and all-solid battery

CN117425940BActive Publication Date: 2026-11-20CANON OPTRON INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180096555.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-05-31
Filing Date
2021-12-09
Publication Date
2026-11-20
Estimated Expiration
2041-12-09

AI Technical Summary

Technical Problem

然而,由于以往的氧化物系固体电解质在加热处理中需要900℃以上的高温,因此固体电解质和电极活性物质有可能发生反应而形成高电阻相

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004472450270000033
    Figure BDA0004472450270000033
  • Figure BDA0004472450270000161
    Figure BDA0004472450270000161
  • Figure BDA0004472450270000171
    Figure BDA0004472450270000171
Patent Text Reader

Abstract

The present application provides an ion-conductive solid having high ion conductivity and capable of being produced by low-temperature heat treatment, and a full solid battery having the ion-conductive solid. The ion-conductive solid contains an oxide represented by the general formula Li 6‑3a‑2b‑c‑d Y 1‑c‑d Al a Mg b Zr c Ce d B3O9. The full solid battery has at least a positive electrode, a negative electrode, and an electrolyte, and at least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte contains the ion-conductive solid. (In the formula, a is a real number satisfying 0.000 ≤ a ≤ 0.800, b is a real number satisfying 0.000 ≤ b ≤ 0.800, c is a real number satisfying 0.000 ≤ c ≤ 0.400, d is a real number satisfying 0.000 ≤ d ≤ 0.400, and a and b satisfy 0.005 ≤ a + b ≤ 0.800.)
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to an ion-conducting solid-state battery and an all-solid-state battery. Background Technology

[0002] Lightweight and high-capacity lithium-ion rechargeable batteries have long been used in mobile devices such as smartphones and laptops, as well as in transportation equipment such as electric vehicles and hybrid vehicles.

[0003] However, because traditional lithium-ion secondary batteries used liquids containing flammable solvents as electrolytes, there were concerns about leakage of these flammable solvents and potential fires due to short circuits. Therefore, in recent years, to ensure safety, attention has been paid to secondary batteries that use ion-conducting solids as electrolytes, unlike liquid electrolytes. These secondary batteries are called all-solid-state batteries.

[0004] As electrolytes used in all-solid-state batteries, well-known solid electrolytes include oxide-based solid electrolytes and sulfide-based solid electrolytes. Among them, oxide-based solid electrolytes do not react with moisture in the atmosphere to produce hydrogen sulfide, and are therefore safer than sulfide-based solid electrolytes.

[0005] Furthermore, all-solid-state batteries include: a positive electrode containing positive active material; a negative electrode containing negative active material; an electrolyte containing an ion-conducting solid disposed between the positive and negative electrodes; and a current collector as needed (the positive and negative active materials are also collectively referred to as "electrode active materials"). When using oxide-based solid electrolytes to fabricate all-solid-state batteries, heat treatment is performed to reduce the contact resistance between the particles of the oxide-based materials contained in the solid electrolyte. However, since conventional oxide-based solid electrolytes require temperatures above 900°C during heat treatment, the solid electrolyte and electrode active materials may react to form a high-resistivity phase. This high-resistivity phase may lead to a decrease in the ionic conductivity of the ion-conducting solid and even a decrease in the output of the all-solid-state battery.

[0006] Li can be listed as an oxide-based solid electrolyte that can be produced by heat treatment at temperatures below 900°C. 2+x C 1-x B x O3 (Non-patent document 1).

[0007] Existing technical documents

[0008] Non-patent literature

[0009] Non-patent literature 1: Solid State Ionic 288(2016)248-252 Summary of the Invention

[0010] The problem that the invention aims to solve

[0011] This disclosure provides an ion-conducting solid with high ion conductivity that can be manufactured by low-temperature heat treatment, and an all-solid-state battery having the ion-conducting solid.

[0012] Solution for solving the problem

[0013] The ion-conducting solid of this disclosure is characterized by containing Li... 6-3a-2b-c-d Y 1-c- d Al a Mg b Zr c Ce d B3O9 represents an oxide.

[0014] (In the formula, a is a real number satisfying 0.000≤a≤0.800, b is a real number satisfying 0.000≤b≤0.800, c is a real number satisfying 0.000≤c≤0.400, d is a real number satisfying 0.000≤d≤0.400, and a and b are real numbers satisfying 0.005≤a+b≤0.800.)

[0015] Furthermore, the all-solid-state battery of this disclosure has at least a positive electrode, a negative electrode, and an electrolyte, wherein at least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte contains the ion-conducting solid of this disclosure.

[0016] Invention Effects

[0017] According to one aspect of this disclosure, it is possible to obtain an ion-conducting solid with high ion conductivity that can be manufactured by low-temperature heat treatment, and an all-solid-state battery having the ion-conducting solid. Detailed Implementation

[0018] In this disclosure, unless otherwise specified, the descriptions of "XX above YY below" or "XX ~ YY" indicating a numerical range refer to a numerical range that includes the lower and upper limits of the endpoints.

[0019] When recording numerical ranges in stages, the upper and lower limits of each numerical range can be combined arbitrarily.

[0020] Furthermore, in this disclosure, "solid" refers to a state of matter with a certain shape and volume among the three states of matter, and the powder state is included in "solid".

[0021] The ion-conducting solid disclosed herein contains Li 6-3a-2b-c-d Y 1-c-d Al a Mg b Zr cCe d B3O9 represents an ion-conducting solid oxide.

[0022] In the formula, a is a real number that satisfies 0.000≤a≤0.800, b is a real number that satisfies 0.000≤b≤0.800, c is a real number that satisfies 0.000≤c≤0.400, d is a real number that satisfies 0.000≤d≤0.400, and a and b are real numbers that satisfy 0.005≤a+b≤0.800.

[0023] In ionically conductive solids containing oxides represented by the above general formula, the inventors have deduced the following as a reason for the increased ion conductivity.

[0024] Within the scope of this disclosure, when a portion of Li, a monovalent metal element, is replaced by at least one element selected from Al (a trivalent metal element) and Mg (a divalent metal element), the charge balance in the crystal lattice is adjusted by the substitution of elements with different valences, thus the Li in the crystal lattice... + It is in a damaged state. Due to the surrounding Li + It will move to fill the Li + The defects in the ions increase the ionic conductivity.

[0025] The ion-conducting solid disclosed herein preferably has a monoclinic crystal structure. When the ion-conducting solid has a monoclinic crystal structure, within the scope of this disclosure, a crystal with a valence greater than Li is selected. + The metallic element is used to replace Li with at least one element from the group consisting of Al and Mg. + In some cases, Li does not contain Al and Mg 6-c- d Y 1-c-d Zr c Ce d Compared to Li6YB3O9 (i.e., the case where a=b=0.000, 0.000≤c≤0.400, and d=0.000≤d≤0.400), B3O9 (i.e., the case where a=b=c=d=0.000) can also affect the lattice volume by influencing the lattice constant, and it can also affect the ionic conductivity.

[0026] In X-ray diffraction analysis using CuKα rays (hereinafter referred to as "XRD"), the diffraction peaks generated near 2θ = 28° can vary depending on the composition of the aforementioned ion-conductive solid.

[0027] In the ion-conducting solid disclosed herein, in XRD using CuKα rays, it is preferable that diffraction peaks are present in the range of 27.90°≤2θ≤28.10°, more preferably in the range of 27.95°≤2θ≤28.05°, and even more preferably in the range of 27.97°≤2θ≤28.03°.

[0028] In XRD using CuKα rays, the position of the diffraction peak generated near 2θ = 28° can be controlled by adjusting the values ​​of a, b, c, and d in the above general formula.

[0029] The ion-conducting solid disclosed herein is such that, when the lattice volume of the ion-conducting solid is set to V, V is preferably... More preferably Further preferred

[0030] The lattice volume of ion-conducting solids can be controlled by adjusting the values ​​of a, b, c, and d in the above general formula.

[0031] In the above general formula, a is a real number that satisfies 0.000≤a≤0.800.

[0032] The lower limit of 'a' can be, for example, above 0.000, above 0.000, above 0.005, above 0.010, above 0.020, above 0.050, or above 0.100. The upper limit of 'a' can be, for example, below 0.800, below 0.400, below 0.200, below 0.100, below 0.050, or below 0.030. This range of values ​​can be combined arbitrarily, but for example, 0.000 < a ≤ 0.800 or 0.000 ≤ a ≤ 0.400.

[0033] In the above general formula, b is a real number that satisfies 0.000≤b≤0.800.

[0034] The lower limit of b can be, for example, above 0.000, above 0.005, or above 0.010. The upper limit of b can be, for example, below 0.800, below 0.400, below 0.100, below 0.050, or below 0.030. This range of values ​​can be combined arbitrarily, but for example, 0.000 ≤ b ≤ 0.400.

[0035] In the above general formula, c is a real number that satisfies 0.000≤c≤0.400.

[0036] The lower limit of c can be, for example, above 0.000, above 0.010, or above 0.030. The upper limit of c can be, for example, below 0.400, below 0.200, or below 0.100. This range of values ​​can be combined arbitrarily, but for example, 0.000 ≤ c ≤ 0.200.

[0037] In the above general formula, d is a real number that satisfies 0.000≤d≤0.400.

[0038] The lower limit of d can be, for example, above 0.000 or above 0.010. The upper limit of d can be, for example, below 0.400, below 0.200, below 0.100, or below 0.030. This range of values ​​can be combined arbitrarily, but for example, 0.000 ≤ d ≤ 0.200.

[0039] In the above general formula, a and b are real numbers that satisfy 0.005≤a+b≤0.800.

[0040] The lower limit of a+b can be, for example, above 0.005 or above 0.010. The upper limit of a+b can be, for example, below 0.800, below 0.400, or below 0.200. This range of values ​​can be combined arbitrarily, but for example, 0.010≤a+b≤0.800 or 0.010≤a+b≤0.400.

[0041] The ion-conducting solid disclosed herein may be implemented in, for example, the following embodiments, but is not limited to these embodiments. (1)

[0043] It is preferable for a to satisfy 0.010≤a≤0.100, b to satisfy 0.010≤b≤0.100, c to satisfy 0.000≤c≤0.200, d to satisfy 0.000≤d≤0.200, and for a and b to satisfy 0.020≤a+b≤0.200. (2)

[0045] It is preferable for a to satisfy 0.010≤a≤0.050, b to satisfy 0.010≤b≤0.050, c to satisfy 0.030≤c≤0.100, d to satisfy 0.010≤d≤0.030, and for a and b to satisfy 0.020≤a+b≤0.100. (3)

[0047] It is preferable for a to satisfy 0.010≤a≤0.100, b to satisfy 0.010≤b≤0.100, c to satisfy 0.000≤c≤0.200, d to satisfy 0.000≤d≤0.200, and for a and b to satisfy 0.020≤a+b≤0.200. (4)

[0049] It is preferable for a to satisfy 0.000≤a≤0.050, b to satisfy 0.000≤b≤0.050, c to satisfy 0.050≤c≤0.150, d to satisfy 0.010≤d≤0.030, and for a and b to satisfy 0.010≤a+b≤0.030.

[0050] The method for manufacturing the ion-conducting solid disclosed herein will now be described.

[0051] The method for manufacturing the ion-conducting solid disclosed herein can be carried out in the following manner, but is not limited thereto.

[0052] A substance containing the general formula Li 6-3a-2b-c-d Y 1-c-d Al a Mg b Zr c Ce d Method for manufacturing ion-conducting solids of oxides represented by B3O9.

[0053] It may have a single firing process in which raw materials mixed in order to obtain an oxide represented by the general formula are heated at a temperature below the melting point of the oxide.

[0054] In the formula, a is a real number that satisfies 0.000≤a≤0.800, b is a real number that satisfies 0.000≤b≤0.800, c is a real number that satisfies 0.000≤c≤0.400, d is a real number that satisfies 0.000≤d≤0.400, and a and b are real numbers that satisfy 0.005≤a+b≤0.800.

[0055] The method for manufacturing an ion-conducting solid disclosed herein may include a single firing step, wherein raw materials are weighed / mixed to obtain an oxide represented by the above general formula, and the raw materials are heated at a temperature below the melting point of the oxide to produce an ion-conducting solid containing the oxide. Alternatively, the manufacturing method may include a second firing step, wherein the ion-conducting solid containing the obtained oxide is heated at a temperature below the melting point of the oxide to produce a sintered body containing the ion-conducting solid.

[0056] The following describes in detail the manufacturing method of the ion-conducting solid of the present disclosure, which includes the above-described primary firing process and the above-described secondary firing process, but the present disclosure is not limited to the manufacturing method described below.

[0057] One-time firing process

[0058] In the firing process, chemical reagent-grade raw materials such as Li3BO3, H3BO3, Y2O3, ZrO2, CeO2, Al2O3, and MgO are weighed according to chemical proportions and mixed to form a product with the general formula Li 6-3a-2b-c-d Y 1-c-d Al a Mg b Zr c Ce dB3O9 (Also, a is a real number satisfying 0.000≤a≤0.800, b is a real number satisfying 0.000≤b≤0.800, c is a real number satisfying 0.000≤c≤0.400, d is a real number satisfying 0.000≤d≤0.400, and a and b are real numbers satisfying 0.005≤a+b≤0.800).

[0059] There are no particular restrictions on the apparatus used for mixing, but a powder mixer such as a planetary ball mill can be used, for example. There are no particular restrictions on the material and capacity of the container used for mixing, nor on the material and diameter of the balls; they can be appropriately selected according to the type and amount of raw materials used. For example, a 45 mL container made of zirconia and 5 mm diameter zirconia balls can be used. Furthermore, there are no particular restrictions on the mixing conditions; for example, a rotation speed of 50 rpm to 2000 rpm and a time of 10 minutes to 60 minutes can be used.

[0060] After obtaining a mixed powder of the above-mentioned raw materials through this mixing process, the obtained mixed powder is pressurized to form granules. Known pressurization methods such as cold uniaxial molding and cold water pressure molding can be used as pressurization methods. There are no particular restrictions on the conditions for pressurization in the single firing process; for example, a pressure of 100 MPa to 200 MPa can be used.

[0061] The obtained particles were sintered using a sintering apparatus similar to an atmospheric sintering device. The temperature for solid-phase synthesis using a single sintering process was kept below the temperature required for the formation of Lip particles. 6-3a-2b-c-d Y 1-c-d Al a Mg b Zr c Ce d There are no particular restrictions on the melting point of the ion-conducting solid represented by B3O9. The temperature for a single firing can be, for example, below 700°C, 680°C, 670°C, 660°C, or 650°C, or above 500°C. This range can be arbitrarily combined. Solid-state synthesis can be sufficiently achieved as long as the temperature is within the above range. There are no particular restrictions on the time of a single firing process, but it can be, for example, around 700 to 750 minutes.

[0062] Through the above-described single firing process, it is possible to produce a product containing the above-described general formula Li. 6-3a-2b-c-d Y 1-c- d Al a Mg b Zr c Ce dB3O9 represents an ion-conducting solid containing an oxide. Powder containing this oxide can also be obtained by pulverizing the ion-conducting solid using a mortar / mortar rod and a planetary mill.

[0063] Secondary firing process

[0064] In the secondary firing process, at least one of the following is selected from the group consisting of an ion-conducting solid containing an oxide obtained from the primary firing process and a powder containing an ion-conducting solid containing an oxide, and is then press-formed and fired to obtain a sintered body containing an ion-conducting solid containing the oxide of the present disclosure.

[0065] Pressure forming and secondary firing can be performed simultaneously using methods such as spark plasma sintering (SPS) and hot pressing. Alternatively, after producing particles through cold uniaxial forming, secondary firing can be performed in an atmospheric, oxidizing, or reducing atmosphere. Under these conditions, ionically conductive solids with high ion conductivity can be obtained without melting caused by heat treatment. There are no particular limitations on the pressure forming conditions in the secondary firing process; for example, pressures of 10 MPa to 100 MPa can be used.

[0066] The temperature for secondary firing is lower than that for Li 6-3a-2b-c-d Y 1-c-d Al a Mg b Zr c Ce d The melting point of the ion-conducting solid represented by B3O9. The temperature for the secondary firing is preferably below 700°C, more preferably below 680°C, further preferably below 670°C, and particularly preferably below 660°C. There is no particular limitation on the lower limit of this temperature; the lower the better, but it is, for example, above 500°C. This temperature range can be arbitrarily combined, but for example, a range of above 500°C and below 700°C can be used. As long as it is within the above range, it is possible to suppress the melting or decomposition of the ion-conducting solid containing the oxide of this disclosure during the secondary firing process, and to obtain a fully sintered sintered body containing the ion-conducting solid containing the oxide of this disclosure.

[0067] The time for the second firing process can be adjusted appropriately based on factors such as the firing temperature, but it is preferably less than 24 hours, although less than 1 hour is also acceptable. For example, the second firing process can take more than 5 minutes.

[0068] There is no particular limitation on the method of cooling the sintered body containing the oxide of the present disclosure obtained through the secondary firing process. It can be cooled naturally (furnace cooling), cooled rapidly, cooled gradually compared to natural cooling, or maintained at a certain temperature during cooling.

[0069] Next, the all-solid-state battery disclosed herein will be described.

[0070] All-solid-state batteries generally have a positive electrode, a negative electrode, an electrolyte containing an ion-conducting solid disposed between the positive and negative electrodes, and a current collector as needed.

[0071] The all-solid-state battery of this disclosure has at least a positive electrode, a negative electrode, and an electrolyte, wherein at least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte contains an ion-conducting solid of this disclosure.

[0072] The all-solid-state battery disclosed herein can be a bulk-type battery or a thin-film-type battery. The specific shape of the all-solid-state battery disclosed herein is not particularly limited, but examples include coin-shaped, button-shaped, sheet-shaped, and laminated types.

[0073] The all-solid-state battery of this disclosure has an electrolyte. Furthermore, in the all-solid-state battery of this disclosure, preferably at least the electrolyte contains the ion-conducting solid of this disclosure.

[0074] The solid electrolyte in the all-solid-state battery disclosed herein may be composed of the ion-conducting solid of this disclosure, or may contain other ion-conducting solids, and may also contain ionic liquids or gel polymers. There are no particular limitations on other ion-conducting solids; they may include ion-conducting solids commonly used in all-solid-state batteries, such as LiI, Li3PO4, and Li7La3Zr2O. 12 The content of the ion-conducting solid of this disclosure in the electrolyte of the all-solid-state battery is not particularly limited, but is preferably 25% by mass or more, more preferably 50% by mass or more, further preferably 75% by mass or more, and particularly preferably 100% by mass.

[0075] The all-solid-state battery disclosed herein has a positive electrode. This positive electrode may contain a positive electrode active material, or it may contain the positive electrode active material and the ion-conducting solid of this disclosure. Known positive electrode active materials, such as sulfides containing transition metal elements and oxides containing lithium and transition metal elements, can be used without particular limitation as the positive electrode active material.

[0076] Furthermore, the positive electrode may also contain binders, conductive agents, etc. Examples of binders include polyvinylidene fluoride, polytetrafluoroethylene, and polyvinyl alcohol. Examples of conductive agents include natural graphite, artificial graphite, acetylene black, and vinyl black.

[0077] The all-solid-state battery disclosed herein has a negative electrode. This negative electrode may contain a negative electrode active material, or it may contain the negative electrode active material and the ion-conducting solid of this disclosure. Known negative electrode active materials, such as inorganic compounds like lithium, lithium alloys, and tin compounds, carbonaceous materials capable of absorbing and releasing lithium ions, and conductive polymers, can be used without particular limitation as the negative electrode active material.

[0078] Furthermore, the negative electrode may also contain binders, conductive agents, etc. The same binders and conductive agents listed in the positive electrode can be used as these.

[0079] Here, "containing" an electrode active material means that the electrode has an active material as a component, element, or property. For example, the presence of an active material within the electrode or the coating of an active material on the electrode surface are equivalent to the aforementioned "containing".

[0080] The positive and negative electrodes can be obtained by known methods such as mixing raw materials, molding, and heat treatment. Therefore, it can be assumed that the ion-conducting solid can easily ensure the lithium-ion conduction path by integrating into the gaps between the electrode active materials. Compared with existing technologies, the ion-conducting solid of this disclosure can be manufactured by low-temperature heat treatment, thus suppressing the formation of a high-resistivity phase resulting from the reaction between the ion-conducting solid and the electrode active material.

[0081] Both the positive and negative electrodes described above can also have current collectors. Known current collectors such as aluminum, titanium, stainless steel, nickel, iron, sintered carbon, conductive polymers, and conductive glass can be used. In addition, for the purpose of improving adhesion, conductivity, oxidation resistance, etc., substances obtained by treating the surface of aluminum, copper, etc., with carbon, nickel, titanium, silver, etc., can also be used as current collectors.

[0082] The all-solid-state battery disclosed herein can be obtained, for example, by known methods such as laminating, molding, and heat-treating a positive electrode, a solid electrolyte, and a negative electrode. Compared to existing technologies, the ion-conducting solid of this disclosure can be fabricated through low-temperature heat treatment, thus suppressing the formation of a high-resistivity phase resulting from the reaction between the ion-conducting solid and the electrode active material. Therefore, it is considered possible to obtain an all-solid-state battery with excellent output characteristics.

[0083] Next, the composition and the methods for measuring the various physical properties involved in this disclosure will be explained.

[0084] Identification and analytical methods for Al, Mg, Zr, and Ce

[0085] Compositional analysis of ion-conducting solids is performed using samples solidified by pressure molding via wavelength dispersive X-ray diffraction (XRF). However, in cases where analysis is difficult due to particle size effects, it is preferable to perform XRF-based compositional analysis by vitrifying the ion-conducting solid using the glass bead method. Furthermore, when the yttrium peak overlaps with the peaks of Al, Mg, Zr, and Ce in the XRF, compositional analysis is preferable using inductively coupled plasma atomic emission spectrometry (ICP-AES).

[0086] In the XRF case, the analytical apparatus used was the Rigaku ZSX Primus II manufactured by Rigaku Corporation. The analytical conditions were: Rh was used at the anode of the X-ray tube bulb, under vacuum, with an analytical diameter of 10 mm, an analytical range of 17-81 degrees, a step size of 0.01 degrees, and a scan rate of 5 seconds per step. Furthermore, a proportional counter was used for the determination of light elements, and a scintillation counter was used for the determination of heavy elements.

[0087] Elements are identified based on the peak positions of the spectra obtained by XRF, and the molar concentration ratios Y / Al, Y / Mg, Y / Zr, and Y / Ce are calculated based on the number of X-ray photons per unit time, i.e., the count rate (unit: cps), thereby determining a, b, c, and d.

[0088] • Determination of X-ray diffraction peaks and calculation of crystal volume

[0089] In X-ray diffraction analysis of ion-conductive solids, D8 ADVANCE manufactured by BrukerAXS Co., Ltd. was used.

[0090] After the powder obtained by crushing ion-conductive solids with a mortar and pestle is placed in a holder, the substance is pressed and flattened by a glass plate as the analytical sample, and X-ray diffraction analysis (XRD) is performed using a CuKα ray source.

[0091] The temperature was room temperature (25℃), the analysis range was 10deg~70deg, the step size was 0.007, and the scan speed was 0.1 step / second.

[0092] In the diffraction curve obtained by XRD, the 2θ of the peak generated by 2θ = 28.00 ± 0.200 degrees originating from Li6YB3O9 is determined as the peak position.

[0093] The lattice volume of the crystalline phase was calculated using diffraction patterns obtained from XRD and the structural analysis software TOPAS manufactured by BrukerAXS Co., Ltd. TOPAS was used to fit and analyze the diffraction patterns obtained from XRD and the diffraction pattern of the monoclinic crystalline phase to calculate the lattice volume.

[0094] Example

[0095] The following examples illustrate the specific fabrication and evaluation of the ion-conducting solids disclosed herein. However, this disclosure is not limited to these examples.

[0096] [Example 1]

[0097] • Single firing process

[0098] Li3BO3 (manufactured by Toyoshima Corporation, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical Industry, purity 99.9% by mass), and Al2O3 (manufactured by Baikowski, purity 99.9%) are used as raw materials to produce Li 5.970 Y 1.000 Al 0.010 The B3O9 method uses chemical proportions to weigh each raw material, and mixes them for 30 minutes using a Fritsch P-7 planetary mill at 300 rpm. The planetary mill is made of zirconium oxide. A ball and a 45mL container.

[0099] After mixing, the mixed powder was cold uniaxially shaped using an NPASYSTEM 100kN electric stamping device P3052-10 at 147MPa and then sintered in an atmospheric atmosphere. The heating temperature was 650℃ and the holding time was 720 minutes.

[0100] The obtained ion-conducting solid containing oxides was pulverized for 180 minutes using a Fritsch P-7 planetary mill at a disc speed of 230 rpm to produce powder of the ion-conducting solid containing oxides.

[0101] Secondary firing process

[0102] The powder of the oxide-containing ion-conducting solid obtained by the above method was shaped and then sintered a second time to produce the sintered body of the oxide-containing ion-conducting solid of Example 1. The second sintering was carried out in an atmospheric atmosphere, with a heating temperature of 650°C and a holding time of 720 minutes.

[0103] [Examples 2-6]

[0104] Except for weighing the above raw materials by chemical proportions in the manner described in Table 1, the sintered bodies of ion-conducting solids containing oxides of Examples 2 to 6 were prepared by the same procedure as in Example 1.

[0105] [Example 7]

[0106] Using Li3BO3 (manufactured by Toyoshima Corporation, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical Industry, purity 99.9% by mass), and MgO (manufactured by Ube Material, purity 99.0%) as raw materials, to become Li 5.980 Y 1.000 Mg 0.010 The raw materials were weighed using chemical proportions in the B3O9 method. Otherwise, the sintered body of the ion-conducting solid containing oxides of Example 7 was prepared using the same procedure as in Example 1.

[0107] [Examples 8-12]

[0108] Except for weighing the above raw materials by chemical proportions in the manner that b is the value recorded in Table 1, the sintered bodies of the ion-conducting solids containing oxides of Examples 8 to 12 were prepared by the same procedure as in Example 7.

[0109] [Example 13]

[0110] Using Li3BO3 (manufactured by Toyoshima Corporation, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical Industry, purity 99.9% by mass), Al2O3 (manufactured by Baikowski, purity 99.9%), and ZrO2 (manufactured by Shin Nippon Electric Works, purity 99.9%) as raw materials, it becomes Li 5.725 Y 0.800 Al 0.025 Zr 0.200 The raw materials were weighed using chemical proportions in the B3O9 method. Otherwise, the sintered body of the ion-conducting solid containing oxides of Example 13 was prepared using the same procedure as in Example 1.

[0111] [Example 14]

[0112] Except that the raw materials mentioned above are weighed in chemical proportions such that a and c are the values ​​recorded in Table 1, the sintered body of the ion-conducting solid containing oxide of Example 14 is prepared by the same procedure as in Example 13.

[0113] [Example 15]

[0114] Using Li3BO3 (manufactured by Toyoshima Corporation, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical Industry, purity 99.9% by mass), Al2O3 (manufactured by Baikowski, purity 99.9%), and CeO2 (manufactured by Shin-Etsu Chemical Industry, purity 99.9%) as raw materials, it becomes Li5.725 Y 0.800 Al 0.025 Ce 0.200 The raw materials were weighed using chemical proportions in the B3O9 method. Otherwise, the sintered body of the ion-conducting solid containing oxides of Example 15 was prepared using the same procedure as in Example 1.

[0115] [Example 16]

[0116] Except that the raw materials were weighed in chemical proportions such that a and d are the values ​​recorded in Table 1, the sintered body of the ion-conducting solid containing oxide of Example 16 was prepared by the same procedure as in Example 15.

[0117] [Example 17]

[0118] Using Li3BO3 (manufactured by Toyoshima Corporation, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical Industry, purity 99.9% by mass), MgO (manufactured by Ube Materials, purity 99.0%), and ZrO2 (manufactured by Nippon Electric Works, purity 99.9%) as raw materials, it becomes Li 5.750 Y 0.800 Mg 0.025 Zr 0.200 The raw materials were weighed using chemical proportions in the B3O9 method. Otherwise, the sintered body of the ion-conducting solid containing oxides of Example 17 was prepared using the same procedure as in Example 1.

[0119] [Example 18]

[0120] Except that the raw materials were weighed in chemical proportions such that b and c were the values ​​recorded in Table 1, the sintered body of the ion-conducting solid containing oxide of Example 18 was prepared by the same procedure as in Example 17.

[0121] [Example 19]

[0122] Using Li3BO3 (manufactured by Toyoshima Corporation, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical Industry, purity 99.9% by mass), MgO (manufactured by Ube Materials, purity 99.0%), and CeO2 (manufactured by Shin-Etsu Chemical Industry, purity 99.9%) as raw materials, it becomes Li 5.750 Y 0.800 Mg 0.025 Ce 0.200 The raw materials were weighed using chemical proportions in the B3O9 method. Otherwise, the sintered body of the ion-conducting solid containing oxides of Example 19 was prepared using the same procedure as in Example 1.

[0123] [Example 20]

[0124] Except that the raw materials mentioned above are weighed in chemical proportions such that b and d are the values ​​recorded in Table 1, the sintered body of the ion-conducting solid containing oxide of Example 20 is produced by the same procedure as in Example 19.

[0125] [Example 21]

[0126] Using Li3BO3 (manufactured by Toyoshima Corporation, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical Industry, purity 99.9% by mass), Al2O3 (manufactured by Baikowski, purity 99.9%), ZrO2 (manufactured by Nippon Electric Works, purity 99.9%), and CeO2 (manufactured by Shin-Etsu Chemical Industry, purity 99.9%) as raw materials, a process is completed to produce Li 5.800 Y 0.875 Al 0.025 Zr 0.100 Ce 0.025 The raw materials were weighed using chemical proportions in the B3O9 method. Otherwise, the sintered body of the ion-conducting solid containing oxides of Example 21 was prepared using the same procedure as in Example 1.

[0127] [Examples 22-24]

[0128] Except for weighing the above raw materials in chemical proportions such that a, c, and d are the values ​​recorded in Table 1, the sintered bodies of the ion-conducting solids containing oxides of Examples 22 to 24 were prepared using the same procedure as in Example 21.

[0129] [Example 25]

[0130] Using Li3BO3 (manufactured by Toyoshima Corporation, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Y2O3 (manufactured by Shin-Etsu Chemical Industry, purity 99.9% by mass), MgO (manufactured by Ube Materials, purity 99.0%), ZrO2 (manufactured by Nippon Electric Works, purity 99.9%), and CeO2 (manufactured by Shin-Etsu Chemical Industry, purity 99.9%) as raw materials, it becomes Li 5.825 Y 0.875 Mg 0.025 Zr 0.100 Ce 0.025 The raw materials were weighed using chemical proportions in the B3O9 method. Otherwise, the sintered body of the ion-conducting solid containing oxides of Example 25 was prepared using the same procedure as in Example 1.

[0131] [Examples 26-28]

[0132] Except for weighing the above raw materials in chemical proportions such that b, c, and d are the values ​​recorded in Table 1, the sintered bodies of the ion-conducting solids containing oxides of Examples 26 to 28 were prepared using the same procedure as in Example 25.

[0133] [Example 29]

[0134] The following raw materials were used to produce Li₃BO₃ (manufactured by Toyoshima Corporation, purity 99.9% by mass), H₃BO₃ (manufactured by Kanto Chemical, purity 99.5%), Y₂O₃ (manufactured by Shin-Etsu Chemical Industry, purity 99.9% by mass), Al₂O₃ (manufactured by Baikowski, purity 99.9%), and MgO (manufactured by Ube Materials, purity 99.0%). 5.500 Y 1.000 Al 0.100 Mg 0.100 The raw materials were weighed using chemical proportions in the B3O9 method. Otherwise, the sintered body of the ion-conducting solid containing oxides of Example 29 was prepared using the same procedure as in Example 1.

[0135] [Comparative Example 1]

[0136] • Single firing process

[0137] Using Li3BO3 (manufactured by Toyoshima Corporation, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%) and Y2O3 (manufactured by Shin-Etsu Chemical Industry, purity 99.9% by mass) as raw materials, each raw material was weighed in chemical proportions to form Li6YB3O9. Otherwise, the ion-conducting solid and the powder of the ion-conducting solid were prepared using the same process as in Example 1.

[0138] Secondary firing process

[0139] The powder of the ion-conducting solid obtained by the above method was shaped by spark plasma sintering (SPS) and subjected to a second firing to produce a sintered body of the ion-conducting solid containing oxides, as described in Comparative Example 1. The heating temperature was 700°C, the pressure was 30 MPa, and the holding time was 10 minutes.

[0140] [Comparative Example 2]

[0141] • Single firing process

[0142] Using Li3BO3 (manufactured by Toyoshima Corporation, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), ZrO2 (manufactured by Nippon Electric Works, purity 99.9%), and CeO2 (manufactured by Shin-Etsu Chemical Industry, purity 99.9%) as raw materials, it becomes Li 5.000 Zr0.800 Ce 0.200 The raw materials were weighed using chemical proportions in the B3O9 method. Otherwise, the solids and solid powders were prepared using the same procedures as in Example 1.

[0143] Secondary firing process

[0144] The solid powder obtained by the above method was shaped and subjected to a second firing to produce the oxide-containing sintered body of Comparative Example 2. The second firing was carried out in an atmospheric atmosphere, with a heating temperature of 550°C and a holding time of 720 minutes.

[0145] For the sintered bodies of the oxide-containing ion-conducting solids of Examples 1-29, compositional analysis was performed using the methods described above. Furthermore, for the sintered bodies of the oxide-containing ion-conducting solids of Examples 1-29, X-ray diffraction peaks were measured and lattice volumes were calculated. Additionally, for the sintered bodies of Examples 1-29 and Comparative Examples 1-2, ion conductivity was measured using the following methods.

[0146] The method for determining ionic conductivity is described below. Furthermore, the evaluation results obtained are shown in Tables 1 and 2.

[0147] • Determination of ionic conductivity

[0148] In a sintered body of an ion-conducting solid containing oxides in a flat, plate-shaped form obtained by secondary firing, two parallel, facing surfaces with a large surface area are polished with sandpaper. The dimensions of this flat, ion-conducting solid containing oxides can be, for example, 0.9 cm × 0.9 cm × 0.05 cm, but are not limited to this. Polishing begins at #500 grit for 15–30 minutes, followed by #1000 grit for 10–20 minutes, and finally #2000 grit for 5–10 minutes. The process is complete if no visually noticeable unevenness or scratches are observed on the polished surface.

[0149] After grinding, a gold film was formed on the ground surface of the sintered solid containing oxides using a Sanyu SC-701MkII ADVANCE sputtering apparatus. The film formation conditions were: Ar process gas, vacuum degree of 2 Pa to 5 Pa, and film formation time of 5 minutes. The resulting material was used as the test sample. After film formation, the AC impedance of the test sample was measured.

[0150] Impedance measurements were performed using an impedance / gain phase analyzer SI1260 and a dielectric interface system 1296 (both manufactured by SOLARTRON). The measurement conditions were 27°C, 20mV amplitude, and 0.1Hz to 1MHz frequency.

[0151] The resistance of the sintered body containing an oxide-containing ionic conductive solid was calculated using the Nyquist curve obtained from impedance measurement and the Scribner AC analytical software ZVIEW. An equivalent circuit corresponding to the measured sample was set up in ZVIEW, and the equivalent circuit and the Nyquist curve were fitted and analyzed to calculate the resistance of the sintered body containing the oxide-containing ionic conductive solid. The ionic conductivity was calculated using the calculated resistance, the thickness of the sintered body containing the oxide-containing ionic conductive solid, and the electrode area, according to the following formula.

[0152] Ionic conductivity (S / cm) = Thickness of sintered solid containing oxides (cm) / (Resistance of sintered solid containing oxides (Ω) × Electrode area (cm²) 2 ))

[0153] ·result

[0154] Table 1 summarizes the chemical proportions (general formula Li) of the raw materials used in manufacturing the sintered bodies of ion-conducting solids containing each oxide in Examples 1-29 and Comparative Examples 1-2. 6-3a-2b-c-d Y 1-c-d Al a Mg b Zr c Ce d The values ​​of a, b, c, and d in B3O9 and the ionic conductivity are also included. Furthermore, Table 2 summarizes the diffraction peak positions and lattice volumes of the sintered bodies obtained from Examples 1 to 29.

[0155] The results of the above compositional analysis confirm that the sintered bodies of the oxide-containing ion-conducting solids of Examples 1-29 and Comparative Example 1 all have the composition described in the chemical proportions of the raw materials as shown in Table 1. Furthermore, the sintered bodies of the oxide-containing ion-conducting solids of Examples 1-29 exhibit high ion conductivity even when fired at temperatures below 700°C. On the other hand, the main crystalline structure of the sintered body of Comparative Example 2 is a mixture of ZrO2 and CeO2 used as raw materials.

[0156] [Table 1]

[0157] Table 1

[0158]

[0159] In the column for ionic conductivity, “※1” indicates high resistance and that ionic conductivity cannot be measured.

[0160] [Table 2]

[0161] Table 2

[0162]

[0163] In the column for peak position, “※2” indicates that no peak was found in the range of 2θ = 27.50° to 28.50°. In the column for lattice volume, “-” indicates that no data was obtained.

Claims

1. An ion-conducting solid, characterized in that, Contains Li 6-3a-2b-c-d Y 1-c-d Al a Mg b Zr c Ce d B 3O9 represents an oxide. In the formula, a is a real number that satisfies 0.000≤a≤0.400, b is a real number that satisfies 0.000≤b≤0.200, c is a real number that satisfies 0.000≤c≤0.400, d is a real number that satisfies 0.000≤d≤0.400, and a and b are real numbers that satisfy 0.010≤a+b≤0.

400.

2. The ion-conducting solid according to claim 1, characterized in that, The values ​​of c and d are 0.000≤c≤0.200 and 0.000≤d≤0.200, respectively.

3. The ion-conducting solid according to claim 1 or 2, characterized in that, The value of c is 0.

000.

4. The ion-conducting solid according to claim 1 or 2, characterized in that, d is 0.

000.

5. The ion-conducting solid according to claim 1 or 2, characterized in that, The values ​​of a, b, c, and d are 0.000≤c≤0.200, 0.000≤d≤0.200, and 0.010≤a+b≤0.

100.

6. An all-solid-state battery, comprising at least a positive electrode, a negative electrode, and an electrolyte, characterized in that, At least one of the following groups selected from the positive electrode, the negative electrode, and the electrolyte contains an ion-conducting solid as described in any one of claims 1 to 5.

7. The all-solid-state battery according to claim 6, characterized in that, At least the electrolyte contains the ion-conducting solid.