A surface-modified heterojunction nanoarray electrode and a preparation method and application thereof

By constructing a heterojunction nanoarray electrode of transition metal and cerium oxide on a current collector and modifying it with a silane coupling agent, the problems of activity and mass transfer efficiency of non-noble metal catalytic materials were solved, and the catalytic performance of organic electrosynthesis was improved.

CN117431584BActive Publication Date: 2026-11-20SUN YAT SEN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311331080.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-13
Publication Date
2026-11-20
Estimated Expiration
2043-10-13

AI Technical Summary

Technical Problem

Existing non-precious metal organocatalytic materials have limited catalytic activity, poor reaction kinetics, and low mass transfer efficiency, which affect the efficiency and cost of organic electrosynthesis.

Method used

By growing a heterojunction nanoarray of transition metal matrix and cerium oxide in situ on the current collector and modifying it with a silane coupling agent, the electronic structure and organic group fragments of the catalytic material are optimized, thereby improving catalytic activity and mass transfer efficiency.

Benefits of technology

This enables an organic electrosynthesis process with high catalytic activity and excellent reaction kinetics, improving the efficiency of organic electro-oxidation and electro-reduction reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117431584B_ABST
    Figure CN117431584B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of organic electro-synthesis electrode materials, and particularly relates to a surface-modified heterojunction nano-array electrode and a preparation method and application thereof. The application takes a current collector as a carrier, in-situ grows a nano-array precursor through a solvothermal reaction, and then performs high-temperature gas-solid chemical conversion and subsequent silane coupling agent grafting modification to obtain a surface-modified heterojunction nano-array electrode material. The construction of a heterojunction in the material can adjust and optimize the electronic structure of a catalytic center, and improve catalytic activity. At the same time, the surface-modified organic group fragments are beneficial to the enrichment of organic substrates on the surface of the catalytic material, thereby strengthening the mass transfer of the organic substrates in the organic electro-synthesis process. The obtained surface-modified heterojunction nano-array electrode can exhibit high mass transfer efficiency and excellent catalytic activity when applied to a series of organic electro-synthesis reactions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of organic electrosynthesis electrode materials. More specifically, it relates to a surface-modified heterojunction nanoarray electrode, its preparation method, and its application. Background Technology

[0002] Organic electrosynthesis utilizes electrical energy to drive redox reactions of organic compounds. At the anode, it can achieve the electrooxidation of alcohols, aldehydes, ketones, and amines; at the cathode, it can achieve the electroreduction of nitro compounds, halogenated compounds, carboxylic acid compounds, and unsaturated hydrocarbons. Organic electrosynthesis avoids the use of expensive and toxic oxidizing and reducing agents and the harsh reaction conditions required in traditional chemical synthesis. Furthermore, the selectivity and rate of the reaction can be precisely controlled by adjusting the current and potential. In addition, the electricity required for organic electrosynthesis can be supplied by renewable energy sources such as solar energy, making it a green and environmentally friendly technology that meets the requirements of "atom economy" and is one of the important directions for future development. Currently, in the field of organic electrosynthesis, noble metal-based catalysts exhibit excellent catalytic activity. For example, Chinese patent application CN113328105A discloses a method for preparing a heterostructured platinum nanoparticle array modified electrode. The electrode prepared using the noble metals platinum and gold shows good catalytic oxidation effects for methanol. However, the low reserves, high cost, and susceptibility to poisoning and deactivation of precious metals hinder their practical application. Therefore, it is urgent to develop organic electrosynthesis catalysts with excellent electrocatalytic performance, high selectivity, and strong stability based on non-precious metals.

[0003] In recent years, numerous non-noble metal-based transition metal catalytic materials have been applied in the field of organic electrosynthesis due to their certain catalytic activity and low cost. However, the problem of insufficient activity due to unoptimized electronic structures remains. Furthermore, the low diffusion coefficient and / or solubility of organic substrates lead to low mass transfer efficiency, which in turn affects catalytic performance. Therefore, developing low-cost transition metal catalytic materials that combine optimized surface electronic structure, rapid reaction kinetics, and excellent mass transfer efficiency to achieve high-performance organic electro-oxidation / electro-reduction is of great significance for the large-scale application of organic electrosynthesis technology. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of existing non-noble metal organocatalytic materials, such as limited catalytic activity, poor reaction kinetics and low mass transfer efficiency, and to provide a method for preparing a surface-modified heterojunction nanoarray electrode with high catalytic activity, excellent reaction kinetics and mass transfer efficiency.

[0005] The purpose of this invention is to provide a surface-modified heterojunction nanoarray electrode prepared by the aforementioned preparation method.

[0006] Another objective of this invention is to provide the application of the surface-modified heterojunction nanoarray electrode in the field of organic electrosynthesis.

[0007] The above-mentioned objective of this invention is achieved through the following technical solution:

[0008] A method for fabricating a surface-modified heterojunction nanoarray electrode specifically includes the following steps:

[0009] S1. The current collector is placed in a mixed solution containing a precipitant, cerium salt and other transition metal salts, and a solvothermal reaction is carried out at 50-250℃ to obtain a hydroxide nanoarray precursor grown in situ on the current collector.

[0010] S2. Take the nanoarray precursor obtained in step S1, place it in an inert gas atmosphere, add a heat conversion source material, and carry out a high-temperature gas-solid purging reaction at 250-800℃ to obtain a heterojunction nanoarray material composed of transition metal matrix and cerium oxide composite.

[0011] S3. Take the heterojunction nanoarray material composed of transition metal matrix and cerium oxide obtained in step S2 and place it in a solvent containing silane coupling agent. Stir to perform grafting modification, wash and dry to obtain heterojunction nanoarray electrode (TMX / CeO2@SCA) with silane coupling agent surface modification.

[0012] On the one hand, the construction of transition metal-based compounds and cerium oxide heterostructures modulates the electronic structure of the surface catalytic active centers, thereby improving the catalytic activity of the catalytic material. On the other hand, the surface-modified silane coupling agent has abundant organic group fragments, which promotes the enrichment of organic substrates on the surface of the catalytic material, thereby enhancing the mass transfer kinetics of organic materials during organic electrosynthesis.

[0013] Furthermore, in step S1, the transition metal in the transition metal salt is selected from at least one of Ni, Cu, Co, Zn, Fe, Mn, Mo, Zr, W, Sc, Ti, V, Cr, Y, Nb, Tc, and Cd.

[0014] Preferably, in step S1, the transition metal in the transition metal salt is selected from at least one of Fe, Mn, Co, Ni, Cu, Mo, W, and V.

[0015] Further, in step S1, the cerium salt and other transition metal salts are selected from one or more of nitrates, acetates, chlorides, carbonates, and sulfates.

[0016] Further, in step S1, the precipitant is selected from at least one of sodium hydroxide, potassium hydroxide, ammonia, sodium carbonate, sodium bicarbonate, urea, hexamethylenetetramine, and sodium oxalate.

[0017] Further, in step S1, the total concentration of the cerium salt and other transition metal salts is 1 to 2000 mM; preferably, the total concentration of the cerium salt and other transition metal salts is 2 to 2000 mM; specifically, it can be 2 mM, 5 mM, 10 mM, 20 mM, 50 mM, 100 mM, 200 mM, 500 mM, 1000, or 2000 mM.

[0018] Further, in step S1, the molar ratio of the cerium salt to other transition metal salts is 1:(1-49); preferably, the molar ratio of the cerium salt to the transition metal salts is 1:(4-49); specifically, it can be 1:4, 1:9, 1:19, or 1:49.

[0019] Furthermore, in step S1, the molar ratio of the transition metal salt to the precipitant is 1:(1-20); preferably, the molar ratio of the transition metal salt to the precipitant is 1:(1-16); specifically, it can be 1:1, 1:2, 1:4, 1:8, or 1:16.

[0020] Further, in step S1, the current collector is carbon cloth, carbon paper, or a metal current collector; preferably, the metal current collector is metal foam, metal foil, metal plate, or metal mesh; more preferably, the metal of the metal current collector is Fe, Co, Ni, Cu, Zn, Al, Ti, or stainless steel.

[0021] Further, in step S1, the solvothermal reaction temperature is 50–250°C; preferably, it can be 60–200°C; specifically, it can be 60°C, 80°C, 100°C, 120°C, 150°C, 180°C, or 200°C.

[0022] Furthermore, in step S1, the solvothermal reaction time can be 1 to 96 hours; specifically, it can be 1 hour, 2 hours, 5 hours, 8 hours, 12 hours, 24 hours, 48 ​​hours, or 96 hours.

[0023] Further, in step S2, the heat conversion source material is a nitrogen source, a phosphorus source, a sulfur source, a selenium source, or a tellurium source; preferably, the nitrogen source is urea, the phosphorus source is sodium hypophosphite or red phosphorus, the sulfur source is sulfur powder, the selenium source is selenium powder, and the tellurium source is tellurium powder.

[0024] Further, in step S2, the inert gas is selected from at least one of nitrogen (N2), argon (Ar), and helium (He).

[0025] Furthermore, in step S2, the gas flow rate of the inert gas is 1 to 100 mL / min; preferably, the gas flow rate of the inert gas is 1 to 70 mL / min; specifically, it can be 2 mL / min, 5 mL / min, 10 mL / min, 15 mL / min, 30 mL / min, or 70 mL / min.

[0026] Preferably, in step S2, the temperature of the high-temperature gas-solid purging reaction can be 250℃, 300℃, 350℃, 400℃, 500℃, 600℃, 700℃, or 800℃.

[0027] Furthermore, the high-temperature gas-solid purging reaction time is 1 to 24 hours; preferably, the high-temperature gas-solid purging reaction time is 1 to 8 hours; specifically, it can be 1 hour, 2 hours, 4 hours, 6 hours, or 8 hours.

[0028] Furthermore, in step S2, the mass ratio of the nanoarray precursor to the heat conversion source material is 1:(1-200); preferably, the mass ratio of the nanoarray precursor to the heat conversion source material is 1:(1-150); specifically, it can be 1:1, 1:5, 1:10, 1:20, 1:50, 1:100, or 1:150.

[0029] Further, in step S2, the heating rate of the high-temperature gas-solid purging reaction is 1-20℃ / min; preferably, the heating rate of the high-temperature gas-solid purging reaction is 1-10℃ / min; specifically, it can be 2℃ / min, 3℃ / min, 5℃ / min, or 8℃ / min.

[0030] Further, in step S3, the silane coupling agent is selected from at least one of vinyltriethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-ureidopropyltrimethoxysilane, epoxybutyltrimethoxysilane, phenyltrimethoxysilane, 9-anthrayltrimethoxysilane, n-decyltrimethoxysilane, dodecyltrimethoxysilane, dimethyldiethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 5-bromopentyltrimethoxysilane, n-decyltrichlorosilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, and 3-isocyanate-propyltrimethoxysilane.

[0031] Further, in step S3, the solvent used for the modification of the silane coupling agent is selected from one or more of water, methanol, ethanol, isopropanol, ethylene glycol, 1,4-butanediol, 1,2,4-butanetriol, 1,6-hexanediol, pentanediol, glycerol, toluene, acetonitrile, acetone, methyl acetate, and ethyl acetate.

[0032] Further, in step S3, the grafting modification temperature is 25-150℃; preferably, it can be 30-80℃; specifically, it can be 30℃, 40℃, 50℃, 60℃, 70℃, or 80℃.

[0033] Further, in step S3, the grafting modification time is 0.5 to 48 hours; preferably, it is 2 to 24 hours; specifically, it can be 2 hours, 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, 18 hours, or 24 hours.

[0034] Furthermore, in step S3, the volume percentage of the silane coupling agent in the solvent is 0.01-30%; preferably, it can be 0.1-10%; specifically, it can be 0.1%, 0.2%, 0.5%, 1%, 2%, 3%, 5%, or 10%.

[0035] Furthermore, this invention also claims protection for the surface-modified heterojunction nanoarray electrode prepared by the aforementioned preparation method.

[0036] Furthermore, the present invention also claims protection for the application of the surface-modified heterojunction nanoarray electrode in organic electrosynthesis reactions.

[0037] Preferably, the organic electrosynthesis reaction includes the electrooxidation reaction of organic alcohols, aldehydes, ketones, and amines and / or the electroreduction reaction of nitro compounds, carbonyl compounds, and unsaturated hydrocarbons.

[0038] The present invention has the following beneficial effects:

[0039] This invention utilizes a current collector as a carrier to grow a nanoarray precursor in situ on the carrier via a solvothermal reaction. Following this, a high-temperature gas-solid purging reaction yields a heterojunction nanoarray material composed of a transition metal-based compound and cerium oxide. Finally, silane coupling agent grafting modification is applied to obtain a silane coupling agent-modified heterojunction nanoarray electrode. On one hand, the construction of the heterojunction interface between the transition metal-based compound and cerium oxide regulates the electronic structure of the surface catalytic active centers, enhancing the catalytic activity of the material. On the other hand, the surface-modified silane coupling agent possesses abundant organic group fragments, which can promote the enrichment of organic substrates on the catalytic material surface, thereby strengthening the mass transfer kinetics of organic materials during organic electrosynthesis. Based on these structural advantages, the resulting surface-modified heterojunction nanoarray electrode exhibits excellent catalytic performance for a series of organic electrooxidation and electroreduction reactions. Attached Figure Description

[0040] Figure 1 The NiTe / CeO2@C prepared in Example 1 10 H 21 SEM image of Cl3Si heterojunction nanoarray electrode.

[0041] Figure 2 The COVP / CeO2@C7H prepared in Example 2 15 SEM image of NO4Si heterojunction nanoarray electrode.

[0042] Figure 3 The CuWN / CeO2@C8H prepared in Example 3 19 SEM image of BrO3Si heterojunction nanoarray electrode.

[0043] Figure 4 The NiMnSe / CeO2@C prepared in Example 4 17 H 18 SEM image of O3Si heterojunction nanoarray electrode.

[0044] Figure 5 The FeCrP / CeO2@C prepared in Example 5 15 H 34 SEM image of O3Si heterojunction nanoarray electrode.

[0045] Figure 6 The NiYS / CeO2@C7H prepared in Example 6 18 SEM image of N2O4Si heterojunction nanoarray electrode.

[0046] Figure 7 The LSV diagrams show the electro-oxidation reaction of benzyl alcohol at room temperature using array electrodes in Example 1 and Comparative Examples 1 and 2.

[0047] Figure 8 The LSV diagrams show the electro-oxidation reaction of 5-hydroxymethylfurfural (5-HMF) with array electrodes at room temperature in Examples 2, 3, and 4.

[0048] Figure 9 The LSV diagrams show the electro-oxidation reaction of cyclohexanone at room temperature using array electrodes in Examples 3, 5, and 6.

[0049] Figure 10 The LSV diagrams for the electro-oxidation reaction of benzylamine at room temperature are shown for the array electrodes of Example 4, Comparative Examples 7 and 8.

[0050] Figure 11 The LSV diagrams show the electroreduction reaction of nitrobenzene at room temperature using array electrodes in Examples 5, 9, and 10.

[0051] Figure 12 The LSV diagrams for the benzaldehyde electroreduction reaction at room temperature are shown for the array electrodes of Example 6, Comparative Examples 11 and 12. Detailed Implementation

[0052] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.

[0053] Unless otherwise specified, all reagents and materials used in the following examples are commercially available.

[0054] Example 1: NiTe / CeO2@C 10 H 21 Cl3Si heterojunction nanoarray electrode

[0055] The NiTe / CeO2@C 10 H 21 The preparation method of Cl3Si heterojunction nanoarray electrode includes the following steps:

[0056] S1. 0.995 g (4 mmol) nickel acetate tetrahydrate (NiC4H6O4·4H2O), 0.317 g (1 mmol) cerium acetate hydrate (Ce(CH3CO2)3·xH2O) and 1.402 g (10 mmol) hexamethylenetetramine (HMTA) were dissolved in 20 mL of ultrapure water and stirred thoroughly on a stirrer for 0.5 h (stirrer speed 500 rpm) to obtain a mixed solution. The solution was then immersed in two 1×3 cm pretreated titanium mesh (TM), transferred to a high-pressure reactor, sealed, and placed in a forced-air drying oven for solvothermal reaction at 120 °C for 8 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed three times with ultrapure water and anhydrous ethanol, and then dried in a forced-air drying oven at 60 °C for 12 h to obtain the NiCe-OH nanoarray precursor loaded on the TM current collector.

[0057] S2. Place the NiCe-OH nanoarray precursor loaded with TM current collector obtained in step S1 in the downstream of a tube furnace, place tellurium source tellurium powder in the upstream, the mass ratio of NiCe-OH to tellurium source tellurium powder is 1:10, the N2 flow rate is controlled at 5 mL / min, the temperature is increased from room temperature to 800℃ at a heating rate of 5℃ / min, heat-treated at 800℃ for 2 h, and after natural cooling, NiTe / CeO2 heterojunction nanoarray loaded on TM current collector is obtained.

[0058] S3. Immerse the NiTe / CeO2 heterojunction nanoarray loaded on the TM current collector obtained in step S2 into 0.5% n-decyltrichlorosilane (C) solvent with toluene as the solvent. 10 H 21 In a Cl3Si solution, after graft modification at 60℃ for 12 h, the grafted material was washed three times with ethanol and dried in a forced-air drying oven at 60℃ for 6 h to obtain NiTe / CeO2@C supported on a TM current collector. 10 H21 Cl3Si heterojunction nanoarray electrode.

[0059] Material characterization:

[0060] The obtained product was characterized by SEM to obtain the material morphology. Figure 1 As can be seen from the figure, there is a uniformly distributed nanosheet structure on the TM current collector.

[0061] Example 2: CoVP / CeO2@C7H 15 NO4Si heterojunction nanoarray electrode

[0062] The CoVP / CeO2@C7H 15 The fabrication method of NO4Si heterojunction nanoarray electrode includes the following steps:

[0063] S1. Dissolve 0.494 g (1.76 mmol) cobalt sulfate heptahydrate (CoSO4·7H2O), 0.033 g (0.2 mmol) vanadium oxysulfate hydrate (VOSO4·xH2O), 0.016 g (0.04 mmol) cerium sulfate tetrahydrate (Ce(SO4)2·4H2O) and 1.92 g (32 mmol) urea (CH4N2O) in 15 mL of ultrapure water. Stir the mixture thoroughly for 2 h (400 rpm) to obtain a mixed solution. Immerse the solution in two 1×3 cm pretreated stainless steel (SS) sheets, transfer the solution to a high-pressure reactor, seal it, and place it in a forced-air drying oven for a solvothermal reaction at 150 °C for 5 h. After the reaction, allow it to cool naturally. Wash the cooled material three times with ultrapure water and anhydrous ethanol, and dry it in a forced-air drying oven at 60 °C for 8 h to obtain the CoVCe-OH nanoarray precursor loaded on the SS current collector.

[0064] S2. Place the CoVCe-OH nanoarray precursor loaded on the SS current collector obtained in step S1 in the downstream of a tube furnace, place the phosphorus source red phosphorus in the upstream, the mass ratio of CoVCe-OH to phosphorus source red phosphorus is 1:20, the Ar flow rate is controlled at 2 mL / min, the temperature is increased from room temperature to 500℃ at a heating rate of 2℃ / min, heat-treated at 500℃ for 1 h, and after natural cooling, the CoVP / CeO2 heterojunction nanoarray loaded on the SS current collector is obtained.

[0065] S3. Immerse the COVP / CeO2 heterojunction nanoarray loaded on the SS current collector obtained in step S2 into 1% 3-isocyanate-propyltrimethoxysilane (C7H) solvent using isopropanol as the solvent. 15 In a NO4Si solution, the grafting modification was carried out at 30℃ for 24 h. After grafting modification, the sample was washed three times with ethanol and dried in a forced-air drying oven at 60℃ for 6 h to obtain COVP / CeO2@C7H loaded on the SS current collector.15 NO4Si heterojunction nanoarray electrode.

[0066] Material characterization:

[0067] The obtained product was characterized by SEM to obtain the material morphology. Figure 2 As can be seen from the figure, there are uniformly distributed nanosheet structures on the SS current collector.

[0068] Example 3 CuWN / CeO2@C8H 19 BrO3Si heterojunction nanoarray electrode

[0069] The CuWN / CeO2@C8H 19 The fabrication method of BrO3Si heterojunction nanoarray electrodes includes the following steps:

[0070] S1. Dissolve 272.8 g (1600 mmol) copper chloride dihydrate (CuCl2·2H2O), 79.3 g (200 mmol) tungsten chloride (WCl6), 74.5 g (200 mmol) cerium chloride heptahydrate (CeCl3·7H2O), and 280.4 g (4000 mmol) ammonia solution (NH3·H2O) (25%-28% wt) in 5000 mL of ultrapure water, and stir thoroughly on a stirrer for 2 hours. After obtaining a mixed solution by stirring at 400 rpm, three 10×30 cm pretreated nickel foam (NF) sheets were immersed in the solution, transferred to a high-pressure reactor, sealed, and placed in a forced-air drying oven for solvothermal reaction at 60°C for 96 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed three times with ultrapure water and anhydrous ethanol, and then dried in a forced-air drying oven at 60°C for 24 h to obtain CuWCe-OH nanoarray precursor loaded on NF current collector.

[0071] S2. Place the CuWCe-OH nanoarray precursor loaded on the NF current collector obtained in step S1 in the downstream of a tube furnace, place the nitrogen source urea in the upstream, the mass ratio of CuWCe-OH to nitrogen source urea is 1:50, the He flow rate is controlled at 5 mL / min, the temperature is increased from room temperature to 400℃ at a heating rate of 3℃ / min, heat-treated at 400℃ for 4h, and after natural cooling, the CuWN / CeO2 heterojunction nanoarray loaded on the NF current collector is obtained.

[0072] S3. Immerse the CuWN / CeO2 heterostructure nanoarray loaded on the NF current collector obtained in step S2 into 0.1% 5-bromopentyltrimethoxysilane (C8H2O) solvent using ethylene glycol. 19 Grafting modification was performed in BrO3Si solution at 80℃ for 2 h. After grafting modification, the sample was washed three times with ethanol and dried in a forced-air drying oven at 60℃ for 6 h to obtain CuWN / CeO2@C8H supported on NF current collector.19 BrO3Si heterojunction nanoarray electrode.

[0073] Material characterization:

[0074] The obtained product was characterized by SEM to obtain the material morphology. Figure 3 As can be seen from the figure, there is a uniformly distributed nanosheet structure on the NF current collector.

[0075] Example 4 NiMnSe / CeO2@C 17 H 18 O3Si heterojunction nanoarray electrode

[0076] The NiMnSe / CeO2@C 17 H 18 The fabrication method of O3Si heterojunction nanoarray electrodes includes the following steps:

[0077] S1. Dissolve 8.7237 g (30 mmol) nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 2.510 g (10 mmol) manganese nitrate tetrahydrate (Mn(NO3)2·4H2O), 4.342 g (10 mmol) cerium nitrate hexahydrate (Ce(NO3)3·6H2O), and 5.611 g (100 mmol) potassium hydroxide (KOH) in 80 mL of ultrapure water, and stir thoroughly on a stirrer for 3 hours. After obtaining a mixed solution by stirring at 500 rpm, three pieces of 1×3 cm pretreated carbon cloth (CC) were immersed in the solution, transferred to a high-pressure reactor, sealed, and placed in a forced-air drying oven for solvothermal reaction at 180℃ for 2 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed three times with ultrapure water and anhydrous ethanol, and then dried in a forced-air drying oven at 60℃ for 12 h to obtain the NiMnCe-OH nanoarray precursor loaded on the CC current collector.

[0078] S2. Place the NiMnCe-OH nanoarray precursor loaded on the CC current collector obtained in step S1 in the downstream of a tube furnace, place the selenium source powder in the upstream, the mass ratio of NiMnCe-OH to selenium source powder is 1:1, the Ar flow rate is controlled at 2 mL / min, the temperature is increased from room temperature to 600℃ at a heating rate of 5℃ / min, heat-treated at 600℃ for 2 h, and after natural cooling, the NiMnSe / CeO2 heterojunction nanoarray loaded on the CC current collector is obtained.

[0079] S3. Immerse the NiMnSe / CeO2 heterostructure nanoarray loaded on the CC current collector obtained in step S2 into 5% 9-anthrayltrimethoxysilane (C8H) solvent using acetone. 19In a BrO3Si solution, NiMnSe / CeO2@C was grafted onto a CC current collector for 10 h at 40 °C. After grafting, the sample was washed three times with ethanol and dried in a forced-air drying oven at 60 °C for 6 h to obtain NiMnSe / CeO2@C current collector. 17 H 18 O3Si heterojunction nanoarray electrode.

[0080] Material characterization:

[0081] The obtained product was characterized by SEM to obtain the material morphology. Figure 4 As can be seen from the figure, there are uniformly distributed nanosheet structures on the CC current collector.

[0082] Example 5: FeCrP / CeO2@C 15 H 34 O3Si heterojunction nanoarray electrode

[0083] The FeCrP / CeO2@C 15 H 34 The fabrication method of O3Si heterojunction nanoarray electrodes includes the following steps:

[0084] S1. 48.7 g (180 mmol) ferric chloride hexahydrate (FeCl3·6H2O), 2.7 g (10 mmol) chromium chloride hexahydrate (CrCl3·6H2O), 3.7 g (10 mmol) cerium chloride heptahydrate (CeCl3·7H2O) and 56.1 g (400 mmol) hexamethylenetetramine (HMTA) were dissolved in 1500 mL of ultrapure water and stirred thoroughly on a stirrer for 2 h (stirrer speed was 600 rpm) to obtain a mixed solution. Two 5×6 cm pretreated aluminum foils (AlF) were then immersed in the solution and transferred to a high-pressure reactor. After sealing, the reactor was placed in a forced-air drying oven for a solvothermal reaction at 200 °C for 1 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed three times with ultrapure water and three times with anhydrous ethanol, and then dried in a forced-air drying oven at 60 °C for 6 h to obtain the FeCrCe-OH nanoarray precursor loaded on the AlF current collector.

[0085] S2. Place the FeCrCe-OH nanoarray precursor loaded on the AlF current collector obtained in step S1 in the downstream of a tube furnace, and place the phosphorus source sodium hypophosphite in the upstream. The mass ratio of FeCrCe-OH to phosphorus source sodium hypophosphite is 1:150. The N2 flow rate is controlled at 2 mL / min. The temperature is increased from room temperature to 500℃ at a heating rate of 8℃ / min. The temperature is then heat-treated at 500℃ for 6 h. After natural cooling, the FeCrP / CeO2 heterojunction nanoarray loaded on the AlF current collector is obtained.

[0086] S3. Immerse the FeCrP / CeO2 heterostructure nanoarray loaded on the AlF current collector obtained in step S2 into 2% dodecyltrimethoxysilane (C) solvent with acetone. 15 H 34 In an AlF current collector, FeCrP / CeO2@C was grafted onto a CeO2@C solution at 40°C for 10 h. After grafting, the sample was washed three times with ethanol and dried in a forced-air drying oven at 60°C for 6 h to obtain FeCrP / CeO2@C supported on the AlF current collector. 15 H 34 O3Si heterojunction nanoarray electrode.

[0087] Material characterization:

[0088] The obtained product was characterized by SEM to obtain the material morphology. Figure 5 As can be seen from the figure, there are uniformly distributed nanosheet structures on the AlF current collector.

[0089] Example 6 NiYS / CeO2@C7H 18 N2O4Si heterojunction nanoarray electrode

[0090] The NiYS / CeO2@C7H 18 The fabrication method of N2O4Si heterojunction nanoarray electrode includes the following steps:

[0091] S1. 1.902 g (8 mmol) nickel trichloride hexahydrate (NiCl2·6H2O), 0.304 g (1 mmol) yttrium chloride hexahydrate (YCl3·6H2O), 0.372 g (1 mmol) cerium chloride heptahydrate (CeCl3·7H2O) and 1.402 g (10 mmol) hexamethylenetetramine (HMTA) were dissolved in 50 mL of ultrapure water and stirred thoroughly on a stirrer for 3 h (stirrer speed was 500 rpm) to obtain a mixed solution. Then, 3 pieces of 2×3 cm pretreated iron foam (IF) were immersed in the solution, transferred to a high-pressure reactor, sealed and placed in a forced-air drying oven for solvothermal reaction at 150 °C for 24 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed 3 times with ultrapure water and anhydrous ethanol, respectively, and dried in a forced-air drying oven at 60 °C for 6 h to obtain the NiYCe-OH nanoarray precursor loaded on the IF current collector.

[0092] S2. Place the NiYCe-OH nanoarray precursor loaded on the IF current collector obtained in step S1 in the downstream of a tube furnace, place the sulfur source sulfur powder in the upstream, the mass ratio of NiYCe-OH to sulfur source sulfur powder is 1:100, the He flow rate is controlled at 2 mL / min, the temperature is increased from room temperature to 300℃ at a heating rate of 2℃ / min, heat-treated at 300℃ for 8 h, and after natural cooling, the NiYS / CeO2 heterojunction nanoarray loaded on the IF current collector is obtained.

[0093] S3. Immerse the NiYS / CeO2 heterostructure nanoarray loaded on the IF current collector obtained in step S2 into 10% 3-ureidopropyltrimethoxysilane (C7H) solvent using acetonitrile. 18 In a N2O4Si solution, NiYS / CeO2@C7H was grafted and modified at 30℃ for 18 h. After grafting modification, the sample was washed three times with ethanol and dried in a forced-air drying oven at 60℃ for 6 h to obtain NiYS / CeO2@C7H supported on an IF current collector. 18 N2O4Si heterojunction nanoarray electrode.

[0094] Material characterization:

[0095] The obtained product was characterized by SEM to obtain the material morphology. Figure 6 As can be seen from the figure, there is a uniformly distributed nanosheet structure on the IF current collector.

[0096] Comparative Example 1: NiTe Nanoarray Electrode

[0097] The method for preparing the NiTe nanoarray electrode includes the following steps:

[0098] S1. Dissolve 0.995 g (4 mmol) nickel acetate tetrahydrate (NiC4H6O4·4H2O) and 1.402 g (10 mmol) hexamethylenetetramine (HMTA) in 20 mL of ultrapure water. Stir the mixture thoroughly for 0.5 h (stirrer speed 500 rpm) to obtain a mixed solution. Immerse two 1×3 cm pretreated titanium mesh (TM) pieces in the solution, transfer the solution to a high-pressure reactor, seal it, and place it in a forced-air drying oven for a solvothermal reaction at 120 °C for 8 h. After the reaction is completed, allow it to cool naturally. Wash the cooled material three times with ultrapure water and anhydrous ethanol, respectively, and dry it in a forced-air drying oven at 60 °C for 12 h to obtain the Ni(OH)2 nanoarray precursor loaded on the TM current collector.

[0099] S2. Place the Ni(OH)2 nanoarray precursor loaded with TM current collector obtained in step S1 in the downstream of a tube furnace, and place the tellurium source powder in the upstream. The mass ratio of Ni(OH)2 to tellurium source powder is 1:10. The N2 flow rate is controlled at 5 mL / min. The temperature is increased from room temperature to 800℃ at a heating rate of 5℃ / min. Heat treatment is carried out at 800℃ for 2 hours. After natural cooling, the NiTe nanoarray electrode loaded with TM current collector is obtained.

[0100] Compared with Example 1, Comparative Example 1 did not add cerium salt and was not modified with silane coupling agent, but the remaining steps were the same as in Example 1.

[0101] Comparative Example 2: NiTe / CeO2 heterojunction nanoarray electrode

[0102] The method for preparing the NiTe / CeO2 heterojunction nanoarray electrode includes the following steps:

[0103] S1. 0.995 g (4 mmol) nickel acetate tetrahydrate (NiC4H6O4·4H2O), 0.317 g (1 mmol) cerium acetate hydrate (Ce(CH3CO2)3·xH2O) and 1.402 g (10 mmol) hexamethylenetetramine (HMTA) were dissolved in 20 mL of ultrapure water and stirred thoroughly on a stirrer for 0.5 h (stirrer speed 500 rpm) to obtain a mixed solution. The solution was then immersed in two 1×3 cm pretreated titanium mesh (TM), transferred to a high-pressure reactor, sealed, and placed in a forced-air drying oven for solvothermal reaction at 120 °C for 8 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed three times with ultrapure water and anhydrous ethanol, and then dried in a forced-air drying oven at 60 °C for 12 h to obtain the NiCe-OH nanoarray precursor loaded on the TM current collector.

[0104] S2. Place the NiCe-OH nanoarray precursor loaded with the TM current collector obtained in step S1 in the downstream of a tube furnace, and place the tellurium source powder in the upstream. The mass ratio of NiCe-OH to tellurium source powder is 1:10. The N2 flow rate is controlled at 5 mL / min. The temperature is increased from room temperature to 800℃ at a heating rate of 5℃ / min. The temperature is then heat-treated at 800℃ for 2 hours. After natural cooling, the NiTe / CeO2 heterojunction nanoarray loaded with the TM current collector is obtained.

[0105] Compared to Example 1, Comparative Example 2 had no silane coupling agent modification, but the remaining steps were the same as in Example 1. Comparative Example 3: CoVP nanoarray electrode

[0106] The preparation method of the CoVP nanoarray electrode includes the following steps:

[0107] S1. Dissolve 0.494 g (1.76 mmol) cobalt sulfate heptahydrate (CoSO4·7H2O), 0.033 g (0.2 mmol) vanadium oxysulfate hydrate (VOSO4·xH2O) and 1.92 g (32 mmol) urea (CH4N2O) in 15 mL of ultrapure water. Stir the mixture thoroughly for 2 h (400 rpm) to obtain a mixed solution. Immerse the solution in two 1×3 cm pretreated stainless steel (SS) sheets, transfer the solution to a high-pressure reactor, seal it, and place it in a forced-air drying oven for a solvothermal reaction at 150 °C for 5 h. After the reaction, allow it to cool naturally. Wash the cooled material three times with ultrapure water and anhydrous ethanol, and dry it in a forced-air drying oven at 60 °C for 8 h to obtain the CoV-OH nanoarray precursor loaded on the SS current collector.

[0108] S2. Place the CoV-OH nanoarray precursor loaded on the SS current collector obtained in step S1 in the downstream of a tube furnace, place the red phosphorus source in the upstream, the mass ratio of CoV-OH to red phosphorus source is 1:20, the Ar flow rate is controlled at 2 mL / min, the temperature is increased from room temperature to 500℃ at a heating rate of 2℃ / min, heat-treated at 500℃ for 1 h, and after natural cooling, the COVP nanoarray electrode loaded on the SS current collector is obtained.

[0109] Compared with Example 2, Comparative Example 3 did not add cerium salt and was not modified with silane coupling agent, while the remaining steps were the same as in Example 2.

[0110] Comparative example: 4CoVP / CeO2 heterojunction nanoarray electrode

[0111] The fabrication method of the COVP / CeO2 heterojunction nanoarray electrode includes the following steps:

[0112] S1. Dissolve 0.494 g (1.76 mmol) cobalt sulfate heptahydrate (CoSO4·7H2O), 0.033 g (0.2 mmol) vanadium oxysulfate hydrate (VOSO4·xH2O), 0.016 g (0.04 mmol) cerium sulfate tetrahydrate (Ce(SO4)2·4H2O) and 1.92 g (32 mmol) urea (CH4N2O) in 15 mL of ultrapure water. Stir the mixture thoroughly for 2 h (400 rpm) to obtain a mixed solution. Immerse the solution in two 1×3 cm pretreated stainless steel (SS) sheets, transfer the solution to a high-pressure reactor, seal it, and place it in a forced-air drying oven for a solvothermal reaction at 150 °C for 5 h. After the reaction, allow it to cool naturally. Wash the cooled material three times with ultrapure water and anhydrous ethanol, and dry it in a forced-air drying oven at 60 °C for 8 h to obtain the CoVCe-OH nanoarray precursor loaded on the SS current collector.

[0113] S2. Place the CoVCe-OH nanoarray precursor loaded on the SS current collector obtained in step S1 in the downstream of a tube furnace, place the red phosphorus source in the upstream, the mass ratio of CoVCe-OH to red phosphorus source is 1:20, the Ar flow rate is controlled at 2 mL / min, the temperature is increased from room temperature to 500℃ at a heating rate of 2℃ / min, heat-treated at 500℃ for 1 h, and after natural cooling, the COVP / CeO2 heterojunction nanoarray electrode loaded on the SS current collector is obtained.

[0114] Compared to Example 2, Comparative Example 4 was modified without silane coupling agent, but the remaining steps were the same as in Example 2. Comparative Example 5: CuWN nanoarray electrode

[0115] The method for preparing the CuWN nanoarray electrode includes the following steps:

[0116] S1. Dissolve 272.8 g (1600 mmol) copper chloride dihydrate (CuCl2·2H2O), 79.3 g (200 mmol) tungsten chloride (WCl6) and 280.4 g (4000 mmol) ammonia water (NH3·H2O) (25%-28% wt) in 5000 mL of ultrapure water. Stir the mixture thoroughly for 2 h (stirrer speed 400 rpm) to obtain a mixed solution. Immerse three 10×30 cm pretreated nickel foam (NF) sheets in the solution. Transfer the solution to a high-pressure reactor, seal it, and place it in a forced-air drying oven for a solvothermal reaction at 60 °C for 96 h. After the reaction, allow it to cool naturally. Wash the cooled material three times with ultrapure water and anhydrous ethanol, and dry it in a forced-air drying oven at 60 °C for 24 h to obtain the CuW-OH nanoarray precursor loaded on the NF current collector.

[0117] S2. Place the CuW-OH nanoarray precursor loaded on the NF current collector obtained in step S1 in the downstream of a tube furnace, and place the nitrogen source urea in the upstream. The mass ratio of CuW-OH to nitrogen source urea is 1:50. The He flow rate is controlled at 5 mL / min. The temperature is increased from room temperature to 400℃ at a heating rate of 3℃ / min. Heat treatment is carried out at 400℃ for 4 hours. After natural cooling, the CuWN nanoarray electrode loaded on the NF current collector is obtained.

[0118] Compared with Example 3, Comparative Example 5 did not add cerium salt and was not modified with silane coupling agent, while the remaining steps were the same as in Example 3.

[0119] Comparative example: 6CuWN / CeO2 heterojunction nanoarray electrode

[0120] The method for preparing the CuWN / CeO2 heterojunction nanoarray electrode includes the following steps:

[0121] S1. Dissolve 272.8 g (1600 mmol) copper chloride dihydrate (CuCl2·2H2O), 79.3 g (200 mmol) tungsten chloride (WCl6), 74.5 g (200 mmol) cerium chloride heptahydrate (CeCl3·7H2O), and 280.4 g (4000 mmol) ammonia solution (NH3·H2O) (25%-28% wt) in 5000 mL of ultrapure water, and stir thoroughly on a stirrer for 2 hours. After obtaining a mixed solution by stirring at 400 rpm, three 10×30 cm pretreated nickel foam (NF) sheets were immersed in the solution, transferred to a high-pressure reactor, sealed, and placed in a forced-air drying oven for solvothermal reaction at 60°C for 96 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed three times with ultrapure water and anhydrous ethanol, and then dried in a forced-air drying oven at 60°C for 24 h to obtain CuWCe-OH nanoarray precursor loaded on NF current collector.

[0122] S2. Place the CuWCe-OH nanoarray precursor loaded on the NF current collector obtained in step S1 in the downstream of a tube furnace, and place the nitrogen source urea in the upstream. The mass ratio of CuWCe-OH to nitrogen source urea is 1:50. The He flow rate is controlled at 5 mL / min. The temperature is increased from room temperature to 400℃ at a heating rate of 3℃ / min. Heat treatment is carried out at 400℃ for 4 hours. After natural cooling, the CuWN / CeO2 heterojunction nanoarray electrode loaded on the NF current collector is obtained.

[0123] Compared to Example 3, Comparative Example 6 was modified without silane coupling agent, but the remaining steps were the same as in Example 3. Comparative Example 7: NiMnSe nanoarray electrode

[0124] The method for preparing the NiMnSe nanoarray electrode includes the following steps:

[0125] S1. Dissolve 8.7237 g (30 mmol) nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 2.510 g (10 mmol) manganese nitrate tetrahydrate (Mn(NO3)2·4H2O) and 5.611 g (100 mmol) potassium hydroxide (KOH) in 80 mL of ultrapure water. Stir the mixture thoroughly for 3 h (stirrer speed 500 rpm) to obtain a mixed solution. Immerse 3 pieces of 1×3 cm pretreated carbon cloth (CC) in the solution, transfer it to a high-pressure reactor, seal it, and place it in a forced-air drying oven for a solvothermal reaction at 180 °C for 2 h. After the reaction is completed, allow it to cool naturally. Wash the cooled material three times with ultrapure water and anhydrous ethanol, respectively, and dry it in a forced-air drying oven at 60 °C for 12 h to obtain the NiMn-OH nanoarray precursor loaded on the CC current collector.

[0126] S2. Place the NiMn-OH nanoarray precursor loaded with CC current collector obtained in step S1 in the downstream of a tube furnace, place the selenium source powder in the upstream, the mass ratio of NiMn-OH to selenium source powder is 1:1, the Ar flow rate is controlled at 2 mL / min, the temperature is increased from room temperature to 600℃ at a heating rate of 5℃ / min, heat-treated at 600℃ for 2 h, and after natural cooling, the NiMnSe nanoarray electrode loaded with CC current collector is obtained.

[0127] Compared with Example 4, Comparative Example 7 did not add cerium salt and was not modified with silane coupling agent, while the remaining steps were the same as in Example 4.

[0128] Comparative example: 8NiMnSe / CeO2 heterojunction nanoarray electrode

[0129] The method for preparing the NiMnSe / CeO2 heterojunction nanoarray electrode includes the following steps:

[0130] S1. Dissolve 8.7237 g (30 mmol) nickel nitrate hexahydrate (Ni(NO3)2·6H2O), 2.510 g (10 mmol) manganese nitrate tetrahydrate (Mn(NO3)2·4H2O), 4.342 g (10 mmol) cerium nitrate hexahydrate (Ce(NO3)3·6H2O), and 5.611 g (100 mmol) potassium hydroxide (KOH) in 80 mL of ultrapure water, and stir thoroughly on a stirrer for 3 hours. After obtaining a mixed solution by stirring at 500 rpm, three pieces of 1×3 cm pretreated carbon cloth (CC) were immersed in the solution, transferred to a high-pressure reactor, sealed, and placed in a forced-air drying oven for solvothermal reaction at 180℃ for 2 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed three times with ultrapure water and anhydrous ethanol, and then dried in a forced-air drying oven at 60℃ for 12 h to obtain the NiMnCe-OH nanoarray precursor loaded on the CC current collector.

[0131] S2. Place the NiMnCe-OH nanoarray precursor loaded on the CC current collector obtained in step S1 in the downstream of a tube furnace, place the selenium source powder in the upstream, the mass ratio of NiMnCe-OH to selenium source powder is 1:1, the Ar flow rate is controlled at 2 mL / min, the temperature is increased from room temperature to 600℃ at a heating rate of 5℃ / min, heat-treated at 600℃ for 2 h, and after natural cooling, the NiMnSe / CeO2 heterojunction nanoarray loaded on the CC current collector is obtained.

[0132] Compared to Example 4, Comparative Example 8 was modified without silane coupling agent, but the remaining steps were the same as in Example 4. Comparative Example 9: FeCrP nanoarray electrode

[0133] The preparation method of the FeCrP nanoarray electrode includes the following steps:

[0134] S1. 48.7 g (180 mmol) ferric chloride hexahydrate (FeCl3·6H2O), 2.7 g (10 mmol) chromium chloride hexahydrate (CrCl3·6H2O) and 56.1 g (400 mmol) hexamethylenetetramine (HMTA) were dissolved in 15 mL of ultrapure water and stirred thoroughly on a stirrer for 2 h (stirrer speed 600 rpm) to obtain a mixed solution. Two 5×6 cm pretreated aluminum foils (AlF) were then immersed in the solution and transferred to a high-pressure reactor. After sealing, the reactor was placed in a forced-air drying oven for a solvothermal reaction at 200 °C for 1 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed three times with ultrapure water and three times with anhydrous ethanol, and then dried in a forced-air drying oven at 60 °C for 6 h to obtain the FeCr-OH nanoarray precursor loaded on the AlF current collector.

[0135] S2. Place the FeCr-OH nanoarray precursor loaded on the AlF current collector obtained in step S1 in the downstream of a tube furnace, and place the phosphorus source sodium hypophosphite in the upstream. The mass ratio of FeCr-OH to phosphorus source sodium hypophosphite is 1:150. The N2 flow rate is controlled at 2 mL / min. The temperature is increased from room temperature to 500℃ at a heating rate of 8℃ / min. Heat treatment is carried out at 500℃ for 6 hours. After natural cooling, the FeCrP nanoarray electrode loaded on the AlF current collector is obtained.

[0136] Compared with Example 5, Comparative Example 9 did not add cerium salt and was not modified with silane coupling agent, while the remaining steps were the same as in Example 5.

[0137] Comparative Example: 10FeCrP / CeO2 heterojunction nanoarray electrode

[0138] The preparation method of the FeCrP / CeO2 heterojunction nanoarray electrode includes the following steps:

[0139] S1. 48.7 g (180 mmol) ferric chloride hexahydrate (FeCl3·6H2O), 2.7 g (10 mmol) chromium chloride hexahydrate (CrCl3·6H2O), 3.7 g (10 mmol) cerium chloride heptahydrate (CeCl3·7H2O) and 56.1 g (400 mmol) hexamethylenetetramine (HMTA) were dissolved in 1500 mL of ultrapure water and stirred thoroughly on a stirrer for 2 h (stirrer speed was 600 rpm) to obtain a mixed solution. Two 5×6 cm pretreated aluminum foils (AlF) were then immersed in the solution and transferred to a high-pressure reactor. After sealing, the reactor was placed in a forced-air drying oven for a solvothermal reaction at 200 °C for 1 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed three times with ultrapure water and three times with anhydrous ethanol, and then dried in a forced-air drying oven at 60 °C for 6 h to obtain the FeCrCe-OH nanoarray precursor loaded on the AlF current collector.

[0140] S2. Place the FeCrCe-OH nanoarray precursor loaded on the AlF current collector obtained in step S1 in the downstream of a tube furnace, and place the phosphorus source sodium hypophosphite in the upstream. The mass ratio of FeCrCe-OH to phosphorus source sodium hypophosphite is 1:150. The N2 flow rate is controlled at 2 mL / min. The temperature is increased from room temperature to 500℃ at a heating rate of 8℃ / min. The temperature is then heat-treated at 500℃ for 6 h. After natural cooling, the FeCrP / CeO2 heterojunction nanoarray loaded on the AlF current collector is obtained.

[0141] Compared to Example 5, Comparative Example 10 was modified without silane coupling agent, but the remaining steps were the same as in Example 5. Comparative Example 11: NiYS nanoarray electrode

[0142] The method for preparing the NiYS nanoarray electrode includes the following steps:

[0143] S1. Dissolve 1.902 g (8 mmol) nickel trichloride hexahydrate (NiCl2·6H2O), 0.304 g (1 mmol) yttrium chloride hexahydrate (YCl3·6H2O) and 1.402 g (10 mmol) hexamethylenetetramine (HMTA) in 50 mL of ultrapure water. Stir the mixture thoroughly for 3 h (stirrer speed 500 rpm) to obtain a mixed solution. Immerse 3 pieces of 2×3 cm pretreated iron foam (IF) in the solution, transfer it to a high-pressure reactor, seal it, and place it in a forced-air drying oven for solvothermal reaction at 150 °C for 24 h. After the reaction is completed, allow it to cool naturally. Wash the cooled material three times with ultrapure water and anhydrous ethanol, respectively, and dry it in a forced-air drying oven at 60 °C for 6 h to obtain the NiY-OH nanoarray precursor loaded on the IF current collector.

[0144] S2. Place the NiY-OH nanoarray precursor loaded on the IF current collector obtained in step S1 in the downstream of a tube furnace, and place the sulfur source sulfur powder in the upstream. The mass ratio of NiY-OH to sulfur source sulfur powder is 1:100. The He flow rate is controlled at 2 mL / min. The temperature is increased from room temperature to 300℃ at a heating rate of 2℃ / min. Heat treatment is carried out at 300℃ for 8 hours. After natural cooling, the NiYS heterojunction nanoarray electrode loaded on the IF current collector is obtained.

[0145] Compared with Example 6, Comparative Example 11 did not add cerium salt and was not modified with silane coupling agent, while the remaining steps were the same as in Example 6.

[0146] Comparative Example 12NiYS / CeO2 heterojunction nanoarray electrode

[0147] The method for preparing the NiYS / CeO2 heterojunction nanoarray electrode includes the following steps:

[0148] S1. 1.902 g (8 mmol) nickel trichloride hexahydrate (NiCl2·6H2O), 0.304 g (1 mmol) yttrium chloride hexahydrate (YCl3·6H2O), 0.372 g (1 mmol) cerium chloride heptahydrate (CeCl3·7H2O) and 1.402 g (10 mmol) hexamethylenetetramine (HMTA) were dissolved in 50 mL of ultrapure water and stirred thoroughly on a stirrer for 3 h (stirrer speed was 500 rpm) to obtain a mixed solution. Then, 3 pieces of 2×3 cm pretreated iron foam (IF) were immersed in the solution, transferred to a high-pressure reactor, sealed and placed in a forced-air drying oven for solvothermal reaction at 150 °C for 24 h. After the reaction was completed, the solution was allowed to cool naturally. The cooled material was washed 3 times with ultrapure water and anhydrous ethanol, respectively, and dried in a forced-air drying oven at 60 °C for 6 h to obtain the NiYCe-OH nanoarray precursor loaded on the IF current collector.

[0149] S2. Place the NiYCe-OH nanoarray precursor loaded on the IF current collector obtained in step S1 in the downstream of a tube furnace, place the sulfur source sulfur powder in the upstream, the mass ratio of NiYCe-OH to sulfur source sulfur powder is 1:100, the He flow rate is controlled at 2 mL / min, the temperature is increased from room temperature to 300℃ at a heating rate of 2℃ / min, heat-treated at 300℃ for 8 h, and after natural cooling, the NiYS / CeO2 heterojunction nanoarray loaded on the IF current collector is obtained.

[0150] Compared to Example 6, Comparative Example 12 was modified without silane coupling agent, and the remaining steps were the same as in Example 6. Performance testing of benzyl alcohol electro-oxidation (BAOR) in Application Example 1.

[0151] Electrochemical tests were performed using a computer-controlled electrochemical workstation (Autolab, PGSTAT302N) with a standard three-electrode system. The main indicators for evaluating the activity of electrocatalytic materials were: the voltage (E) required to achieve the same current density, the formation rate of the target product, and the Faraday efficiency.

[0152] The electrocatalytic performance of the samples was investigated in a three-electrode system using an array electrode (1×1 cm) as the working electrode, a Pt sheet (2×2 cm) as the counter electrode, and an Hg / HgO electrode (immersed in 1.0 M KOH solution) as the reference electrode, prepared according to the examples or comparative examples. The solution resistance (Rt) of all materials was measured at open-circuit potential before each electrochemical data acquisition. s The potential values ​​were repeatedly scanned using CV curves within the voltage range of 0.2–0.8 V vs. Hg / HgO until stable. Then, LSV tests were performed within the voltage range of 0.1–1.0 V vs. Hg / HgO, and the LSV curves were compensated for with 95% IR. Simultaneously, the potential value E(Hg / HgO) was converted to E(RHE) according to the formula E(RHE) = E(Hg / HgO) + 0.0977 + 0.05916 × pH. Furthermore, the BAOR performance of the material was tested for a longer period using chronoamperometry, and the product was quantitatively analyzed by HPLC. The specific test procedure was as follows: After the CA test, 200 μL of the reaction solution was injected into a certain amount of deionized water for dilution, and a small amount of 0.5 M H₂SO₄ was added to adjust the pH value. The solution was filtered through a 0.22 μm filter membrane, and 20 μL of the sample was injected into the syringe. HPLC test parameters: UV detector, C18 column, mobile phase: a mixture of methanol and 0.05M potassium dihydrogen phosphate (methanol:potassium dihydrogen phosphate = 70:30), wavelength: 250 nm, column temperature: 50℃, flow rate: 0.8 mL / min, detection time: 7 min. Qualitative analysis was subsequently performed using HPLC-MS.

[0153] This application example tests the BAOR performance of Example 1 (NiTe / CeO2@C 10 H 21 Cl3Si), Comparative Example 1 (NiTe), and Comparative Example 2 (NiTe / CeO2), and the LSV results refer to Figure 7 . As can be seen from the figure, in terms of BAOR performance, NiTe / CeO2@C 10 H 21 Cl3Si has a smaller E than NiTe / CeO2 and NiTe 100 , and the E 100 vs. RHE are NiTe / CeO2@C 10 H 21 Cl3Si (1.338V) < NiTe / CeO2 (1.354V) < NiTe (1.387V), respectively. According to the HPLC test, the formation rate of benzoic acid for NiTe / CeO2@C 10 H 21 Cl3Si at 1.45V vs. RHE is 0.617mmol / (h·cm 2 ), with a Faraday efficiency of 91.2%; the formation rate of benzoic acid for NiTe / CeO2 at 1.45V vs. RHE is 0.524mmol / (h·cm 2 ), with a Faraday efficiency of 82.1%; the formation rate of benzoic acid for NiTe at 1.45V vs. RHE is 0.383mmol / (h·cm 2 ), with a Faraday efficiency of 69.8%. It can be seen from the above performance results that the BAOR performance of Example 1 (NiTe / CeO2@C 10 H 21 Cl3Si) is superior to that of Comparative Example 2 (NiTe / CeO2), and the BAOR performance of Comparative Example 2 (NiTe / CeO2) is superior to that of Comparative Example 1 (NiTe).

[0154] Application Example 2 Performance test of 5-HMF electrooxidation reaction (HMFOR)

[0155] The electrochemical test is carried out by using a computer-controlled electrochemical workstation (Autolab, PGSTAT302N) with a standard three-electrode system; the main indicators for evaluating the activity of electrocatalytic materials are: the voltage (E) required to reach the same current density, the formation rate of the target product, and the Faraday efficiency.

[0156] The electrocatalytic performance of the samples was studied in a three-electrode system, where the array electrode prepared in the example or comparative example served as the working electrode (1×1 cm), a Pt sheet (2×2 cm) served as the counter electrode, and an Hg / HgO electrode (immersed in 1.0 M KOH solution) served as the reference electrode. Before each electrochemical data collection, the solution resistance (R s ) value of all materials was collected at the open circuit potential, and CV curves were scanned multiple times in the voltage range of 0.2 to 0.8 V vs. Hg / HgO until stable, then LSV test was carried out in the voltage range of 0.1 to 1.0 V vs. Hg / HgO, and 95% IR compensation was performed on the LSV curve. Meanwhile, according to the formula E(RHE) = E(Hg / HgO) + 0.0977 + 0.05916×pH, the potential value E(Hg / HgO) was converted to E(RHE). In addition, the HMFOR performance of the material was tested for a long time by chronoamperometry, and the product was quantitatively analyzed by HPLC. The specific test process: after the CA test is completed, use a syringe to extract 200 μL of the reaction solution and inject it into a certain amount of deionized water for dilution, then add a small amount of 0.5 M H₂SO₄ to adjust the pH value of the solution, filter the solution through a 0.22 μm filter membrane, and take 20 μL of the sample to inject into the sampler. HPLC test parameters: the detector is a UV detector, the chromatographic column is C18, the mobile phase is a mixed solution of methanol and 0.05 M potassium dihydrogen phosphate (methanol: potassium dihydrogen phosphate = 70:30), the wavelength is 250 nm, the column temperature is 50 °C, the flow rate is 0.8 mL / min, and the detection time is 7 min. Qualitative analysis was subsequently performed using HPLC-MS.

[0157] In this application example, the HMFOR performance of Example 2 (CoVP / CeO₂@C₇H 15 NO₄Si), Comparative Example 3 (CoVP), and Comparative Example 4 (CoVP / CeO₂) was tested, and the LSV results refer to Figure 8 . It can be seen from the figure that for the HMFOR performance, CoVP / CeO₂@C₇H 15 NO₄Si has a smaller E compared with CoVP / CeO₂ and CoVP 100 , E 100 vs. RHE are respectively CoVP / CeO₂@C₇H 15 NO₄Si (1.367 V) < CoVP / CeO₂ (1.418 V) < CoVP (1.456 V). According to the HPLC test, the formation rate of furandicarboxylic acid (FDCA) of CoVP / CeO₂@C₇H 15 NO₄Si at 1.45 V vs. RHE is 0.164 mmol / (h·cm 2The Faraday efficiency was 90.5%, and the production rate of furanyl dicarboxylic acid (FDCA) from COVP / CeO2 at 1.45V vs. RHE was 0.117 mmol / (h·cm). 2 The Faraday efficiency was 79.1%, and the FDCA production rate of COVP at 1.45V vs. RHE was 0.084 mmol / (h·cm). 2 The Faraday efficiency is 67.5%. Based on the above performance results, it can be seen that Example 2 (CoVP / CeO2@C7H) 15 The HMFOR performance of NO4Si was better than that of Comparative Example 4 (CoVP / CeO2), and the HMFOR performance of Comparative Example 4 (CoVP / CeO2) was better than that of Comparative Example 3 (CoVP).

[0158] Application Example 3: Performance Testing of Cyclohexanone Electro-oxidation Reaction (CYCOR)

[0159] Electrochemical tests were performed using a computer-controlled electrochemical workstation (Autolab, PGSTAT302N) with a standard three-electrode system. The main indicators for evaluating the activity of electrocatalytic materials were: the voltage (E) required to achieve the same current density, the formation rate of the target product, and the Faraday efficiency.

[0160] The electrocatalytic performance of the samples was studied in a three-electrode system using an array electrode (1×1 cm) prepared in the examples or comparative examples as the working electrode, a Pt sheet (2×2 cm) as the counter electrode, and an Hg / HgO electrode (immersed in 1.0 M KOH solution) as the reference electrode. The solution resistance (R0) of all materials was measured at open-circuit potential before each electrochemical data acquisition. s) value, all were subjected to multiple CV curve scans within the voltage range of 0.2 to 0.8 V vs. Hg / HgO until stable, then LSV tests were performed within the voltage range of 0.1 to 1.0 V vs. Hg / HgO, 95% IR compensation was performed on the LSV curves, and at the same time, the potential value E(Hg / HgO) was converted to E(RHE) according to the formula E(RHE) = E(Hg / HgO) + 0.0977 + 0.05916 × pH. In addition, the CYCOR performance of the material was tested for a long time by chronoamperometry, and the product was quantitatively analyzed by GC. Specific test procedure: After the CA test is completed, use a syringe to extract 2 mL of the reaction solution and inject it into a certain amount of deionized water for dilution, then add a small amount of 1 M HCl to adjust the pH value of the solution, then add dichloromethane for extraction, transfer the organic phase to a sample vial, add a small amount of Na₂SO₄ for dehydration, and take 2 μL of the sample to inject into the sampler. GC test parameters: The detector is an FID detector, the chromatographic column is a DB-5ms capillary column, and the carrier gas is N₂. The inlet temperature is 250 °C, the FID detector temperature is 300 °C, the H₂ flow rate is 30 mL / min, the air flow rate is 400 mL / min, and the make-up N₂ flow rate is 25 mL / min. Subsequent qualitative analysis was performed using GC-MS.

[0161] This application example tests the CYCOR performance of Example 3 (CuWN / CeO₂@C₈H 19 BrO₃Si) and Comparative Example 5 (CuWN) and Comparative Example 6 (CuWN / CeO₂), the LSV results refer to Figure 9 . As can be seen from the figure, for the CYCOR performance, compared with CuWN, CuWN / CeO₂@C₈H 19 BrO₃Si has a smaller E 50 , E 50 vs. RHE are respectively CuWN / CeO₂@C₈H 19 BrO₃Si (1.361 V) < CuWN / CeO₂ (1.413 V) < CuWN (1.442 V). According to GC tests, the adipic acid generation rate of CuWN / CeO₂@C₈H 19 BrO₃Si at 1.45 V vs. RHE is 0.181 mmol / (h·cm 2 ), the Faraday efficiency is 83.4%, the adipic acid generation rate of CuWN / CeO₂ at 1.45 V vs. RHE is 0.129 mmol / (h·cm 2 ), the Faraday efficiency is 72.4%, the adipic acid generation rate of CuWN at 1.45 V vs. RHE is 0.075 mmol / (h·cm 2The Faraday efficiency is 56.1%. Based on the above performance results, it can be seen that Example 3 (CuWN / CeO2@C8H) 19 The HMFOR performance of BrO3Si is better than that of Comparative Example 6 (CuWN / CeO2), and the HMFOR performance of Comparative Example 6 (CuWN / CeO2) is better than that of Comparative Example 5 (CuWN).

[0162] Application Example 4: Performance Testing of the Electro-oxidation Reaction of Benzylamine (BANOR)

[0163] Electrochemical tests were performed using a computer-controlled electrochemical workstation (Autolab, PGSTAT302N) with a standard three-electrode system. The main indicators for evaluating the activity of electrocatalytic materials were: the voltage (E) required to achieve the same current density, the formation rate of the target product, and the Faraday efficiency.

[0164] The electrocatalytic performance of the samples was investigated in a three-electrode system using an array electrode (1×1 cm) as the working electrode, a Pt sheet (2×2 cm) as the counter electrode, and an Hg / HgO electrode (immersed in 1.0 M KOH solution) as the reference electrode, prepared according to the examples or comparative examples. The solution resistance (Rt) of all materials was measured at open-circuit potential before each electrochemical data acquisition. s The potential values ​​were repeatedly scanned using CV curves within the voltage range of 0.2–0.8 V vs. Hg / HgO until stable. Then, LSV tests were performed within the voltage range of 0.1–1.0 V vs. Hg / HgO, and the LSV curves were compensated for with 95% IR. Simultaneously, the potential value E(Hg / HgO) was converted to E(RHE) according to the formula E(RHE) = E(Hg / HgO) + 0.0977 + 0.05916 × pH. Furthermore, the BANOR performance of the material was tested for a longer period using chronoamperometry, and the product was quantitatively analyzed by HPLC. The specific test procedure was as follows: After the CA test, 200 μL of the reaction solution was injected into a certain amount of deionized water for dilution, and a small amount of 0.5 M H₂SO₄ was added to adjust the pH value. The solution was filtered through a 0.22 μm filter membrane, and 20 μL of the sample was injected into the syringe. HPLC test parameters: UV detector, C18 column, mobile phase: a mixture of methanol and 0.05M potassium dihydrogen phosphate (methanol:potassium dihydrogen phosphate = 70:30), wavelength: 250 nm, column temperature: 50℃, flow rate: 0.8 mL / min, detection time: 7 min. Qualitative analysis was subsequently performed using HPLC-MS.

[0165] This application example relates to Example 4 (NiMnSe / CeO2@C 17 H 18O3Si), Comparative Example 7 (NiMnSe) and Comparative Example 8 (NiMnSe / CeO2) were tested for BANOR performance, and the LSV results are shown in Figure 10 . It can be seen from the figure that for BANOR performance, NiMnSe / CeO2@C 17 H 18 O3Si has a smaller E compared with NiMnSe 50 , the E 50 vs. RHE values are NiMnSe / CeO2@C 17 H 18 O3Si (1.365V) < NiMnSe / CeO2 (1.404V) < NiMnSe (1.481V). According to the HPLC test, the formation rate of benzonitrile over NiMnSe / CeO2@C 17 H 18 O3Si at 1.45V vs. RHE is 0.425mmol / (h·cm 2 ), with a Faraday efficiency of 93.2%; the formation rate of benzonitrile over NiMnSe / CeO2 at 1.45V vs. RHE is 0.315mmol / (h·cm 2 ), with a Faraday efficiency of 80.2%; the formation rate of benzonitrile over NiMnSe at 1.45V vs. RHE is 0.222mmol / (h·cm 2 ), with a Faraday efficiency of 73.6%. It can be seen from the above performance results that the BANOR performance of Example 4 (NiMnSe / CeO2@C 17 H 18 O3Si) is better than that of Comparative Example 8 (NiMnSe / CeO2), and the BANOR performance of Comparative Example 8 (NiMnSe / CeO2) is better than that of Comparative Example 7 (NiMnSe).

[0166] Application Example 5 Performance Test of Nitrobenzene Electroreduction Reaction (NBRR)

[0167] The electrochemical test adopts a computer-controlled electrochemical workstation (Autolab, PGSTAT302N), and the measurement is carried out using a standard three-electrode system; the main indicators for evaluating the activity of electrocatalytic materials are: the voltage (E) required to reach the same current density, the formation rate of the target product, and the Faraday efficiency.

[0168] The electrocatalytic performance of the samples was studied in a three-electrode system where the array electrode prepared in the example or comparative example was used as the working electrode (1×1cm), a Pt sheet (2×2cm) was used as the counter electrode, and an Hg / HgO electrode (immersed in 1.0M KOH solution) was used as the reference electrode. Before each electrochemical data collection, the solution resistance (Rs ) value, the CV curves were scanned multiple times within the voltage range of 0 to -0.4 V vs. Hg / HgO until stable, then the LSV test was performed within the voltage range of 0.4 to -0.8 V vs. Hg / HgO, and 95% IR compensation was performed on the LSV curves. Meanwhile, according to the formula E(RHE) = E(Hg / HgO) + 0.0977 + 0.05916 × pH, the potential value E(Hg / HgO) was converted to E(RHE). In addition, the NBRR performance of the material was tested for a long time by chronoamperometry, and the product was quantitatively analyzed by HPLC. Specific test process: After the CA test is completed, use a syringe to extract 200 μL of the reaction solution and inject it into a certain amount of deionized water for dilution, then add a small amount of 0.5 M H2SO4 to adjust the pH value of the solution. After the solution is filtered through a 0.22 μm filter membrane, 20 μL of the sample is taken and injected into the sampler. HPLC test parameters: The detector is a UV detector, the chromatographic column is C18, the mobile phase is a mixed solution of methanol and 0.05 M potassium dihydrogen phosphate (methanol: potassium dihydrogen phosphate = 70:30), the wavelength is 250 nm, the column temperature is 50 °C, the flow rate is 0.8 mL / min, and the detection time is 7 min. Qualitative analysis is subsequently performed using HPLC-MS.

[0169] This application example tests the NBRR performance of the array electrodes prepared in Example 5 (FeCrP / CeO2@C 15 H 34 O3Si), Comparative Example 9 (FeCrP), and Comparative Example 10 (FeCrP / CeO2), and the LSV results refer to Figure 11 . It can be seen from the figure that for NBRR performance, FeCrP / CeO2@C 15 H 34 O3Si has a smaller E than FeCrP 50 , E 50 vs. RHE are respectively FeCrP / CeO2@C 15 H 34 O3Si (-0.039 V) < FeCrP / CeO2 (-0.148 V) < FeCrP (-0.224 V). According to the HPLC test, the aniline formation rate of FeCrP / CeO2@C 15 H 34 O3Si at 0 V vs. RHE is 0.193 mmol / (h·cm 2 ), the Faraday efficiency is 98.1%, and the aniline formation rate of FeCrP / CeO2 at 0 V vs. RHE is 0.132 mmol / (h·cm 2The Faraday efficiency was 87.8%, and the aniline formation rate of FeCrP under 0V vs. RHE conditions was 0.072 mmol / (h·cm). 2 The Faraday efficiency is 74.2%. Based on the above performance results, it can be seen that Example 5 (FeCrP / CeO2@C) 15 H 34 The NBRR performance of (O3Si) is better than that of Comparative Example 10 (FeCrP / CeO2), and the NBRR performance of Comparative Example 10 (FeCrP / CeO2) is better than that of Comparative Example 9 (FeCrP).

[0170] Application Example 6: Performance Testing of the Benzaldehyde Electroreduction Reaction (BARR)

[0171] Electrochemical tests were performed using a computer-controlled electrochemical workstation (Autolab, PGSTAT302N) with a standard three-electrode system. The main indicators for evaluating the activity of electrocatalytic materials were: the voltage (E) required to achieve the same current density, the formation rate of the target product, and the Faraday efficiency.

[0172] The electrocatalytic performance of the samples was studied in a three-electrode system using an array electrode (1×1 cm) prepared in the examples or comparative examples as the working electrode, a Pt sheet (2×2 cm) as the counter electrode, and an Hg / HgO electrode (immersed in 1.0 M KOH solution) as the reference electrode. The solution resistance (R0) of all materials was measured at open-circuit potential before each electrochemical data acquisition. s The potential values ​​were repeatedly scanned within the voltage range of 0 to -0.4V vs. Hg / HgO until stable. Then, LSV testing was performed within the voltage range of 0 to -0.8V vs. Hg / HgO, and the LSV curves were compensated for with 95% IR. Simultaneously, the potential value E(Hg / HgO) was converted to E(RHE) according to the formula E(RHE) = E(Hg / HgO) + 0.0977 + 0.05916 × pH. Furthermore, the BARR performance of the material was tested for a longer period using chronoamperometry, and the products were quantitatively analyzed by GC. The specific testing procedure was as follows: After the CA test, 2 mL of the reaction solution was drawn into a syringe and diluted with a certain amount of deionized water. A small amount of 1M HCl was added to adjust the pH of the solution, followed by extraction with dichloromethane. The organic phase was transferred to a sample vial, and a small amount of Na2SO4 was added for dehydration. 2 μL of sample was then injected into the syringe. GC test parameters: FID detector, DB-5ms capillary column, N2 carrier gas. Injector temperature 250℃, FID detector temperature 300℃, H2 flow rate 30mL / min, air flow rate 400mL / min, and make-up N2 flow rate 25mL / min. Qualitative analysis was subsequently performed using GC-MS.

[0173] This application example tests the BARR performance of the array electrodes prepared in Example 6 (NiYS / CeO2@C7H 18 N2O4Si), Comparative Example 11 (NiYS), and Comparative Example 12 (NiYS / CeO2), and the LSV results are referred to in Figure 12 . As can be seen from the figure, in terms of BARR performance, NiYS / CeO2@C7H 18 N2O4Si has a smaller E compared with NiYS 100 , the E 100 vs. RHE are respectively NiYS / CeO2@C7H 18 N2O4Si (-0.199V) < NiYS / CeO2 (-0.241V) < NiYS (-0.288V). According to the HPLC test, the formation rate of benzyl alcohol for NiYS / CeO2@C7H 18 N2O4Si at -0.2V vs. RHE is 0.373mmol / (h·cm 2 ), with a Faraday efficiency of 89.2%; the formation rate of benzyl alcohol for NiYS / CeO2 at -0.2V vs. RHE is 0.267mmol / (h·cm 2 ), with a Faraday efficiency of 76.2%; the formation rate of benzyl alcohol for NiYS at -0.2V vs. RHE is 0.144mmol / (h·cm 2 ), with a Faraday efficiency of 61.5%. It can be seen from the above performance results that the BARR performance of Example 6 (NiYS / CeO2@C7H 18 N2O4Si) is superior to that of Comparative Example 12 (NiYS / CeO2), and the BARR performance of Comparative Example 12 (NiYS / CeO2) is superior to that of Comparative Example 11 (NiYS).

[0174] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments, and any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement modes and are all included within the protection scope of the present invention.

Claims

1. A method for fabricating a surface-modified heterojunction nanoarray electrode, characterized in that, Specifically, the following steps are included: S1. Place the current collector in a mixed solution containing a precipitant, cerium salt and other transition metal salts, and carry out a solvothermal reaction at 50~250℃ to obtain a hydroxide nanoarray precursor grown in situ on the current collector. The transition metal of the transition metal salt is Ni, or Co and V, or Cu and W, or Ni and Mn, or Fe and Cr, or Ni and Y; The precipitant is selected from at least one of sodium hydroxide, potassium hydroxide, ammonia, sodium carbonate, sodium bicarbonate, urea, and hexamethylenetetramine. S2. Take the nanoarray precursor obtained in step S1, place it in an inert gas atmosphere, add a heat conversion source material, and carry out a high-temperature gas-solid purging reaction at 250~800℃ to obtain a heterojunction nanoarray material composed of transition metal matrix and cerium oxide composite. In step S2, the heat conversion source material is a phosphorus source, a sulfur source, a selenium source, or a tellurium source; S3. Take the heterojunction nanoarray material obtained in step S2 and place it in a solvent containing silane coupling agent. Stir to perform grafting modification, wash and dry to obtain a heterojunction nanoarray electrode with silane coupling agent surface modification.

2. The preparation method according to claim 1, characterized in that, In step S1, the current collector is carbon cloth, carbon paper, or a metal current collector.

3. The preparation method according to claim 1, characterized in that, In step S3, the silane coupling agent is selected from at least one of vinyltriethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-ureopropyltrimethoxysilane, epoxybutyltrimethoxysilane, phenyltrimethoxysilane, 9-anthrayltrimethoxysilane, n-decyltrimethoxysilane, dodecyltrimethoxysilane, dimethyldiethoxysilane, 3-glycidyl etheroxypropyltrimethoxysilane, 5-bromopentyltrimethoxysilane, n-decyltrichlorosilane, 1H,1H,2H,2H-perfluorodecyltrimethoxysilane, and 3-isocyanate-propyltrimethoxysilane.

4. The preparation method according to claim 1, characterized in that, In step S3, the grafting modification temperature is 25~150 ℃.

5. The surface-modified heterojunction nanoarray electrode prepared by any of the preparation methods described in claims 1 to 4.

6. The application of the surface-modified heterojunction nanoarray electrode of claim 5 in organic electrosynthesis reactions.

7. The application according to claim 6, characterized in that, The organic electrosynthesis reactions include the electrooxidation reactions of organic alcohols, ketones, and amines, and / or the electroreduction reactions of nitro compounds and carbonyl compounds.

Citation Information

Patent Citations

  • Preparation method of platinum nanoparticle array modified electrode with heterostructure

    CN113328105A

  • Metal-organic complex modified transition metal-based nano array electrode as well as preparation method and application thereof

    CN113957479A

  • Preparation method and application of cerium dioxide nanoparticle / ferronickel bimetallic phosphide / foamed nickel composite electrode

    CN115094456A