A hydrostatically resistant carbon fiber composite clad foam structure and method of making

By using carbon fiber composite material to encapsulate the foam structure in the underwater pressure-resistant structure, and by dividing the structure into sections with carbon fiber composite material and adhesive film layers to form a brick wall-like design, the problems of insufficient lightweight, sound insulation and pressure resistance of existing pressure-resistant structures are solved, thus achieving better protection for underwater equipment.

CN117429545BActive Publication Date: 2026-11-20AEROSPACE INST OF ADVANCED MATERIALS & PROCESSING TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311419015.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-30
Publication Date
2026-11-20
Estimated Expiration
2043-10-30

AI Technical Summary

Technical Problem

Existing underwater pressure-resistant structures struggle to balance lightweight, sound insulation, and pressure resistance, especially in deep-water environments where the protection requirements for electronic components and testing equipment in submersibles are not effectively met.

Method used

The foam structure is encapsulated with carbon fiber composite material. By dividing the main foam structure into multiple regions along the radial direction and encapsulating each region with a carbon fiber composite material layer and an adhesive film layer, a brick wall-like structure is formed, which enhances the overall rigidity and sound insulation performance.

Benefits of technology

It significantly improves the pressure resistance and sound insulation of underwater pressure-resistant structures, reduces the risk of local stress concentration, and protects underwater equipment from hydrostatic pressure and noise.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117429545B_ABST
    Figure CN117429545B_ABST
Patent Text Reader

Abstract

The present application relates to a kind of carbon fiber composite material pressure-resistant foam structure and preparation method.The carbon fiber composite material pressure-resistant foam structure includes foam main structure and carbon fiber composite material layer covering foam main structure, the foam main structure has 3-5 regions radially outward, each region has multiple pieces of covering foam block, each region includes the number of covering foam block a n =2 n+1 , n≥1, each piece of covering foam block includes foam block and carbon fiber composite material layer and adhesive film layer sequentially covering the surface of foam block.The carbon fiber composite material pressure-resistant foam structure in the present application can meet the demand of light weight, sound insulation performance demand and the improvement of pressure resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of underwater high-pressure resistant structural components, and particularly relates to a carbon fiber composite material-coated foam structure resistant to hydrostatic pressure and its preparation method. Background Technology

[0002] Currently, as submersibles operate at greater depths, their internal pressure-resistant structures play a crucial role in enhancing performance. These structures house electronic components and testing equipment, requiring sufficient strength and stability to prevent damage from seawater pressure. However, excessive weight gain can hinder performance; furthermore, the acoustic insulation of the mounted electronic components (such as sensors) limits the use of high-rigidity materials. Due to the high-pressure requirements of deep-sea components and their acoustic demands, underwater pressure-resistant structures now face higher demands in terms of configuration design, material selection, and application.

[0003] Therefore, it is essential to provide a novel hydrostatic pressure-resistant carbon fiber composite material-coated foam structure and its preparation method. Summary of the Invention

[0004] To address one or more technical problems existing in the prior art, this invention provides a hydrostatic pressure-resistant carbon fiber composite material-coated foam structure and its preparation method; the hydrostatic pressure-resistant carbon fiber composite material-coated foam structure of this invention can simultaneously meet the requirements of lightweighting, sound insulation performance, and improved pressure resistance.

[0005] The present invention provides, in a first aspect, a carbon fiber composite material-coated foam structure resistant to hydrostatic pressure. The carbon fiber composite material-coated foam structure includes a foam body structure and a carbon fiber composite material layer covering the foam body structure. The foam body structure has 3 to 5 regions radially outward, each region having multiple coated foam blocks, and the number of coated foam blocks in each region is a. n =2 n+1 , n≥1, each foam block includes a foam block and a carbon fiber composite material layer and a film layer sequentially covering the surface of the foam block.

[0006] Preferably, the foam blocks are distributed in a brick wall-like structure.

[0007] Preferably, the foam body structure has three regions in a radially outward direction, namely an inner region, a middle region, and an outer region; the number of covered foam blocks included in the inner region, the middle region, and the outer region are 4, 8, and 16 respectively.

[0008] Preferably, the outer diameter of the intermediate region is 2.4 to 2.8 times the outer diameter of the inner region; and the outer diameter of the outer region is 1.4 to 1.6 times the outer diameter of the intermediate region.

[0009] In a second aspect, the present invention provides a method for preparing the hydrostatic pressure-resistant carbon fiber composite material-coated foam structure described in the first aspect, the method comprising the following steps:

[0010] (1) Divide the disc-shaped foam into 3 to 5 regions radially outward, and further divide each region into a circumferential division. n A block of foam, a n =2 n+1 , n≥1;

[0011] (2) Each foam block is coated and layered with carbon fiber composite prepreg and film in sequence, and then placed in a mold for pre-compacting after coating;

[0012] (3) Use carbon fiber composite prepreg to cover the pre-compacted 3 to 5 areas of segmented foam blocks as a whole. After covering, put them into a mold for molding and curing to obtain a carbon fiber composite covered foam structure resistant to hydrostatic pressure.

[0013] Preferably, the carbon fiber composite prepreg is made by impregnating carbon fiber with epoxy resin; the carbon fiber is unidirectional T300, T700, T800 or T1000 carbon fiber; the epoxy resin is a medium-low temperature curing epoxy resin or a high temperature curing epoxy resin; and the foam is PMI foam.

[0014] Preferably, the pre-compression is performed by holding the pressure at a temperature of 60–80°C and a pressure of 2–4 MPa for 10–30 minutes.

[0015] Preferably, the material is molded and cured for 2-4 hours at a temperature of 100-140°C and a pressure of 5-6 MPa.

[0016] Preferably, based on the pressure resistance requirements, a static simulation of the carbon fiber composite material-coated foam structure with hydrostatic pressure resistance is performed using simulation software to obtain an optimized carbon fiber composite material-coated foam structure with hydrostatic pressure resistance.

[0017] Preferably, the static simulation includes the following steps:

[0018] (a) Establish a solid model of a carbon fiber composite material foam structure resistant to hydrostatic pressure, and import the established solid model into simulation software to establish a finite element model.

[0019] (b) Assign material properties to each component separately, establish a compressive failure criterion, apply a given compressive load, and perform analysis;

[0020] (c) Adjust key structural and material parameters based on the results of finite element simulation to optimize the design; the adjustment includes adjusting the thickness and layup of carbon fiber composite materials or using carbon fiber composite materials or foams with better performance; the simulation results include stress distribution cloud maps and failure coefficient cloud maps under a given compressive load, and determine whether the structure fails under a given strength criterion; the optimal solution of the design structure is obtained through step-by-step iterative design.

[0021] Compared with the prior art, the present invention has at least the following beneficial effects:

[0022] (1) The hydrostatic pressure resistant carbon fiber composite material foam-coated structure provided by the present invention uses foam material as the main structure of the pressure-resistant element. The main structure of the foam is reasonably divided into sections and foam blocks. The sections of foam are then coated with carbon fiber composite material and adhesive film in sequence. The structure is reinforced with carbon fiber composite material, thereby improving the overall stiffness and strength of the structural components. More importantly, the distributed distribution of each coated foam block forms a brick wall structure to support the overall pressure-resistant structure. This can effectively share the pressure required by the structure, help to evenly disperse the underwater hydrostatic pressure, and reduce the risk of local stress concentration. In the brick wall structure, the edges of the coated foam blocks in two adjacent areas are staggered along the radial direction. In addition to effectively sharing the pressure required by the structure, this can also effectively improve the sound insulation performance of the structure.

[0023] (2) The foam block of the present invention comprises a foam block and a carbon fiber composite material layer and an adhesive film layer sequentially covering the surface of the foam block. That is, the foam block of the present invention creatively adds an additional adhesive film layer on top of the carbon fiber composite material layer. The adhesive film layer forms an additional sound insulation layer on top of the carbon fiber composite material layer. This sound insulation layer can effectively absorb and reduce the energy of incoming sound waves, thereby weakening the propagation of sound. The present invention finds that the adhesive film has a certain elasticity and can vibrate and absorb the mechanical energy of sound waves to a certain extent, which helps to reduce the possibility of sound propagation inside the structure. Furthermore, the foam block of the present invention comprises a foam block, a carbon fiber composite material layer, and an adhesive film layer, forming multiple barriers. The multi-layered design of the carbon fiber composite material can reflect, absorb, and scatter sound waves, thereby effectively improving sound insulation. This multi-layered design hinders the free propagation of sound waves and reduces the possibility of sound transmission through the structure. In addition, the present invention has found that the film layer can also seal the structure, preventing sound waves from propagating through the gaps between the carbon fiber composite layers, which also helps to significantly improve the sound insulation effect. This is crucial for sound insulation in underwater applications, because water is an effective medium for sound wave propagation, and even small sound leaks can be propagated over long distances in the underwater environment. The hydrostatic pressure-resistant carbon fiber composite material-coated foam structure in this invention helps to significantly improve the sound insulation effect of the pressure-resistant structure, which is very important for applications that need to reduce noise or protect sensitive equipment in underwater environments.

[0024] (3) The preparation method of the hydrostatic pressure resistant carbon fiber composite material foam structure of the present invention is simple, the structure has high fabricationability, and can significantly improve the pressure resistance and sound insulation performance of underwater components. Attached Figure Description

[0025] The accompanying drawings are provided for illustrative purposes only, and the proportions and sizes of the parts in the drawings may not be consistent with the actual product.

[0026] Figure 1 This is a block diagram of the disc-shaped foam main body structure in some specific embodiments of the present invention;

[0027] Figure 2 This is a schematic diagram showing the distribution of the foam blocks within the carbon fiber composite foam structure in some specific embodiments of the present invention;

[0028] Figure 3 This is a schematic diagram showing the distribution of the foam blocks covering the underwater pressure-resistant structure in Comparative Example 2 of the present invention.

[0029] In the figure: 1: Inner region; 2: Middle region; 3: Outer region; 4: Radial edge; 5: Carbon fiber composite material layer covering the foam main structure. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0031] In a first aspect, the present invention provides a hydrostatic pressure-resistant carbon fiber composite material-coated foam structure (abbreviated as carbon fiber composite material-coated foam structure or underwater pressure-resistant structure), wherein the carbon fiber composite material-coated foam structure comprises a foam body structure and a carbon fiber composite material layer covering the foam body structure, wherein the foam body structure has 3 to 5 (e.g., 3, 4, or 5) regions radially outward, for example, as... Figure 1 and Figure 2 As shown; each region has multiple covered foam blocks, and the number of covered foam blocks in each region is a. n =2 n+1 n≥1, each foam-coated block includes a foam block and a carbon fiber composite material layer and a film layer sequentially coated on the surface of the foam block; specifically, in this invention, the carbon fiber composite material-coated foam structure is disc-shaped, and each region is divided into a number of a. n =2n+1 The foam block; when the main foam structure has 3 regions radially outward, n takes values ​​of 1, 2, and 3 in sequence; when the main foam structure has 4 regions radially outward, n takes values ​​of 1, 2, 3, and 4 in sequence; when the main foam structure has 5 regions radially outward, n takes values ​​of 1, 2, 3, 4, and 5 in sequence; in this invention, the thickness of the carbon fiber composite material layer covering the surface of the main foam structure and / or the carbon fiber composite material layer covering the surface of the foam block can be, for example, 1.5 to 2.5 mm, preferably 2 mm, and the thickness of the adhesive film layer is, for example, 0.1 to 0.2 mm.

[0032] According to some preferred embodiments, the covered foam blocks are distributed in an overall brick-wall-like structure, for example, as... Figure 2 As shown; in this invention, for a brick wall-type structure, specifically, it means that the radial edges (similar to walls) of the foam blocks in two adjacent areas are staggered, and the outer circumferential arc length of the foam block in the inner area is greater than the inner circumferential arc length of the foam block in the outer area.

[0033] The hydrostatic pressure-resistant carbon fiber composite foam-coated structure provided by this invention can simultaneously meet the requirements of lightweighting, sound insulation, and improved pressure resistance. This hydrostatic pressure-resistant carbon fiber composite foam-coated structure uses foam material as the main material for pressure-resistant components. The main foam structure is rationally divided into sections and foam blocks, which are then sequentially coated with carbon fiber composite material and an adhesive film. The carbon fiber composite material is used to reinforce the structure, thereby improving the overall stiffness and strength of the structural components. More importantly, the distributed distribution of the coated foam blocks forms a brick-wall-like structure that supports the entire pressure-resistant structure, effectively distributing the pressure required by the structure. This helps to evenly disperse underwater hydrostatic pressure, reducing the risk of localized stress concentration. Furthermore, in the brick-wall-like structure, the radial edges of the coated foam blocks in adjacent areas are staggered, which, in addition to effectively distributing the pressure required by the structure, also effectively improves the sound insulation performance of the structure.

[0034] The foam block of this invention comprises a foam block and a carbon fiber composite material layer and a film layer sequentially covering the surface of the foam block. Specifically, the foam block of this invention creatively adds an additional film layer on top of the carbon fiber composite material layer. This film layer, placed on top of the carbon fiber composite material layer, forms an additional sound insulation layer. This sound insulation layer can effectively absorb and reduce the energy of incoming sound waves, thereby weakening sound propagation. This invention also discovers that the film has a certain degree of elasticity and can vibrate to some extent, absorbing the mechanical energy of sound waves. This helps reduce the possibility of sound propagation within the structure. Furthermore, the foam block of this invention, comprising the foam block, the carbon fiber composite material layer, and the film layer, forms multiple barriers. It can reflect, absorb, and scatter sound waves, thereby effectively improving sound insulation. This multi-layer design hinders the free propagation of sound waves and reduces the possibility of sound transmission through the structure. In addition, the present invention found that the film layer can also seal the structure, preventing sound waves from propagating through the gaps between the carbon fiber composite material layers, which also helps to significantly improve the sound insulation effect. This is crucial for sound insulation in underwater applications, because water is an effective medium for sound wave propagation, and even small sound leaks can be propagated over long distances in the underwater environment. The hydrostatic pressure-resistant carbon fiber composite material-coated foam structure in the present invention helps to significantly improve the sound insulation effect of the pressure-resistant structure, which is very important for applications that need to reduce noise or protect sensitive equipment in underwater environments.

[0035] According to some preferred embodiments, the foam main structure has three regions radially outward, namely an inner region, a middle region, and an outer region, in that order. For example, Figure 1 and Figure 2 As shown; the inner region, the middle region, and the outer region each include 4, 8, and 16 covered foam blocks respectively; in this invention, the radial edges of the covered foam blocks in the inner region are offset from the radial edges of the covered foam blocks in the middle region, and the radial edges of the covered foam blocks in the middle region are offset from the radial edges of the covered foam blocks in the outer region. The outer circumferential arc length of the covered foam blocks in the inner region is greater than the inner circumferential arc length of the covered foam blocks in the middle region, and the outer circumferential arc length of the covered foam blocks in the middle region is greater than the inner circumferential arc length of the covered foam blocks in the outer region. The covered foam blocks are distributed in a brick-wall-like structure, for example, as... Figure 2 As shown.

[0036] According to some preferred embodiments, the outer diameter of the intermediate region is 2.4 to 2.8 times (e.g., 2.4, 2.5, 2.6, 2.7, or 2.8 times) the outer diameter of the inner region; the outer diameter of the outer region is 1.4 to 1.6 times (e.g., 1.4, 1.5, or 1.6 times) the outer diameter of the intermediate region; in this invention, preferably, the diameter of the foam body structure is 180 to 250 mm.

[0037] In this invention, preferably, the foam main structure is divided into an inner region, a middle region, and an outer region, with each region having a specific number of covered foam blocks. This partitioning and segmentation helps to evenly distribute the load, providing more uniform support. It allows for gradual addition of support and protection to the structure, ensuring that the structure is not easily damaged under high pressure, thereby improving the overall pressure resistance of the carbon fiber composite-covered foam structure. Preferably, the diameter of the foam main structure is 180–250 mm, the outer diameter of the middle region is 2.4–2.8 times the outer diameter of the inner region, and the outer diameter of the outer region is 1.4–1.6 times the outer diameter of the middle region. The size of the foam main structure and the proportions of the outer diameters of each region ensure that the inner region, middle region, and outer region are properly supported. The consistency of the bearing area of ​​the upper and lower arc surfaces of the segmented foam in the inner and outer regions effectively ensures the compressive strength of the structure, giving it better compressive strength, more effectively resisting external hydrostatic pressure, reducing the risk of damage caused by stress concentration, thereby extending its service life and improving safety. This invention also reveals that, while ensuring consistent outer diameters in the inner regions, if the ratio of the outer diameter of the middle region to the inner region and the ratio of the outer region to the middle region are too small, although this effectively ensures the compressive strength of the structure, it will lead to a reduction in the structure's lightweight performance. Conversely, if the ratio of the outer diameter of the middle region to the inner region and the ratio of the outer region to the middle region are too large, the surface area of ​​the foam main structure is too large, making it prone to crushing under compressive loads, which is not conducive to effectively improving the compressive strength of the structure.

[0038] The present invention provides, in a second aspect, a method (i.e., a molding method) for preparing the hydrostatic pressure-resistant carbon fiber composite material-coated foam structure described in the first aspect of the present invention, the method comprising the following steps:

[0039] (1) Divide the disc-shaped foam (disc-shaped monolithic foam) radially outward into 3 to 5 regions, and further divide each region circumferentially into a... n A block of foam, a n =2 n+1 , n≥1;

[0040] (2) Each foam block is sequentially coated and laid up with carbon fiber composite prepreg and adhesive film, and then placed in a mold for pre-compacting. It is worth noting that in this invention, the carbon fiber composite prepreg is coated with adhesive liquid and adhesive film, and then an additional layer of adhesive film is applied on top of the prepreg coating. Specifically, a layer of adhesive liquid (e.g., J-47B adhesive liquid) is first applied to the surface of the foam block and left to dry at room temperature (20-30°C) for 20-30 minutes, then an adhesive film is applied, followed by the prepreg coating, and then the adhesive film is applied again. In this invention, the preferred thickness of the prepreg and adhesive film is such that the thickness of the carbon fiber composite layer is 1.5-2.5 mm and the thickness of the adhesive film layer is 0.1-0.2 mm.

[0041] (3) The pre-compacted foam blocks in 3 to 5 regions after step (2) are completely covered with carbon fiber composite prepreg, that is, the outer periphery of 3 to 5 regions is completely covered with carbon fiber composite prepreg. After covering, the foam blocks are placed in a mold for molding and curing to obtain a carbon fiber composite foam structure resistant to hydrostatic pressure. In this invention, the carbon fiber composite prepreg covering the pre-compacted foam blocks in 3 to 5 regions forms a carbon fiber composite layer on the surface of the foam main structure after molding and curing. In this invention, the preparation method of the hydrostatic pressure-resistant carbon fiber composite material-coated foam structure is simple, the structure has high fabricationability, and can significantly improve the pressure resistance and sound insulation performance of underwater components. Specifically, the preparation method of this invention divides the foam into blocks according to the specific shape of the structure, and coats the blocks of foam with carbon fiber composite prepreg and film. Finally, the carbon fiber composite prepreg is used to completely coat all the blocks of foam in 3 to 5 regions, and the carbon fiber composite material-coated foam structure is obtained by molding and curing. In this invention, in the carbon fiber composite material-coated foam structure, multiple coated foam blocks in each region form a brick wall-like configuration to provide overall support for the pressure-resistant structure. Since the radial edges (walls) of the coated foam blocks in different regions of the brick wall-like structure are staggered, the sound insulation performance of the structure can be effectively improved.

[0042] According to some preferred embodiments, the carbon fiber composite prepreg is made by impregnating carbon fibers with epoxy resin; the carbon fibers are unidirectional T300, T700, T800, or T1000 carbon fibers; the epoxy resin is a medium-low temperature curing epoxy resin or a high temperature curing epoxy resin; in some specific embodiments, the carbon fiber composite prepreg may be, for example, T800 / 9368 prepreg (T800 / 9368 unidirectional epoxy resin prepreg), and the adhesive film is J-47A adhesive film; the foam is PMI foam, and in some specific embodiments, the foam used has, for example, a density of 200 kg / m³. 3The Zhaosai series PMI foam has a compressive strength of 6MPa.

[0043] According to some preferred embodiments, the pre-compression is performed by holding the pressure at a temperature of 60-80°C (e.g., 60°C, 70°C, or 80°C) and a pressure of 2-4 MPa (e.g., 2, 3, or 4 MPa) for 10-30 minutes (e.g., 10, 15, 20, 25, or 30 minutes).

[0044] According to some preferred embodiments, the material is molded and cured for 2 to 4 hours (e.g., 2, 3 or 4 hours) at a temperature of 100 to 140°C (e.g., 100°C, 110°C, 120°C, 130°C or 140°C) and a pressure of 5 to 6 MPa (e.g., 5, 5.5 or 6 MPa).

[0045] According to some preferred embodiments, based on the pressure resistance requirements, the static simulation of the carbon fiber composite foam structure resistant to hydrostatic pressure is performed using simulation software to verify the pressure resistance performance of the components and check the pressure resistance strength of the structure. The carbon fiber composite foam structure and material parameters are gradually optimized to obtain an optimized carbon fiber composite foam structure resistant to hydrostatic pressure.

[0046] According to some preferred embodiments, the static simulation method uses 3D modeling software to model each component of the fiber composite foam structure, establishes a finite element model using simulation software, and performs loading analysis. Specifically, the static simulation includes the following steps:

[0047] (a) Establish a solid model of a carbon fiber composite material foam structure resistant to hydrostatic pressure, import the established solid model into simulation software to establish a finite element model, and assemble it into an assembly.

[0048] (b) Assign material properties to each component separately, establish a compressive failure criterion, apply a given compressive load, and perform analysis;

[0049] (c) Adjust key structural and material parameters based on the results of finite element simulation to optimize the design; the adjustment includes adjusting the thickness and layup of carbon fiber composite materials or using carbon fiber composite materials or foams with better performance; the simulation results include stress distribution cloud maps and failure coefficient cloud maps under a given compressive load, and determine whether the structure fails under a given strength criterion; the optimal solution of the design structure is obtained through step-by-step iterative design.

[0050] Based on specific implementation methods, and building upon the innovative structural features and advantages of the carbon fiber composite-coated foam structure obtained in this invention, the compressive strength characteristics of the carbon fiber composite material in the carbon fiber composite-coated foam structure are further optimized through static simulation, including the layup thickness and material selection. The specific process for analyzing and optimizing the compressive strength characteristics is as follows:

[0051] First, a solid model of the structural component is established, and the initial design thickness of the carbon fiber composite layer is assigned. A finite element model is then established for the solid model. The solid model of the structure is established using NX UG software. The three-dimensional model of the structure is then imported into Abaqus software to generate a mesh and perform analysis. The foam part is divided into CSD8R solid elements, and the carbon fiber composite material is divided into S8R shell elements.

[0052] Secondly, after the finite element model is established, material parameters and physical properties are set for the model.

[0053] The pressure resistance analysis requires the application of a failure criterion for the carbon fiber composite material, specifically the Cai-Wu failure criterion. The foam component's failure is determined based on the selected foam material's pressure resistance test data. Under a given compressive load, a static strength analysis is performed on the carbon fiber composite-coated foam structure. The results are then used to extract the maximum principal stress cloud map of the foam component and the Cai-Wu failure coefficient cloud map of the carbon fiber composite component.

[0054] Optimize the geometry and material parameters of carbon fiber composite-coated foam structures. Increase or decrease the load-bearing capacity of the carbon fiber composite by increasing or decreasing the thickness of the carbon fiber composite layup. Improve material utilization by selecting higher or lower strength grades of foam materials to enhance or reduce the load-bearing capacity of the foam material.

[0055] Finally, the load-bearing capacity of the new carbon fiber composite foam structure under a given compressive load was solved using Abaqus, verifying that its load-bearing performance met the requirements and obtaining an optimized design scheme.

[0056] The present invention will be further described below with reference to the embodiments. These embodiments are merely illustrative examples of preferred implementations of the present invention, and the scope of protection of the present invention should not be construed as being limited to these embodiments.

[0057] Example 1

[0058] This embodiment provides a carbon fiber composite material-coated foam structure resistant to hydrostatic pressure. The carbon fiber composite material-coated foam structure includes a disc-shaped foam body structure and a carbon fiber composite material layer covering the foam body structure. The foam body structure has three regions radially outward: an inner region, a middle region, and an outer region, in that order. For example, ... Figure 1 and Figure 2 As shown, each region has multiple covered foam blocks, and the number of covered foam blocks in each region is a. n =2 n+1n≥1, meaning the number of covered foam blocks included in the inner region, the middle region, and the outer region are 4, 8, and 16 respectively; each covered foam block includes a foam block and a carbon fiber composite material layer and a film layer sequentially covering the surface of the foam block. The carbon fiber composite material layer is formed by coating the surface of the foam block with carbon fiber composite prepreg through adhesive and film; the thickness of the carbon fiber composite material layer covering the surface of the foam main structure and the carbon fiber composite material layer covering the foam block are both 2mm, and the thickness of the film layer covering the carbon fiber composite material layer is 0.2mm; the covered foam blocks are distributed in a brick wall-like structure. Specifically, the number of covered foam blocks included in the inner region is... The radial edges are offset from the radial edges of the foam blocks included in the middle region, and the radial edges of the foam blocks included in the middle region are offset from the radial edges of the foam blocks included in the outer region. The outer circumferential arc length of the foam blocks included in the inner region is greater than the inner circumferential arc length of the foam blocks included in the middle region, and the outer circumferential arc length of the foam blocks included in the middle region is greater than the inner circumferential arc length of the foam blocks included in the outer region. The foam blocks are distributed in a brick wall-like structure. The diameter of the foam main structure is 200mm. The outer diameter of the middle region is 2.5 times the outer diameter of the inner region, and the outer diameter of the outer region is 1.5 times the outer diameter of the middle region.

[0059] The preparation process of the hydrostatic pressure-resistant carbon fiber composite material-coated foam structure provided in this embodiment is as follows:

[0060] Step 1: As Figure 1 As shown, the disc-shaped foam is first divided into three regions along the radial direction: the outermost region (outer region) is divided into 16 blocks along the circumference, the middle layer region (middle region) is divided into 8 blocks along the circumference, and the innermost region (inner region) is divided into 4 blocks along the circumference.

[0061] Step Two: Each foam block, after being divided into sections, is sequentially covered and layered with carbon fiber composite prepreg and adhesive film, as follows: Figure 2 As shown, after coating, it is placed in a matching molding die and the die is closed. Then the die is placed in a press and pre-compacted at 80°C and 4MPa for 30 minutes. Specifically, a layer of J-47B adhesive with a thickness of 0.1mm is first coated on the surface of the foam block and left to dry at room temperature of 25°C for 20 minutes. Then a layer of J-47A adhesive film with a thickness of 0.2mm is applied. Then carbon fiber composite prepreg is wrapped, and then another layer of J-47A adhesive film with a thickness of 0.2mm is wrapped.

[0062] Step 3: The pre-compacted foam blocks in three areas are completely encapsulated with carbon fiber composite prepreg. After encapsulation, they are placed in matching molding dies and closed. The dies are then placed in a press and cured at 130℃ and 6MPa for 2 hours to obtain a hydrostatically resistant carbon fiber composite-encapsulated foam structure. This structure includes a main foam structure and a 2mm thick carbon fiber composite layer covering the main foam structure. In this embodiment, the carbon fiber composite prepreg is T800 / 9368, the adhesive film is J-47A, and the disc-shaped foam uses PMI foam with a density of 200kg / m³. 3 The compressive strength is 6 MPa.

[0063] Example 2

[0064] Example 2 is basically the same as Example 1, except that:

[0065] In the hydrostatic pressure resistant carbon fiber composite foam structure provided in this embodiment, the outer diameter of the inner region is the same as that of the inner region in Embodiment 1, the outer diameter of the middle region is twice that of the inner region, and the outer diameter of the outer region is once that of the middle region.

[0066] In this embodiment, the ratio of the outer diameter of the middle region to the outer diameter of the inner region and the ratio of the outer diameter of the middle region are too small. Although this can effectively ensure the pressure resistance of the structure, the reduced surface area of ​​the foam main structure and the smaller overall material used in the foam blocks result in an excessive proportion of carbon fiber composite materials, which in turn reduces the lightweight performance of the structure.

[0067] Example 3

[0068] Example 3 is basically the same as Example 1, except that:

[0069] In the hydrostatic pressure resistant carbon fiber composite foam structure provided in this embodiment, the outer diameter of the inner region is the same as that of the inner region in Embodiment 1, the outer diameter of the middle region is 3 times that of the inner region, and the outer diameter of the outer region is 2 times that of the middle region.

[0070] Comparative Example 1

[0071] This comparative example provides an underwater pressure-resistant structure, which is disc-shaped. The underwater pressure-resistant structure includes a disc-shaped foam main body structure and a carbon fiber composite material layer covering the foam main body structure. The foam main body structure has three radially outward regions: an inner region, a middle region, and an outer region. The number of foam-covered blocks included in the inner region, the middle region, and the outer region are 4, 8, and 16 respectively. Each foam-covered block includes a foam block and a carbon fiber composite material layer covering the surface of the foam block. The carbon fiber composite material layer is formed by coating the surface of the foam block with an adhesive and an adhesive film. The thickness of both the carbon fiber composite material layer covering the surface of the foam main body structure and the carbon fiber composite material layer covering the foam block is 2 mm. The distribution of each foam-covered block is as follows: The overall structure forms a brick wall-like structure. Specifically, the radial edges of the foam blocks in the inner region are offset from the radial edges of the foam blocks in the middle region, and the radial edges of the foam blocks in the middle region are offset from the radial edges of the foam blocks in the outer region. The outer circumferential arc length of the foam blocks in the inner region is greater than the inner circumferential arc length of the foam blocks in the middle region, and the outer circumferential arc length of the foam blocks in the middle region is greater than the inner circumferential arc length of the foam blocks in the outer region. The distribution of the foam blocks forms a brick wall-like structure. The diameter of the four foam blocks divided in the inner region is the same as in Example 1. The outer diameter of the middle region is 2.5 times the outer diameter of the inner region, and the outer diameter of the outer region is 1.5 times the outer diameter of the middle region.

[0072] The fabrication process of the underwater pressure-resistant structure provided in this comparative example is as follows:

[0073] Step 1: As Figure 1 As shown, the disc-shaped foam is first divided into three regions along the radial direction: the outermost region (outer region) is divided into 16 blocks along the circumference, the middle layer region (middle region) is divided into 8 blocks along the circumference, and the innermost region (inner region) is divided into 4 blocks along the circumference.

[0074] Step 2: Each foam block after being divided into sections is covered and laid with carbon fiber composite prepreg. After covering, it is placed in a matching molding die and closed. Then, the die is placed in a press and pre-compacted at 80°C and 4MPa for 30 minutes. Specifically, a 0.1mm thick layer of J-47B adhesive is first coated on the surface of the foam block and left to dry at room temperature (25°C) for 20 minutes. Then, a 0.2mm thick layer of J-47A adhesive film is applied, followed by covering with carbon fiber composite prepreg.

[0075] Step 3: The pre-compacted foam blocks in the three regions are completely covered with carbon fiber composite prepreg. After covering, they are placed in matching molding molds and closed. Then, the molds are placed in a press and cured at 130℃ and 6MPa for 2 hours to obtain an underwater pressure-resistant structure. The underwater pressure-resistant structure includes a foam main structure and a 2mm thick carbon fiber composite layer covering the foam main structure. In this comparative example, the carbon fiber composite prepreg is T800 / 9368 prepreg; the disc-shaped foam uses PMI foam with a density of 200kg / m³. 3 The compressive strength is 6 MPa.

[0076] Comparative Example 2

[0077] This comparative example provides an underwater pressure-resistant structure, which is disc-shaped. The underwater pressure-resistant structure includes a disc-shaped foam main body structure and a carbon fiber composite material layer covering the foam main body structure. The foam main body structure has three regions radially outward: an inner region, a middle region, and an outer region. The number of foam blocks included in the inner region, the middle region, and the outer region are 4, 8, and 16 respectively. Each foam block includes a foam block and a carbon fiber composite material layer and a film layer sequentially covering the surface of the foam block. The carbon fiber composite material layer is formed by coating the surface of the foam block with carbon fiber composite prepreg using an adhesive and a film. The thickness of both the carbon fiber composite material layer covering the surface of the foam main body structure and the carbon fiber composite material layer covering the foam block is 2 mm. The thickness of the adhesive film layer covering the composite material layer is 0.2 mm. The outer circumferential arc length of one covered foam block in the inner region is equal to the sum of the inner circumferential arc lengths of the two covered foam blocks in the middle region. In the middle region, the radial edge of each pair of adjacent covered foam blocks corresponds to the radial edge of the covered foam block in the inner region. The outer circumferential arc length of one covered foam block in the middle region is equal to the sum of the inner circumferential arc lengths of the two covered foam blocks in the outer region. In the outer region, the radial edge of each pair of adjacent covered foam blocks corresponds to the radial edge of the covered foam block in the middle region. The diameter of the foam main structure is 200 mm. The outer diameter of the middle region is 2.5 times the outer diameter of the inner region, and the outer diameter of the outer region is 1.5 times the outer diameter of the middle region. The preparation process of the underwater pressure-resistant structure provided in this comparative example is as follows:

[0078] Step 1: According to the design of the underwater pressure-resistant structure, the disc-shaped foam is first divided into three areas along the radial direction. The outermost area (outer area) is divided into 16 pieces along the circumference, the middle layer area (middle area) is divided into 8 pieces along the circumference, and the innermost area (inner area) is divided into 4 pieces along the circumference.

[0079] Step Two: Each foam block, after being divided into sections, is sequentially covered and layered with carbon fiber composite prepreg and adhesive film, as follows: Figure 3 As shown, after coating, it is placed in a matching molding die and the die is closed. Then the die is placed in a press and pre-compacted at 80°C and 4MPa for 30 minutes. Specifically, a layer of J-47B adhesive with a thickness of 0.1mm is first coated on the surface of the foam block and left to dry at room temperature of 25°C for 20 minutes. Then a layer of J-47A adhesive film with a thickness of 0.2mm is applied. Then carbon fiber composite prepreg is wrapped, and then another layer of J-47A adhesive film with a thickness of 0.2mm is wrapped.

[0080] Step 3: The pre-compacted foam blocks in the three regions are completely covered with carbon fiber composite prepreg. After covering, they are placed in matching molding molds and closed. Then, the molds are placed in a press and cured at 130℃ and 6MPa for 2 hours to obtain an underwater pressure-resistant structure. The underwater pressure-resistant structure includes a foam main structure and a 2mm thick carbon fiber composite layer covering the foam main structure. In this comparative example, the carbon fiber composite prepreg is T800 / 9368 prepreg, the adhesive film is J-47A adhesive film, and the disc-shaped foam uses PMI foam with a density of 200kg / m³. 3 The compressive strength is 6 MPa.

[0081] The present invention conducted performance tests on the carbon fiber composite foam-coated structures obtained in each embodiment and the underwater pressure-resistant structures obtained in each comparative example. The test results are shown in Table 1. Among them, the hydrostatic pressure resistance was measured with reference to the test standard GB / T4744, and the average sound transmission coefficient (average sound pressure transmission coefficient) was measured with reference to the test standard GB / T 32523-2016. In the present invention, the smaller the average sound transmission coefficient, the better the sound insulation effect.

[0082] Table 1

[0083]

[0084] In Table 1, the symbol " / " indicates that the performance metric was not tested.

[0085] The parts of this invention not described in detail are techniques known to those skilled in the art.

[0086] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in each embodiment, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a hydrostatic pressure-resistant carbon fiber composite material-coated foam structure, characterized in that, The method includes the following steps: (1) Divide the disc-shaped foam into 3 to 5 regions radially outward, and divide each region into a circumferential division. n A block of foam, a n =2 n+1 , n≥1; (2) Each foam block is coated and laid with carbon fiber composite prepreg and film in sequence, and then placed in a mold for pre-compacting after coating; (3) The pre-compacted foam blocks in 3-5 regions are completely covered with carbon fiber composite prepreg, and then placed in a mold for molding and curing to obtain a carbon fiber composite covered foam structure resistant to hydrostatic pressure; the carbon fiber composite covered foam structure includes a foam body structure and a carbon fiber composite layer covering the foam body structure. The foam body structure has 3-5 regions radially outward, and each region has multiple covered foam blocks. The number of covered foam blocks in each region is a. n =2 n+1 , n≥1, each foam block includes a foam block and a carbon fiber composite material layer and a film layer sequentially covering the surface of the foam block.

2. The preparation method according to claim 1, characterized in that: The distribution of each encapsulated foam block forms a brick wall-like structure.

3. The preparation method according to claim 1, characterized in that: The foam main structure has three regions radially outward: an inner region, a middle region, and an outer region. The inner region, the middle region, and the outer region each contain 4, 8, and 16 foam blocks, respectively.

4. The preparation method according to claim 3, characterized in that: The outer diameter of the intermediate region is 2.4 to 2.8 times the outer diameter of the inner region; The outer diameter of the outer region is 1.4 to 1.6 times the outer diameter of the middle region.

5. The preparation method according to claim 1, characterized in that: The carbon fiber composite prepreg is made by impregnating carbon fibers with epoxy resin; The carbon fiber used is unidirectional T300, T700, T800 or T1000 carbon fiber; The epoxy resin used is a medium-low temperature curing epoxy resin or a high temperature curing epoxy resin. The foam is PMI foam.

6. The preparation method according to claim 1, characterized in that: The pre-compression is actually a pressure holding process at a temperature of 60~80℃ and a pressure of 2~4MPa for 10~30 minutes.

7. The preparation method according to claim 1, characterized in that: The material is molded and cured for 2-4 hours at a temperature of 100-140℃ and a pressure of 5-6MPa.

8. The preparation method according to claim 1, characterized in that: Based on the pressure resistance requirements, static simulation of the carbon fiber composite foam structure with hydrostatic pressure resistance was performed using simulation software to obtain an optimized carbon fiber composite foam structure with hydrostatic pressure resistance.

9. The preparation method according to claim 8, characterized in that, The static simulation includes the following steps: (a) Establish a solid model of a carbon fiber composite material foam structure resistant to hydrostatic pressure, and import the established solid model into simulation software to establish a finite element model; (b) Assign material properties to each component separately, establish a compressive failure criterion, apply a given compressive load, and perform analysis; (c) Adjust key structural and material parameters based on the results of finite element simulation to optimize the design; the adjustment includes adjusting the thickness and layup of carbon fiber composite materials or using carbon fiber composite materials or foams with better performance; the simulation results include stress distribution cloud maps and failure coefficient cloud maps under a given compressive load, and determine whether the structure fails under a given strength criterion; the optimal solution of the design structure is obtained through step-by-step iterative design.

Citation Information

Patent Citations

  • Composite dot-matrix interlayer double-skin cylindrical shell structure with metal liner for bearing inner pressure and preparation process thereof