A method for in-situ SEM observation of nucleation and growth behavior of copper ion electrodeposition
By employing a quasi-in-situ method of feature marking and SEM observation on titanium cathodes, the correlation between the microstructure of titanium cathodes and the nucleation and growth behavior of copper ion electrodeposition was resolved, thereby improving the quality of copper foil and providing theoretical support.
Patent Information
- Application Number
- CN202311365731.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-20
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-10-20
AI Technical Summary
Existing technologies lack quasi-in-situ observation methods, which cannot effectively reveal the correspondence between the microstructure of cathode titanium materials and the nucleation and growth behavior of copper ion electrodeposition, thus limiting the development of electrocrystallization epitaxial growth theory and the improvement of copper foil quality.
A quasi-in-situ method involving feature marking on a titanium cathode and SEM observation was employed to track the morphological changes of the copper deposition layer at different times. This included preparing titanium cathode samples, surface treatment, feature marking, electrodeposition, and SEM observation. The feature marking depth was ensured to be greater than the final thickness of the copper deposition layer, and the morphological changes were recorded using SEM at different magnifications.
This study enabled intuitive point-to-point tracking of the copper ion electrodeposition process, revealed the influence of titanium cathode grain characteristics on the nucleation and growth behavior of copper ions, provided a theoretical basis for the design and fabrication of titanium cathodes for electrolytic copper foil, and improved the quality of copper foil.
Smart Images

Figure CN117434096B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal material sample preparation and electrodeposition morphology observation and characterization technology, specifically a quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior. Background Technology
[0002] When copper ions are electrodeposited on a titanium roller, in the initial period after energization, copper atoms preferentially enter the existing lattice positions on the titanium roller surface under the influence of the force field on the titanium substrate surface. The deposited layer formed by the lattice can be completely consistent with the crystal orientation of the titanium roller surface. This phenomenon of the deposited layer inheriting the lattice growth of the substrate is called epitaxial growth. At the microscopic level, the lattice size, arrangement, grain size, and grain geometry of the cathode roller titanium surface determine the electrochemical properties of the cathode roller surface, which in turn affect the crystallization state and crystal arrangement growth of the initial copper ion deposited layer. Therefore, the essence of electrolytic copper foil formation is the continuation of electrocrystallization products of copper ions on the lattice of the cathode roller titanium material. The microstructure and surface state of the cathode roller titanium material directly affect the nucleation and growth process of copper ion electrodeposition. Studying the nucleation and growth behavior of copper ions on the cathode titanium material during the electrodeposition preparation of copper foil, and revealing the influence of the cathode titanium material's microstructure characteristics on the inherited characteristics of the initial copper deposited layer's microstructure, is the basis for the microstructure regulation of the cathode titanium material. However, due to the challenges of quasi-in-situ observation techniques for the electrodeposition process and the lack of a correspondence between the microstructure of cathode titanium materials and the nucleation and growth evolution behavior of copper ions, the development of intermetallic electrocrystallization epitaxial growth theory and research on improving copper foil quality based on the microstructure regulation of cathode titanium materials have been constrained. Summary of the Invention
[0003] To address the shortcomings of existing technologies, this invention provides a quasi-in-situ SEM observation method for the nucleation and growth behavior of copper ions on a titanium cathode. This method can obtain the grain morphology of titanium material in the same region and the evolution process of the initial deposition layer for the formation and growth of copper nuclei at the corresponding location. It can be used to reveal the influence of the grain structure characteristics of the cathode titanium material on the nucleation and growth behavior of copper ions.
[0004] To achieve the above objectives, the specific solution adopted by the present invention is as follows: A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior on titanium cathodes, tracking the morphological evolution of copper deposition layers at the same location on titanium cathode samples at different deposition times, specifically includes the following steps: (1) Preparation of titanium cathode sample Argon gas is introduced into the heat treatment furnace as a protective gas and the furnace temperature is raised to the target temperature of 500℃~600℃. After reaching the temperature, the original titanium sample of the spun cathode roller is placed in the furnace for heat treatment to obtain the recrystallized titanium cathode sample. (2) Surface treatment of titanium cathode samples The surface of each titanium cathode sample to be deposited is treated to reveal the grain boundary features of the surface to be deposited. (3) Processing of feature markers Feature marks were processed on the surface to be deposited of the surface-treated titanium cathode sample, and photographs were taken to record the full appearance of the feature marks. (4) Record the SEM morphology of the titanium surface grains in the target area. Select a clean area near the feature mark as the target area, and take a picture to record the SEM morphology of the sample surface grains within the target area; (5) Copper ion electrodeposition Copper ions were electrodeposited in an electrolytic cell under DC conditions to obtain an electrodeposited sample. (6) SEM observation of copper deposits The electrodeposited sample was transferred to a scanning electron microscope (SEM). First, the feature markers were located in the SEM field of view, and the tilt angle of the feature markers in the image was adjusted to correspond to the original position before deposition. After finding the same target area as before deposition, the sample position was kept still, and the images were taken step by step from low magnification to high magnification. Then, the target area was adjusted to the required magnification to record the SEM morphology of the copper ion deposition surface. (7) SEM observation of copper deposits at different cumulative deposition times Repeat steps (5) to (6) and accumulate the copper ion deposition time. Take pictures of the surface morphology of the copper deposition layer under different accumulated deposition times. In turn, obtain the quasi-in-situ SEM morphology of the copper electrodeposition nucleation and growth process in the same target area with different accumulated deposition times.
[0005] Furthermore, in step (1), the original sample of the spun cathode roller titanium material is a small titanium sheet cut from the titanium cylinder by wire cutting. The titanium cylinder is obtained by integral spun forming of industrial pure titanium TA1.
[0006] Further, in step (2), the titanium cathode sample is subjected to surface treatment by mechanical grinding, electrolytic polishing and chemical etching in sequence, wherein the chemical etching time is 120 s.
[0007] Furthermore, in step (3), the depth of the feature marker is greater than the final thickness of the copper deposition layer.
[0008] Furthermore, in step (4), the images obtained are several SEM morphology images with magnification ranging from 50 to 1000 times.
[0009] Furthermore, in step (5), the electrolyte contains copper ions, sulfuric acid, gelatin and SPS, wherein the concentration of copper ions is 100 g / L, the concentration of sulfuric acid is 95 g / L, the concentration of gelatin is 5 mg / L and the concentration of SPS is 0.3 mg / L.
[0010] A titanium cathode sample was used as the cathode, and iridium-plated titanium material was used as the anode. The distance between the cathode and anode was 6 cm. The back and sides of the cathode plate were bonded together with insulating adhesive. The deposition current density remained constant at 16.7 ± 0.1 A / dm³. 2 After deposition, immediately clean the copper deposition surface with deionized water, peel off the insulating adhesive, and rinse and dry with alcohol.
[0011] Furthermore, during the electrodeposition process, a constant temperature water bath is used to keep the electrolytic cell at 50°C.
[0012] Furthermore, low-speed magnetic stirring is performed during electrodeposition.
[0013] Furthermore, the deposition time was controlled by momentarily cutting off the power during the initial electrodeposition.
[0014] Furthermore, in step (7), steps (5) to (6) are repeated three times, with the cumulative deposition times for the three times being 3 s, 10 s, and 30 s, respectively.
[0015] Beneficial effects: 1) The quasi-in-situ SEM observation method designed in this invention can intuitively track the nucleation and growth behavior of copper ion electrodeposition process at specific points. It overcomes the problem that the evolution of the grain structure characteristics of titanium cathode and the initial deposited layer of copper ion structure characteristics cannot be directly correlated. It details the growth process of copper ion deposition in the same area on titanium cathode, and reveals the influence of titanium cathode grain characteristics on the nucleation and growth behavior of copper ion electrodeposition. It provides a theoretical basis for promoting the design and preparation of titanium cathodes for electrolytic copper foil.
[0016] 2) Using diamond tools or a Vickers hardness tester, feature marks are machined on the surface of the titanium cathode sample to be deposited, enabling rapid and accurate location and tracking of the same target area. Additionally, ensure the depth of the feature marks is greater than the final thickness of the copper deposition layer to be observed to avoid the inability to track the mark position after multiple depositions.
[0017] 3) Before the electrodeposition experiment, the titanium cathode was surface-treated by electrolytic polishing and chemical etching. Electrolytic polishing can remove surface stress on the titanium cathode and avoid the influence of defects such as scratches on electrodeposition; chemical etching reveals the grain morphology characteristics, making it convenient to observe the evolution process of copper nucleus formation and growth at different grain characteristics, and the operation is simple. Attached Figure Description
[0018] Figure 1 This is a schematic diagram showing the relative position of the "cross" shaped feature mark on the surface of the titanium sample to be deposited and the target area.
[0019] Figure 2This is a SEM image of the titanium sample to be deposited on the surface marked with a cross in Example 1 of the present invention.
[0020] Figure 3 The images show the SEM morphology and a magnified high-magnification image of a portion of the structure at 1 second after copper electrodeposition in Example 1 of this invention.
[0021] Figure 4 The images show the SEM morphology and a magnified high-magnification image of a portion of the structure after copper electrodeposition for 3 seconds in Example 1 of this invention.
[0022] Figure 5 The images show the SEM morphology and a magnified high-magnification image of a portion of the structure after copper electrodeposition for 10 seconds in Example 1 of this invention.
[0023] Figure 6 The images show the SEM morphology and a magnified high-magnification image of a portion of the structure after copper electrodeposition for 30 seconds in Example 1 of this invention. Detailed Implementation
[0024] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the protection scope of the present invention.
[0025] This invention provides a quasi-in-situ SEM scanning observation method for copper electrodeposition nucleation and growth behavior, comprising the following steps: (1) Preparation of several titanium cathode samples with different grain sizes: Argon gas was introduced into a vacuum atmosphere tube resistance furnace as a protective gas, and the furnace temperature was raised to the target temperature of 500℃~600℃. After reaching the temperature, the original sample of the spun cathode roller titanium material was placed in the heat treatment furnace and kept at the temperature for 60 min to obtain the titanium cathode sample; wherein, the original sample of the spun cathode roller titanium material was a 24 mm×12 mm×4 mm small titanium sheet cut from the titanium cylinder by wire cutting. The titanium cylinder was obtained by integral spinning of industrial pure titanium TA1. The outer diameter of the spun titanium cylinder was 2700~3000 mm, the wall thickness was 20~25 mm, and the spinning deformation was 50%~60%; (2) Surface treatment of titanium cathode sample: The deposition surface of the heat-treated titanium cathode sample is subjected to mechanical grinding, electrolytic polishing and chemical etching in sequence. The chemical etching time is 120 s to make the grain boundary characteristics of the titanium cathode sample visible. (3) Processing of feature marks: Use diamond tools or Vickers hardness testers to process feature marks on the surface of the titanium cathode to be deposited. It should be noted that the depth of the feature marks should be greater than the final thickness of the copper deposition layer to be observed. Take low-magnification (50x~1000x) pictures to record the full position of the feature marks, which will facilitate the subsequent positioning of the target area of the sample at different electrodeposition times. (4) SEM observation of the grain characteristics of titanium material surface: Select a clean area near the feature mark as the target area, and take pictures to record the SEM morphology of the grains on the sample surface in the target area. (5) Copper ion electrodeposition experiment: Copper ion electrodeposition experiments were conducted in an electrolytic cell under DC conditions. The electrolyte composition was: copper ion concentration 100 g / L, sulfuric acid concentration 95 g / L, gelatin concentration 5 mg / L, and SPS concentration 0.3 mg / L. Titanium cathode samples with different grain sizes were used as cathodes, and iridium-plated titanium materials were used as anodes. The distance between the cathode and anode was fixed at 6 cm. The back and sides of the cathode plate were sealed with insulating adhesive to prevent interference with the contact current and reduce the current efficiency. The deposition current density was kept constant at 50℃ using a constant temperature water bath at 16.7 ± 0.1 A / dm³. 2 During electrodeposition, a slight magnetic stirring is applied. After deposition, the copper deposition surface is immediately rinsed with deionized water, the insulating adhesive is removed, and the surface is rinsed and dried with alcohol. It should be noted that the deposition time is controlled by momentarily cutting off the power during the first electrodeposition to obtain the initial deposition characteristics of copper ions. (6) SEM observation of copper deposition layer: Transfer the electrodeposited sample to a scanning electron microscope (SEM). First, find the feature markers in the SEM field of view and adjust the tilt angle of the feature markers in the image to correspond to the pre-deposition area. Find the target area that is the same as before the deposition. Select a relatively clean area near the feature marker as the target area. Keep the sample position still and take pictures step by step from low magnification to high magnification to locate the area at different deposition times. Then, adjust the target area to the magnification required for actual use and record the SEM morphology of the copper ion deposition surface. (7) SEM observation of the surface morphology of copper deposited layer under different deposition time: Repeat steps (5)~(6) and accumulate the copper ion deposition time, take pictures of the surface morphology of copper deposited layer of sample at different accumulated deposition time, and obtain quasi-in-situ SEM observation of copper electrodeposition nucleation growth process in the same target area at different accumulated deposition time.
[0026] In step (4), the SEM observation equipment used for the grain characteristics of the titanium surface is model JSM-7800 with a scanning voltage of 20.0 kV. When the target area is selected and the first SEM image is acquired, it is necessary to ensure that the image is 50 times to 1000 times larger to facilitate the accurate positioning of the same target area of samples with different cumulative deposition times.
[0027] The present invention will now be described in further detail with reference to the accompanying drawings and embodiments.
[0028] First, the source of the original samples in the following embodiments will be explained. The original samples are several titanium sheets cut from the cathode roller shape by wire cutting, with a size of 24 mm (tangential) × 12 mm (axial) × 4 mm (radial). The cathode roller shape is manufactured by integral spinning using industrial pure titanium TA1.
[0029] Example 1 A quasi-in-situ SEM scanning observation method for copper electrodeposition nucleation and growth behavior includes the following steps: (1) Argon gas is introduced into the vacuum atmosphere tube resistance furnace as a protective gas, and the furnace temperature is raised to the target temperature of 500℃. After the temperature is reached, the original titanium material sample of the spun cathode roller is placed in the heat treatment furnace and kept at the temperature for 60 min to obtain the titanium cathode sample. (2) The titanium cathode sample obtained by heat treatment was ground with metallographic sandpaper of No. 240, No. 400, No. 500, No. 600, No. 800, No. 1000, No. 2000 and No. 3000 in sequence. After grinding, the sample was subjected to electrolytic polishing treatment with a constant current of 2.5A for 110s. After polishing, the surface was cleaned and dried, and then chemical etching was performed. The volume ratio of the etching liquid was hydrofluoric acid: nitric acid: water = 1:2:100, and the etching time was 120s, so that the grain boundary morphology of the titanium material surface could be revealed. (3) Using a diamond tool, easily identifiable "cross" shaped scratches are machined on the surface of the titanium cathode sample to be deposited, such as... Figure 1 As shown; (4) The titanium sample was prepared according to Figure 1 The sample was fixed on the SEM sample stage in the orientation shown, with the long side of the sample parallel to side AB of the sample stage. The scanning voltage was 20.0 kV. SEM observation was performed on the relatively clean area near the feature marks. The average grain size of the titanium surface was found to be approximately 5.6 μm. The results are as follows: Figure 2 ; (5) The titanium sample was removed and copper foil electrodeposition experiment was conducted: Copper foil was prepared by direct current electrodeposition in an electrolytic cell. The electrolyte composition was as follows: copper ion concentration of 100 g / L, sulfuric acid concentration of 95 g / L, gelatin concentration of 5 mg / L, and SPS concentration of 0.3 mg / L. The titanium sample to be deposited was used as the cathode, and an iridium-coated titanium plate was used as the anode. The distance between the cathode and anode was fixed at 6 cm. The back and sides of the plates were bonded together with insulating adhesive, and the deposition area was fixed at 15 mm × 12 mm. The solution was kept at 50℃ in a constant temperature water bath, and the density was kept constant at 16.7 ± 0.1 A / dm³. 2During electrodeposition, a slight magnetic stirring is applied. After 1 second of deposition, the insulating adhesive is peeled off, rinsed several times with deionized water, rinsed with alcohol, and then dried with cold air. (6) Following the same setup method as before titanium sample deposition, the deposited sample was placed on the scanning electron microscope (SEM) stage. Based on the characteristic markings, the same target area was located. The SEM image was finely adjusted by rotation until the long scratch on the sample intersected with the upper edge of the SEM field of view. At this point, the field of view included part of the scratch marking and the area affected by the marking. To remove the influence of this scratch defect area on the SEM morphology observation, the sample position was kept unchanged, and the magnification was adjusted to 1000x for the first SEM observation of the copper ion deposition structure. The results are as follows: Figure 3 ; (7) Repeat steps (5) to (6) for a cumulative deposition time of 3 seconds, and perform a second SEM observation of the copper ion deposition morphology. The results are as follows: Figure 4 ; (8) Repeat step (7) for a cumulative deposition time of 10 seconds, and perform a third SEM observation of the copper ion deposition morphology. The results are as follows: Figure 5 ; (9) Repeat step (8) for a cumulative deposition time of 30 seconds, and perform a third SEM observation of the copper ion deposition morphology. The results are as follows: Figure 6 ; from Figure 3 , 4 As can be seen in sections 5 and 6, the method of this invention can achieve SEM tracking of the evolution of the microstructure morphology of copper ion electrodeposition in the same region on the surface of a titanium cathode with an average grain size of approximately 5.6 μm. The results show that copper ions preferentially nucleate at grain boundaries. With prolonged deposition time, copper deposition particles cluster and connect in series at the grain boundaries, further expanding into the grain until they cover the entire grain. Simultaneously, comparing titanium grains of different sizes in the target region reveals that the titanium grain size affects the nucleation rate of copper ion electrodeposition. The smaller the titanium grain size, the faster the copper ion nucleation rate, and the shorter the time required for copper particles to expand into the grain to achieve full coverage. Furthermore, copper particles can fill the entire grain or reach the target deposition thickness in a shorter time.
[0030] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of the invention in any way. All equivalent transformations or modifications made in accordance with the essence of the present invention should be covered within the protection scope of the present invention.
Claims
1. A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior, characterized in that, Includes the following steps: (1) Preparation of titanium cathode sample Argon gas is introduced into the heat treatment furnace as a protective gas and the furnace temperature is raised to the target temperature of 500℃~600℃. After reaching the temperature, the original titanium sample of the spun cathode roller is placed in the furnace for heat treatment to obtain the recrystallized titanium cathode sample. (2) Surface treatment of titanium cathode samples The surface of each titanium cathode sample to be deposited is treated to reveal the grain boundary features of the surface to be deposited. (3) Processing of feature markers Feature marks were processed on the surface to be deposited of the surface-treated titanium cathode sample, and photographs were taken to record the full appearance of the feature marks. (4) Record the SEM morphology of the titanium surface grains in the target area. Select a clean area near the feature mark as the target area, and take a picture to record the SEM morphology of the sample surface grains within the target area; (5) Copper ion electrodeposition Copper ions were electrodeposited in an electrolytic cell under DC conditions to obtain an electrodeposited sample. (6) SEM observation of copper deposits The electrodeposited sample was transferred to a scanning electron microscope (SEM). First, the feature markers were located in the SEM field of view, and the tilt angle of the feature markers in the image was adjusted to correspond to the original position before deposition. After finding the same target area as before deposition, the sample position was kept still, and the images were taken step by step from low magnification to high magnification. Then, the target area was adjusted to the required magnification to record the SEM morphology of the copper ion deposition surface. (7) SEM observation of copper deposits at different cumulative deposition times Repeat steps (5) to (6) and accumulate the copper ion deposition time. Take pictures of the surface morphology of the copper deposition layer under different accumulated deposition times. In turn, obtain the quasi-in-situ SEM morphology of the copper electrodeposition nucleation and growth process in the same target area with different accumulated deposition times.
2. A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior according to claim 1, characterized in that: In step (1), the original sample of the spun cathode roller titanium material is a small titanium sheet cut from the titanium cylinder by wire cutting. The titanium cylinder is obtained by integral spinning of industrial pure titanium TA1.
3. A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior according to claim 1, characterized in that: In step (2), the titanium cathode sample is subjected to surface treatment by mechanical grinding, electrolytic polishing and chemical etching in sequence, wherein the chemical etching time is 120 s.
4. A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior according to claim 1, characterized in that: In step (3), the depth of the feature marker is greater than the final thickness of the copper deposit.
5. A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior according to claim 1, characterized in that: In step (4), the photos obtained are several SEM morphology images with magnification ranging from 50 to 1000 times.
6. A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior according to claim 1, characterized in that: In step (5), the electrolyte contains copper ions, sulfuric acid, gelatin and SPS, wherein the concentration of copper ions is 100 g / L, the concentration of sulfuric acid is 95 g / L, the concentration of gelatin is 5 mg / L and the concentration of SPS is 0.3 mg / L. A titanium cathode sample was used as the cathode, and iridium-plated titanium material was used as the anode. The distance between the cathode and anode was 6 cm. The back and sides of the cathode plate were bonded together with insulating adhesive. The deposition current density remained constant at 16.7 ± 0.1 A / dm³. 2 After deposition, immediately clean the copper deposition surface with deionized water, peel off the insulating adhesive, and rinse and dry with alcohol.
7. A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior according to claim 6, characterized in that: During the electrodeposition process, a constant temperature water bath is used to keep the electrolytic cell at 50°C.
8. A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior according to claim 6, characterized in that: Low-speed magnetic stirring is used during electrodeposition.
9. A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior according to claim 6, characterized in that: The deposition time was controlled by momentarily cutting off the power during the first electrodeposition.
10. A quasi-in-situ SEM observation method for copper ion electrodeposition nucleation and growth behavior according to claim 1, characterized in that: In step (7), steps (5) to (6) are repeated three times, and the cumulative deposition times for the three times are 3 s, 10 s, and 30 s, respectively.
Citation Information
Patent Citations
Method for measuring austenite grain size of low alloy steel in heat treatment process
CN110487985A
Development method for three-dimensional morphology of boride in gamma-TiAl-based alloy