Composite metal lithium negative electrode and preparation method and use thereof

By designing an ellipsoidal lithium-carbon material cocoon structure, the problems of lithium dendrite growth and volume expansion in the lithium metal anode were solved, achieving a stable solid electrolyte membrane and high energy density, and improving cycle life and coulombic efficiency.

CN117438536BActive Publication Date: 2026-11-24CHINA ENERGY LITHIUM
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210817431.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-12
Publication Date
2026-11-24
Estimated Expiration
2042-07-12

AI Technical Summary

Technical Problem

Existing technologies struggle to form a stable solid electrolyte membrane in lithium metal anodes and provide sufficient space for lithium dendrite growth and volume expansion, leading to a decrease in cycle life and coulombic efficiency.

Method used

A composite lithium metal anode is designed using ellipsoidal lithium-carbon material. The structural carbon materials interweave to form a three-dimensional cocoon structure, which is combined with a lithium metal core to form a cocoon structure. The ratio and shape ratio of the structural carbon material to the lithium metal are optimized. The cocoon structure lithium-carbon material is formed by high-speed dispersion and spray drying, and the ellipsoid is formed by pressure control on the current collector.

Benefits of technology

It improves the cycle life and energy density of the negative electrode, reduces contact resistance, forms a stable solid electrolyte membrane, solves the problems of lithium dendrite growth and volume expansion, and has good cycle performance and high energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117438536B_ABST
    Figure CN117438536B_ABST
Patent Text Reader

Abstract

This invention relates to a composite lithium metal anode, its preparation method, and its applications. The composite lithium metal anode includes an active material layer containing an ellipsoidal lithium-carbon material. The lithium-carbon material has a cocoon structure, comprising a cocoon formed of structural carbon material and one or more lithium metal cores contained within the cocoon. The structural carbon materials interweave to form a three-dimensional cocoon structure, providing sufficient space for lithium metal dendrite growth and volume expansion while facilitating the formation of a stable solid electrolyte membrane, resulting in a long cycle life for the anode. The anode has a low thickness and low contact resistance, making it suitable for fabricating high-energy-density lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium battery technology, specifically to a composite lithium metal anode, its preparation method, and its applications. Background Technology

[0002] Lithium metal possesses a high theoretical specific capacity (3860 mAh / g) and a low potential (-3.04 V vs SHE), making it an ideal anode material. However, lithium metal is chemically reactive and exhibits significant drawbacks during use. For instance, the large volume expansion during lithium deposition / stripping cycles easily leads to lithium dendrite formation, resulting in decreased coulombic efficiency and even serious safety issues such as short circuits, thus limiting the commercial application of lithium metal.

[0003] Currently, constructing a three-dimensional framework to provide sufficient space for lithium dendrites and volume expansion is a research hotspot. CN114203963A discloses a carbon-material lithium-metal composite anode, its preparation method, and applications. This carbon-material lithium-metal composite anode is composed of a surface-modified three-dimensional carbon material current collector built on a copper foil surface and lithium metal. By surface-treating the carbon material to improve the lithiophilicity of the three-dimensional current collector, and then using electrochemical deposition or molten lithium infusion to composite the lithium metal with the three-dimensional current collector, the cycle stability of the carbon-material lithium-metal composite anode is improved. Although choosing carbon material as the three-dimensional current collector is a good choice, lithium metal tends to deposit on the surface of the three-dimensional current collector, which is not conducive to the formation of a stable solid electrolyte interphase (SEI) membrane.

[0004] CN108365202A discloses a lithium-carbon composite material comprising alternating lithium and carbon layers, wherein both the bottom and top layers of the composite material are carbon layers. The carbon and lithium layers are stacked by hand or mechanical pressing, resulting in poor interlayer contact. With immersion in the electrolyte and during charge-discharge cycles, the layered structure collapses, affecting the material's cycle performance. Furthermore, the compacted carbon layers have small pores, failing to provide sufficient space for lithium dendrite growth and volume expansion.

[0005] Based on the above literature, it is clear that how to facilitate the formation of a stable solid electrolyte membrane while providing sufficient space for the growth and volume expansion of lithium metal dendrites, thereby improving the cycle life of composite lithium metal anodes, has become an urgent problem to be solved at this stage. Summary of the Invention

[0006] In view of the problems existing in the prior art, the present invention provides a composite lithium metal anode, its preparation method, and its uses. The anode comprises an ellipsoidal lithium-carbon material with a cocoon structure, wherein the structural carbon materials are interwoven to form a three-dimensional cocoon structure, which not only provides sufficient space for the growth and volume expansion of lithium metal dendrites, but also facilitates the formation of a stable solid electrolyte film on the anode surface. The ellipsoidal shape of the lithium-carbon composite material effectively reduces the anode thickness and contact resistance, resulting in a longer cycle life and higher energy density. The method is simple to operate, has low production costs, and has high application value.

[0007] To achieve this objective, the present invention adopts the following technical solution:

[0008] In a first aspect, the present invention provides a composite lithium metal anode, the composite lithium metal anode comprising an active material layer, the active material layer comprising an ellipsoidal lithium-carbon material having a cocoon structure, the cocoon structure comprising a cocoon formed of structural carbon material and one or more lithium metal cores contained in the cocoon.

[0009] In this invention, the high specific surface area, high aspect ratio, and easy bending deformation of structural carbon materials are utilized, combined with the good ductility of the lithium metal core, to ingeniously design a composite lithium metal anode with an ellipsoidal cocoon structure. The structural carbon materials interweave to form a three-dimensional cocoon structure, which possesses good stability and conductivity, facilitating the formation of a stable solid electrolyte film on the anode surface. Simultaneously, it provides sufficient space for lithium metal dendrite growth and volume expansion, resulting in excellent cycle performance of the anode. By designing the lithium carbon material to have an ellipsoidal shape, the anode thickness and contact resistance are reduced, effectively improving the battery's energy density.

[0010] Optionally, the thickness of the negative electrode active material layer is 1-200 μm, for example, it can be 1.5 μm, 3 μm, 5 μm, 10 μm, 20 μm, 30 μm, 50 μm, 80 μm, 100 μm, 120 μm, 150 μm, 180 μm, and 200 μm, preferably 10-150 μm. The thickness of the film layer is designed according to actual needs. If the thickness is too large, ion migration is slow, affecting the electrochemical response; if there is too much negative electrode, it will reduce the energy density of the battery. If the thickness is too small, it is not easy to form a uniform and stable active material layer.

[0011] Optionally, the major axis of the lithium-carbon material (measured by the major axis for ellipsoidal lithium-carbon materials) is 1-100 μm, for example, it can be 1 μm, 3 μm, 5 μm, 7 μm, 10 μm, 15 μm, 20 μm, 25 μm, 40 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 90 μm, 95 μm, and 100 μm. Preferably, it is 5-60 μm, and more preferably 10-30 μm.

[0012] Optionally, the minor axis of the ellipsoidal lithium-carbon material is 1-60 μm, for example, it can be 1 μm, 2 μm, 3 μm, 5 μm, 7 μm, 10 μm, 12 μm, 15 μm, 17 μm, 20 μm, 25 μm, 40 μm, 42 μm, 45 μm, 48 μm, 50 μm, 55 μm, or 60 μm. Preferably, it is 3-45 μm, and more preferably 5-20 μm.

[0013] Optionally, the structural carbon material used to form the lithium-carbon material includes any one or a combination of at least two of fibrous carbon materials, tubular carbon materials, or sheet-like carbon materials. Carbon materials of a specific shape can be wound around the surface of the metallic lithium core, which facilitates the interweaving to form a stable cocoon, preferably any one or a combination of at least two of carbon nanotubes, carbon fibers, or graphene.

[0014] In this invention, the types of carbon nanotubes, carbon fibers, or graphene are not specifically limited. They can be carbon nanotubes doped with lithium-loving elements such as nitrogen and phosphorus, carbon fibers deposited with lithium-loving metal particles such as Ag, Sn, and Zn, or hollow carbon nanotubes deposited with lithium-loving compounds such as Co3O4, SnS2, and Ni2P. Any material that can perform the same function as this invention is applicable to this invention.

[0015] Optionally, the lithium metal core includes a pure lithium metal core and / or a lithium metal core containing a protective layer.

[0016] In this invention, the protective layer includes, but is not limited to, a passivation layer formed by lithium fluoride, lithium carbonate, etc., and an organic conductive layer formed by polyethylene oxide, polyethylene glycol, polysiloxane, polytrimethylene carbonate, polycarbonate, polyvinyl carbonate, polypropylene carbonate, polyvinyl carbonate, polyvinylidene carbonate, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, poly(vinylidene fluoride-hexafluoropropylene), polyphenylene sulfide, p-benzoquinone, and copolymers or mixtures of at least two of the above polymers.

[0017] As a preferred technical solution of the present invention, the mass ratio of structural carbon material to lithium metal core is 1:(200-1300), for example, it can be 1:200, 1:210, 1:240, 1:280, 1:300, 1:350, 1:380, 1:420, 1:470, 1:500, 1:550, 1:600, 1:700, 1:800, 1:900, 1:930, 1:960, 1:1000, 1:1050, 1:1150, 1:1200, 1:1250, or 1:1300, etc. The mass ratio can form a good cocoon structure, and at the same time, the content of structural carbon material in the negative electrode is low, which is beneficial to improving the energy density of the battery. Preferably, it is 1:(400-1100), and more preferably 1:(500-950).

[0018] Optionally, the ratio of the short axis of the lithium metal core to the length of the structural carbon material is (1-10):1, for example, it can be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1 or 10:1, etc. If the ratio is too small (less than 1:1), the length of the carbon material is too long relative to the core, and it is easy for it to entangle itself into a spherical structure similar to a ball of yarn, which is not conducive to forming a cocoon structure of lithium carbon material; if the ratio is too large, the core is too large relative to the carbon material, and the carbon material is not easy to disperse and will stack on the surface of the lithium metal core, making it difficult to form a cocoon structure. Preferably, it is (3-7):1.

[0019] In this invention, the active material layer of the negative electrode may further include a binder and / or a conductive agent.

[0020] Optionally, the adhesive comprises any one or a combination of at least two of styrene-butadiene rubber, polystyrene, polyvinylidene fluoride, polyvinylpyrrolidone, or cyclodextrin.

[0021] Optionally, the conductive agent includes any one or a combination of at least two of acetylene black, Super P (SP), Cabot carbon black, graphene, and conductive graphite.

[0022] Optionally, based on the mass of the active material layer as 100%, the mass fraction of the lithium-carbon material is 80-99.9%, for example, it can be 80%, 85%, 90%, 95% or 99%, etc., preferably 90-99.5%. In this invention, the mass fraction of the lithium-carbon material includes metallic lithium powder and interwoven carbon material on its surface.

[0023] Optionally, the mass fraction of the adhesive is 2-10% based on the mass of the active material layer as 100%, for example, it can be 2%, 2.5%, 3%, 5%, 8% or 10%, etc.

[0024] Optionally, the mass fraction of the conductive agent is 1-10% based on the mass of the active material layer being 100%. For example, it can be 1%, 2%, 2.5%, 3%, 5%, 8%, or 10%, etc.

[0025] In a second aspect, the present invention provides a method for preparing a negative electrode as described in the first aspect above, the method comprising the following steps:

[0026] (1) Mix structural carbon material, organic solvent and lithium metal powder, and then disperse and / or spray dry to obtain lithium carbon material containing one or more lithium metal cores in the cocoon;

[0027] (2) The lithium-carbon material in step (1) is placed on the current collector, and then the lithium-carbon material is made into an ellipsoid by pressure control to obtain a composite lithium metal anode.

[0028] In this invention, the organic solvent in step (1) is not specifically limited. The organic solvent may include, but is not limited to, any one or a combination of at least two of the following: liquid aliphatic alkanes such as n-hexane, liquid cycloalkanes such as cyclohexane, N-methylpyrrolidone, benzene, p-xylene, carbon tetrachloride, tetrahydrofuran, liquid paraffin, or 1,2-dichloroethane.

[0029] In this invention, structural carbon materials and lithium metal powder are dispersed in an organic solvent system. Then, by applying high shear force (high-speed dispersion or spray drying), the structural carbon materials interweave and entwine on the surface of the lithium metal powder, forming a cocoon-like lithium-carbon material with lithium metal powder as the core and structural carbon materials as the shell. Pressure is applied to this lithium-carbon material (after it is placed on the surface of the current collector as an active material), causing the lithium-carbon material to form an ellipsoidal shape, thus obtaining a composite lithium metal anode. The preparation method is simple and easy to implement, and readily applicable for industrial application.

[0030] Optionally, the structural carbon material in step (1) includes any one or a combination of at least two of fibrous, tubular, or sheet-like carbon materials, preferably any one or a combination of at least two of carbon nanotubes, carbon fibers, or graphene.

[0031] Optionally, the lithium metal powder in step (1) includes pure lithium metal powder and / or lithium metal powder containing a protective layer.

[0032] Optionally, the lithium metal powder in step (1) may have a spherical or near-spherical shape.

[0033] Optionally, the average particle size of the lithium metal powder in step (1) is 1-80 μm, for example, it can be 1 μm, 3 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 50 μm, 60 μm, 70 μm, 75 μm, 80 μm, etc., preferably 5-60 μm, and more preferably 10-30 μm.

[0034] Optionally, the ratio of the average particle size of the lithium metal powder to the length of the structural carbon material in step (1) is (1-10):1, for example, it can be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1 or 10:1, etc.

[0035] Optionally, the mass ratio of the structural carbon material to the lithium metal powder in step (1) is 1:(200-1300), for example, it can be 1:200, 1:210, 1:240, 1:280, 1:300, 1:350, 1:380, 1:420, 1:470, 1:500, 1:550, 1:600, 1:700, 1:800, 1:900, 1:930, 1:960, 1:1000, 1:1050, 1:1150, 1:1200, 1:1250 or 1:1300, etc. The mass ratio can form a good cocoon structure while having a low content in the negative electrode, which is beneficial to improving the energy density of the battery. Preferably, it is 1:(400-1100), and more preferably 1:(500-950).

[0036] Optionally, the dispersion rate of high-speed dispersion in step (1) is 5000-20000 rpm, for example, it can be 5000 rpm, 6000 rpm, 7000 rpm, 8000 rpm, 9000 rpm, 10000 rpm, 11000 rpm, 12000 rpm, 13000 rpm, 14000 rpm, 15000 rpm, 17000 rpm, 19000 rpm or 20000 rpm, etc., preferably 6000-15000 rpm.

[0037] Optionally, the high-speed dispersion time in step (1) is 1-10 min, for example, it can be 1 min, 1.5 min, 2 min, 2.5 min, 3 min, 3.5 min, 4 min, 4.5 min, 5 min, 6 min, 7 min, 8 min, 9 min, 9.5 min or 10 min, preferably 3-5 min.

[0038] Optionally, the spray drying conditions in step (1) include: an inlet air temperature of 180-240℃, preferably 200-220℃; an outlet air temperature of 90-110℃, preferably 100-110℃; and an atomization pressure of 0.1-0.5 MPa, preferably 0.2-0.4 MPa.

[0039] As an optional technical solution of the present invention, a stabilizer may be added during the mixing process in step (1). The stabilizer includes, but is not limited to, any one or a combination of at least two of styrene-butadiene rubber, polyvinyl alcohol, polystyrene, polyvinylidene fluoride, polyvinylpyrrolidone, or cyclodextrin. The selection of a stabilizer is beneficial to the stable existence of the structural carbon material in organic solvents, forming a cocoon-structured lithium-carbon material with a better morphology.

[0040] Optionally, the mass ratio of the stabilizer to the structural carbon material is 1:(5-60), for example, it can be 1:5, 1:7, 1:10, 1:12, 1:15, 1:20, 1:25, 1:30, 1:35, 1:37, 1:40, 1:45, 1:50, 1:55 or 1:60, etc., preferably 1:(10-40).

[0041] Optionally, the pressure in step (2) is 10-100 MPa, for example, it can be 10 MPa, 15 MPa, 20 MPa, 23 MPa, 25 MPa, 27 MPa, 30 MPa, 40 MPa, 50 MPa, 60 MPa, 70 MPa, 75 MPa, 80 MPa, 90 MPa or 100 MPa. If the pressure is too low, the deformation of the lithium carbon material is small, the shape is close to a circle, and the negative electrode active material layer is thick, which is not conducive to the preparation of high energy density batteries. If the pressure is too high, it will destroy the cocoon structure of the lithium carbon material, which is not conducive to improving the cycle performance of the negative electrode. Preferably, it is 25-80 MPa.

[0042] As a further preferred technical solution of the present invention, the pressure control in step (2) is achieved by controlling the compaction density through cold pressing and then controlling the morphology of the lithium-carbon material through hot pressing; or, the morphology of the lithium-carbon material is controlled by hot pressing first, and then the compaction density is controlled by cold pressing.

[0043] In this invention, the cold pressing and hot pressing work together to achieve the designed thickness of the negative electrode active material layer while controlling the shape of the lithium-carbon material.

[0044] Optionally, the thickness of the cold-pressed active material layer is 1.3-1.9 times the thickness of the negative electrode active material layer, for example, it can be 1.3, 1.5, 1.52, 1.55, 1.57, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.88 or 1.9, etc.

[0045] Optionally, the hot pressing temperature is 60-180℃, for example, it can be 60℃, 65℃, 70℃, 75℃, 80℃, 90℃, 95℃, 100℃, 105℃, 110℃, 120℃, 130℃, 140℃, 145℃, 150℃, 155℃, 160℃, 170℃, 175℃ or 180℃, etc. If the temperature is too high, the cocoon structure will be destroyed during the process of lithium carbon material becoming ellipsoidal, and if the temperature is too low, it is not conducive to the lithium carbon material becoming ellipsoidal. Preferably, it is 100-150℃.

[0046] Optionally, the current collector in step (2) includes any one or a combination of at least two of three-dimensional carbon current collector, copper foil, copper foam, nickel foil or nickel foam, preferably any one or a combination of at least two of three-dimensional carbon current collector, copper foam or nickel foam.

[0047] Optionally, before pressure control in step (2), the following operation is performed: mixing lithium-carbon material, conductive agent, and binder. In this invention, the addition of conductive agent to the mixed system improves the electronic conductivity of the negative electrode, especially the particulate conductive agent which can fill the gaps between the structural carbon materials, and the binder improves the bonding force between the film layer and the current collector.

[0048] Optionally, the conductive agent includes any one or a combination of at least two of acetylene black, SP, Cabot carbon black, graphene, and conductive graphite.

[0049] Optionally, the adhesive comprises any one or a combination of at least two of styrene-butadiene rubber, polyvinyl alcohol, polystyrene, polyvinylidene fluoride, polyvinylpyrrolidone, or cyclodextrin.

[0050] As a further preferred technical solution of the present invention, the method includes the following steps:

[0051] (1) The structural carbon material and organic solvent are first dispersed at high speed, and then the dispersion is dispersed at high speed with stabilizer and lithium metal powder to obtain a mixed system;

[0052] The structural carbon material includes any one or a combination of at least two of carbon nanotubes, carbon fibers, or graphene.

[0053] The organic solvent includes any one or a combination of at least two of the following: n-hexane, cyclohexane, N-methylpyrrolidone, benzene, p-xylene, carbon tetrachloride, tetrahydrofuran, liquid paraffin, or 1,2-dichloroethane.

[0054] The stabilizer includes any one or a combination of at least two of styrene-butadiene rubber, polyvinyl alcohol, polyvinylidene fluoride, polyvinylpyrrolidone, or cyclodextrin.

[0055] The lithium metal powder includes pure lithium metal powder and / or lithium metal powder containing a protective layer, with an average particle size of 10-80 μm.

[0056] The mass ratio of the structural carbon material to the lithium metal powder is 1:(400-1100), and the mass ratio of the stabilizer to the structural carbon material is 1:(10-40).

[0057] The rates of the first and second high-speed dispersions are independently 8000-10000 rpm;

[0058] (2) The lithium-carbon material in step (1) is placed on the current collector and formed into an ellipsoid by adjusting the pressure of 25-80 MPa. The current collector includes any one or at least two of three-dimensional carbon current collector, copper foam or nickel foam, to obtain a composite lithium metal anode.

[0059] Thirdly, the present invention provides a lithium battery, the lithium battery comprising a negative electrode as described in the first aspect above.

[0060] Compared with the prior art, the present invention has at least the following beneficial effects:

[0061] (1) The composite lithium metal anode provided by the present invention has interwoven structural carbon materials set on the surface of an ellipsoidal lithium metal core to form a three-dimensional cocoon structure, which provides sufficient space for the growth of lithium metal dendrites and volume expansion. At the same time, it is beneficial for the anode to form a relatively stable solid electrolyte film on the surface during cycling, so that the anode has a longer cycle life and lower resistance.

[0062] (2) By further controlling parameters such as the ratio of structural carbon material to lithium metal core and the ratio of the length of structural carbon material to the average particle size of lithium metal core in the negative electrode, the present invention obtains a negative electrode with high energy density and long cycle life.

[0063] (3) The preparation method provided by the present invention is simple to operate, has high production efficiency, and is easy to industrialize. Furthermore, the method optimizes parameters such as the length of the structural carbon material to the average particle size ratio of the lithium metal powder, the mass ratio of the structural carbon material to the lithium metal powder, and the pressure, so that the rigid structural carbon materials intertwine to form a continuous and stable three-dimensional cocoon structure, and leave enough space, effectively solving the problems of lithium metal dendrite growth and volume expansion. Attached Figure Description

[0064] Figure 1 The image shows the SEM image of the lithium-carbon material from step (1) in Example 2.

[0065] Figure 2 This is a SEM image of the negative electrode in Example 2.

[0066] Figure 3The graphs show the cycle curves of the negative electrode in Example 2 and Comparative Example 1.

[0067] Figure 4 The graphs show the cycle curves of the negative electrode in Example 2 and Comparative Example 2. Detailed Implementation

[0068] To facilitate understanding of the present invention, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of the invention.

[0069] In this invention, the impedance testing device in the embodiment is CHI660E, and the test conditions are: frequency range 100KHz-100mHz, AC amplitude 5mV.

[0070] Example 1

[0071] This embodiment provides a composite lithium metal anode, which includes an active material layer formed by an ellipsoidal lithium-carbon material with a thickness of 10 μm. The lithium-carbon material has a cocoon structure with an average major axis of 6 μm and an average minor axis of 3 μm. The cocoon structure includes a cocoon body formed by multi-walled carbon nanotubes and a lithium metal core contained in the cocoon body.

[0072] The method for preparing the negative electrode sheet includes the following steps:

[0073] (1) 1.2 g of lithium metal powder with an average particle size of 5 μm, 0.03 g of multi-walled carbon nanotubes (purchased from Beijing Deco Island Gold) dispersion with a length of 1 μm and xylene solvent were dispersed at high speed. The mass fraction of the dispersion was 3%, the rotation speed was 6000 rpm, and the time was 5 min. The mixture was filtered and dried at 70 °C to obtain lithium-carbon material with a lithium metal core coated with multi-walled carbon nanotubes.

[0074] (2) Prepare a slurry in p-xylene by mixing lithium carbon material, acetylene black and styrene-butadiene rubber in step (1) at a mass ratio of 8:1:1. Then, coat the slurry 100 μm thick on the surface of copper foil with a doctor blade. Adjust the thickness of the active material layer to 13 μm by a pressure of 25 MPa. Then, hot press it to 10 μm at 110℃ to form an ellipsoidal shape of lithium carbon material and obtain a composite lithium metal anode.

[0075] The negative electrode and lithium metal sheet are assembled into a button half-cell. After the first cycle, the measured impedance is 20Ω, at 2mA / cm. 2 and 1mAh / cm 2 Under certain conditions, it can stably cycle 390 times.

[0076] Example 2

[0077] This embodiment provides a composite lithium metal anode, which includes an active material layer formed by an ellipsoidal lithium-carbon material with a thickness of 100 μm. The lithium-carbon material has a cocoon structure with an average major axis of 70 μm and an average minor axis of 35 μm. The cocoon structure includes a cocoon body formed by single-walled carbon nanotubes and a lithium metal core contained in the cocoon body.

[0078] The method for preparing the negative electrode sheet includes the following steps:

[0079] (1) 1.2 g of lithium metal powder with an average particle size of 50 μm, 0.05 g of single-walled carbon nanotube dispersion with a length of 5 μm (purchased from Aokeshier), and hexane solvent were dispersed at high speed. The lithium metal powder had a LiF passivation layer on its surface. The mass fraction of the dispersion was 3%. The rotation speed was 10000 rpm for 3 min. The mixture was filtered and dried at 70 °C to obtain a lithium-carbon material with a lithium metal core coated with single-walled carbon nanotubes. The lithium-carbon material was characterized by SEM, as shown below. Figure 1 As shown;

[0080] (2) The lithium-carbon material in step (1) is hot-pressed at 120°C under a pressure of 50 MPa to form an ellipsoid. After hot pressing, the active material layer thickness is 150 μm. Then, it is cold-pressed to a thickness of 100 μm and bonded to the copper foil surface with conductive adhesive to obtain a composite lithium metal anode. Figure 2 The SEM image of the obtained negative electrode clearly shows that the lithium-carbon material is ellipsoidal.

[0081] The negative electrode and lithium metal sheet are assembled into a button half-cell. After the first cycle, the measured impedance is 8Ω, at 2mA / cm². 2 and 1mAh / cm 2 Under certain conditions, it can be stably cycled 500 times.

[0082] Example 3

[0083] This embodiment provides a composite lithium metal anode, the anode comprising an active material layer formed of an ellipsoidal lithium-carbon material, the active material layer having a thickness of 200 μm, the lithium-carbon material having a cocoon structure with an average major axis of 100 μm and an average minor axis of 60 μm, the cocoon structure comprising a cocoon body formed of hollow carbon nanotubes and a lithium metal core contained within the cocoon body.

[0084] The method for preparing the negative electrode sheet includes the following steps:

[0085] (1) 1.2g of lithium metal powder with an average particle size of 80μm, 0.2g of graphene (purchased from Jicang Nano JCPG-99-1-8) dispersion with a size of 8μm*8μm and carbon tetrachloride solvent were dispersed at high speed. The lithium metal powder had a polyvinyl carbonate layer on its surface. The mass fraction of the dispersion was 3%. The rotation speed was 12000rpm and the time was 1min. The mixture was filtered and dried at 80℃ to obtain a lithium-carbon material with a graphene-coated lithium metal core.

[0086] (2) The lithium-carbon material in step (1) is cold-pressed at 80 MPa to form an ellipsoid. After cold pressing, the thickness of the active material layer is 380 μm. Then, it is hot-pressed at 150℃ to 200 μm and pressed onto nickel foam to obtain a composite lithium metal anode.

[0087] The negative electrode and lithium metal sheet are assembled into a button half-cell. After the first cycle, the measured impedance is 15Ω, at 2mA / cm. 2 and 1mAh / cm 2 Under certain conditions, it can stably cycle 340 times.

[0088] Comparative Example 1

[0089] Compared to Example 2, the only difference is that the lithium-carbon material is replaced with pure lithium metal powder. The resulting negative electrode is assembled with a lithium metal sheet to form a button half-cell. After the first cycle, the measured impedance is 300Ω at 2mA / cm². 2 and 1mAh / cm 2 Under certain conditions, it can stably cycle 112 times.

[0090] Comparative Example 2

[0091] Compared to Example 2, the only difference is that the ellipsoidal lithium-carbon material is replaced with a spherical lithium-carbon material; that is, in the preparation method, the lithium-carbon material is directly adhered to the copper foil without a pressure control step. The resulting negative electrode is assembled with a lithium metal sheet to form a button half-cell. After the first cycle, the measured impedance is 126Ω at 2mA / cm². 2 and 1mAh / cm 2 Under certain conditions, it can stably cycle 180 times.

[0092] Figure 3 The cycle curves of the negative electrode in Example 2 and Comparative Example 1 are shown. Figure 4 The cycling curves of the negative electrodes in Example 2 and Comparative Example 2 are shown. Combining Example 2, Comparative Example 1, and Comparative Example 2, it can be seen that the negative electrode provided in Example 2, which has an ellipsoidal cocoon-shaped lithium-carbon material, exhibits significantly lower impedance after one cycle compared to the negative electrodes in Comparative Example 1 and Comparative Example 2. At 2 mA / cm²... 2 and 1mAh / cm 2Under these conditions, the cycle stability is significantly better than that of the negative electrode in Comparative Example 1 and Comparative Example 2.

[0093] The applicant declares that the detailed structural features of the present invention are illustrated through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions for the components selected in the present invention, additions of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A composite lithium metal anode, characterized in that, The composite lithium metal anode includes an active material layer comprising an ellipsoidal lithium-carbon material having a cocoon structure. The cocoon structure comprises a cocoon formed of structural carbon material and one or more lithium metal cores contained within the cocoon. The ellipsoidal lithium-carbon material has a major axis of 1-100 μm and a minor axis of 1-60 μm; the structural carbon material is any one or a combination of at least two of carbon nanotubes, carbon fibers, or graphene. The composite lithium metal anode is prepared by a method comprising the following steps: (1) Mix structural carbon material, organic solvent and lithium metal powder, and then disperse and / or spray dry to obtain lithium carbon material containing one or more lithium metal cores in the cocoon; (2) Place the lithium-carbon material from step (1) onto the current collector, and then use pressure control to make the lithium-carbon material into an ellipsoid. In step (2), the pressure control is achieved by controlling the compaction density through cold pressing and then controlling the morphology of the lithium-carbon material through hot pressing; or, the morphology of the lithium-carbon material is controlled by hot pressing first, and then the compaction density is controlled by cold pressing.

2. The negative electrode according to claim 1, characterized in that, The thickness of the active material layer is 1-200 μm; and / or The major axis of the ellipsoidal lithium-carbon material is 5-60 μm; the minor axis of the ellipsoidal lithium-carbon material is 3-45 μm.

3. The negative electrode according to claim 1 or 2, characterized in that, The lithium metal core includes pure lithium metal and / or lithium metal containing a protective layer.

4. The negative electrode according to claim 1, characterized in that, The mass ratio of the structural carbon material to the lithium metal core is 1:(200-1300); and / or The ratio of the short axis of the lithium metal core to the length of the structural carbon material is (1-10):

1.

5. A method for preparing a negative electrode according to any one of claims 1-4, characterized in that, The method includes the following steps: (1) Mix structural carbon material, organic solvent and lithium metal powder, and then disperse and / or spray dry to obtain lithium carbon material containing one or more lithium metal cores in the cocoon; (2) Place the lithium-carbon material from step (1) on the current collector, and then control the pressure to make the lithium-carbon material into an ellipsoid, thus obtaining a composite lithium metal anode. In step (2), the pressure control is achieved by controlling the compaction density through cold pressing and then controlling the morphology of the lithium-carbon material through hot pressing; or, the morphology of the lithium-carbon material is controlled by hot pressing first, and then the compaction density is controlled by cold pressing.

6. The method according to claim 5, characterized in that, The structural carbon material mentioned in step (1) is any one or a combination of at least two of carbon nanotubes, carbon fibers, or graphene; The lithium metal powder mentioned in step (1) includes pure lithium metal powder and / or lithium metal powder containing a protective layer; The shape of the lithium metal powder mentioned in step (1) includes spherical and / or near-spherical shapes; The average particle size of the lithium metal powder mentioned in step (1) is 1-80 μm; The ratio of the average particle size of the lithium metal powder to the length of the structural carbon material in step (1) is (1-10):1; The mass ratio of the structural carbon material to the lithium metal powder in step (1) is 1:(200-1300). The organic solvent mentioned in step (1) includes any one or a combination of at least two of the following: n-hexane, cyclohexane, N-methylpyrrolidone, benzene, p-xylene, carbon tetrachloride, tetrahydrofuran, liquid paraffin, or 1,2-dichloroethane.

7. The method according to claim 5 or 6, characterized in that, The high-speed dispersion rate in step (1) is 5000-20000 rpm and the time is 1-10 min.

8. The method according to claim 5 or 6, characterized in that, In step (1), a stabilizer is also added during the mixing process. The stabilizer includes any one or a combination of at least two of styrene-butadiene rubber, polyvinyl alcohol, polystyrene, polyvinylidene fluoride, polyvinylpyrrolidone, or cyclodextrin.

9. The method according to claim 8, characterized in that, The mass ratio of the stabilizer to the structural carbon material is 1:(5-60).

10. The method according to claim 5, characterized in that, The pressure mentioned in step (2) is 10-100 MPa.

11. The method according to claim 5, characterized in that, The thickness of the cold-pressed active material layer is 1.3-1.9 times the thickness of the negative electrode active material layer; The hot pressing temperature is 60-180℃.

12. The method according to claim 5, characterized in that, The current collector mentioned in step (2) includes any one or a combination of at least two of the following: three-dimensional carbon current collector, copper foil, copper foam, nickel foil, or nickel foam.

13. The method according to claim 5, characterized in that, The method includes the following steps: (1) The structural carbon material and organic solvent are first dispersed at high speed, and then the dispersion is dispersed at high speed with stabilizer and lithium metal powder to obtain lithium carbon material containing one or more lithium metal cores in the cocoon. The structural carbon material includes any one or a combination of at least two of carbon nanotubes, carbon fibers, or graphene. The organic solvent includes any one or a combination of at least two of the following: n-hexane, cyclohexane, N-methylpyrrolidone, benzene, p-xylene, carbon tetrachloride, tetrahydrofuran, liquid paraffin, or 1,2-dichloroethane. The stabilizer includes any one or a combination of at least two of styrene-butadiene rubber, polyvinyl alcohol, polyvinylidene fluoride, polyvinylpyrrolidone, or cyclodextrin. The lithium metal powder includes pure lithium metal powder and / or lithium metal powder containing a protective layer, with an average particle size of 10-80 μm. The mass ratio of the structural carbon material to the lithium metal powder is 1:(400-1100), and the mass ratio of the stabilizer to the structural carbon material is 1:(10-40). The rates of the first and second high-speed dispersions are independently 8000-10000 rpm; (2) The lithium-carbon material in step (1) is placed on the current collector and formed into an ellipsoid by adjusting the pressure of 25-80 MPa. The current collector includes any one or at least two of three-dimensional carbon current collector, copper foam or nickel foam, to obtain a composite lithium metal anode.

14. A lithium battery, characterized in that, The lithium battery includes a negative electrode as described in any one of claims 1-4.

Citation Information

Patent Citations

  • Lithium-carbon composite material, preparation method thereof, electrode plate and lithium metal battery

    CN108365202A

  • Composite active material for lithium secondary battery and method for producing same

    CN105164836A

  • Metal lithium@carbon composite material, lithium metal anode, and preparation and application of metal lithium@carbon composite material

    CN110875471A

  • Lithium-carbon composite material and preparation method thereof

    CN112133901A