Material for protecting metal negative electrode and application thereof

By forming an MXene-PEG solution protective layer on the surface of the metal anode, the problems of high reactivity and dendrite growth of the metal anode are solved, achieving efficient ion transport and electrochemical stability. This method is suitable for various metal batteries and improves the cycle life and performance of the battery.

CN117438584BActive Publication Date: 2026-11-24UNIV OF SCI & TECH BEIJING
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311451888.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-03
Publication Date
2026-11-24
Estimated Expiration
2043-11-03

AI Technical Summary

Technical Problem

Existing metal anodes in batteries suffer from high reactivity, easy formation of surface passivation films leading to increased electrode impedance, dendrite growth, and short-circuit risks. Existing protective layers also suffer from low ion transport efficiency, high and unstable overpotentials, and complex fabrication processes.

Method used

MXene-PEG solution is used as the protective layer material. A solid electrolyte interface is formed on the surface of the metal anode by soaking or dripping. The fast ion conductor of MXene and the flexible properties of PEG are utilized to form a stable SEI protective layer.

Benefits of technology

It improves the electrochemical stability and ion transport efficiency of metal anodes, inhibits dendrite growth, extends cycle life, and reduces overpotential. It is suitable for various metal batteries, and the preparation process is simple and low-cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117438584B_ABST
    Figure CN117438584B_ABST
Patent Text Reader

Abstract

The application provides a material for protecting a metal negative electrode and an application, and belongs to the technical field of new energy sources. The material is a MXene-PEG solution, which is composed of 1-99% of PEG, 1-50% of MXene powder and the rest of a solvent, the molecular weight of the PEG is 200-4000, the MXene includes any one of Ti3C2T x , Ti2CT x , V2CT x , Nb2CT x , Mo2CT x , Ti3CNT x , Ta4C3T x , Nb4C3T x , V4C3T x , TiVCT x , TiNbCT x or Ti3AlC2, and the solvent includes at least one of DMSO, TEGDME, NMP, DME, DMF, DCM or THF. The material for protecting a metal negative electrode provided by the application has good electrochemical and chemical stability, is not easy to break, has high ion transmission efficiency, good flexibility and high mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of new energy technology, and in particular to a material for protecting metal anodes and its application. Background Technology

[0002] Environmental pollution and energy shortages severely hinder the progress of human society. Batteries, as an emerging energy storage method, have become a research hotspot. In battery systems, metal anodes have higher specific energy compared to anodes made of other materials, attracting considerable attention. However, using metals as battery anodes still presents several problems. One is the high reactivity of metals, which may generate an ever-thickening surface passivation film in the electrolyte, leading to continuously increasing electrode impedance and deposition overpotential. On the other hand, when metal is deposited on the anode surface, uneven current density can easily lead to dendrite growth. When dendrites pierce the separator, they can easily cause serious and dangerous consequences such as short circuits, thermal runaway, and explosions.

[0003] To improve the surface stability of metal anodes, reduce dendrite growth, enhance electrode capacity and cycle life, and lower overpotential, common strategies include constructing artificial surface protective films, modifying electrolytes, building carriers, and optimizing separators. Among these, constructing a protective layer (i.e., a solid electrolyte interface, SEI) on the surface of the metal anode can isolate the metal from direct contact with the electrolyte, preventing side reactions and thus improving battery cycle life and capacity. However, artificial surface protective layers still suffer from problems such as low ion transport efficiency, high and unstable overpotentials, easy detachment, and complex fabrication.

[0004] For example, CN111509195A discloses a method for surface modification of lithium metal anodes in all-solid-state lithium batteries. Under an inert atmosphere, a polyethylene dioxythiophene-polyethylene glycol copolymer solution is coated onto the surface of a lithium metal substrate, and after drying, a uniform and dense PEDOT-PEG modified layer is formed. This method, when applied to all-solid-state lithium metal anodes, can effectively improve the capacity decay problem during battery charge-discharge cycles, increasing the capacity retention from 82.2% to 97% after 100 cycles at 1C rate. However, the battery itself has a very low capacity; when paired with a LiFePO4 cathode, the initial capacity at 60℃ and 1C rate is only 100mAh / g, which is far below the market average.

[0005] CN112111076A discloses an artificial interface protective film, a lithium battery negative electrode, and a method for preparing the same. The method employs a solution casting method to uniformly cast and coat a polyurethane / lithium fluoride-based artificial interface protective film (APM) onto the negative electrode LM (lithium metal substrate) of a lithium metal battery. This method utilizes the Li in lithium fluoride (LiF)... +The cations interact with the NH and C=O groups of polyurethane (PU), respectively, allowing lithium fluoride to dissolve well in the polyurethane and degrading its crystallinity. A composite film is then prepared via solution casting, resulting in excellent mechanical and ionic conductivity properties, and also providing physical isolation between the electrolyte and the lithium battery anode. However, this method only protects the lithium anode and has certain limitations; its effectiveness is limited at a current density of 1 mA·cm⁻¹. -2 The surface area capacity is 1 mAh·cm². -2 Under the specified conditions, the polarization voltage was 37.5 mV, and after 50 cycles, the polarization voltage was 17.3 mV; moreover, the best ionic conductivity of this technology was 8.9 × 10⁻⁶. -4 s·cm -1 At present, this level of ionic conductivity is not commercially viable.

[0006] CN114864858A discloses a zinc battery metal anode with an interface protective layer, its preparation method, and its application. The patent uses chitosan and the two-dimensional material MXene as the interface protective layer for the zinc metal anode. The principle is that, on the one hand, the amino and hydroxyl groups in chitosan have a strong complexing ability for zinc ions, ensuring rapid passage of zinc ions through the protective layer and providing numerous nucleation sites, promoting zinc nucleation and uniform zinc deposition. On the other hand, conductive MXene can promote a uniform electric field distribution on the surface of the zinc metal anode and disperse the electric field at the tips of accidentally grown zinc dendrites, thus protecting the zinc metal anode and suppressing dendrites. However, the chitosan in this technology can only complex zinc and lithium ions, limiting its application scope. The exploration and utilization of MXene's performance is still at a relatively shallow level. Furthermore, the experiments provided in this patent lack full-cell data, thus lacking practical application value.

[0007] Therefore, there is an urgent need to explore protective layers for metal anode surfaces with better physical, chemical, and electrochemical properties. Summary of the Invention

[0008] To address the aforementioned problems in existing technologies, this invention provides a material for protecting metal anodes and its application. The material for protecting metal anodes provided by this invention exhibits good electrochemical and chemical stability, is not easily broken, has high ion transport efficiency, good flexibility, and high mechanical strength.

[0009] The technical solution of the present invention is as follows:

[0010] A material for protecting a metal anode, said material being an MXene-PEG solution, comprising 1-99% PEG, 1-50% MXene powder, and the remainder being solvent.

[0011] Preferably, the molecular weight of the PEG is 200-4000.

[0012] Preferably, the MXene comprises Ti3C2T x Ti2CT x V2CT x Nb2CT x Mo2CT x Ti3CNT x Ta4C3T x Nb4C3T x V4C3T x TiVCT x TiNbCT x Or any of Ti3AlC2.

[0013] Preferably, the solvent includes at least one of DMSO, TEGDME, NMP, DME, DMF, DCM, or THF.

[0014] Furthermore, the MXene-PEG solution is prepared by dissolving PEG in a solvent, then adding MXene powder and stirring until homogeneous.

[0015] The present invention also provides the application of the above-mentioned material for protecting the metal anode, that is, using the MXene-PEG solution to protect the metal anode of the battery.

[0016] Furthermore, the specific method for protecting the metal anode of the battery includes soaking or dripping an MXene-PEG solution onto the surface of the metal anode sheet that has been treated with a surface oxide layer, and then drying it to obtain a protective layer.

[0017] Preferably, the specific methods for protecting the metal negative electrode of the battery include, but are not limited to, the following two:

[0018] Method 1: In a dry environment isolated from oxygen, immerse the metal anode sheet with the treated surface oxide layer in the prepared MXene-PEG solution, let it stand for 0.5-24 hours, remove it, wipe off the excess solution, and let it air dry.

[0019] Method 2: In a dry environment isolated from oxygen, drop MXene-PEG solution onto the surface of the metal anode sheet that has been treated with surface oxide layer, with a drop volume of 0.01ml-100ml. Wipe off any excess solution and let it air dry.

[0020] Preferably, the metal negative electrode is any one of magnesium, lithium, sodium, potassium, aluminum, and zinc.

[0021] Preferably, the metal anode is used as the anode of a metal-gas battery, including but not limited to Li-O2, Na-O2, K-O2, Al-O2, Zn-O2, Mg-O2, Ca-O2 and Li-CO2, Na-CO2, K-CO2, Al-CO2, Zn-CO2, Mg-CO2, Ca-CO2 batteries.

[0022] Preferably, the metal anode is used as the anode of a metal-ion battery, including but not limited to secondary lithium metal batteries, secondary magnesium metal batteries, secondary potassium metal batteries, secondary sodium metal batteries, secondary aluminum metal batteries, secondary calcium metal batteries, and secondary zinc metal batteries.

[0023] In the above text, the Chinese names of PEG, DMSO, TEGDME, NMP, DME, DMF, DCM and THF are respectively: polyethylene glycol, dimethyl sulfoxide, triethylene glycol dimethacrylate, N-methylpyrrolidone, dimethyl ether, dimethylformamide, dichloromethane, and tetrahydrofuran.

[0024] The beneficial technical effects of this invention are as follows:

[0025] 1. This invention allows for the preparation of an artificial solid intermediate phase layer containing MXene material on a metal surface simply by soaking or dripping. This layer can be widely used for negative electrode protection in various metal batteries. The preparation process is simple, low-cost, and can be mass-produced on the surface of metal negative electrodes. The metal negative electrode protection strategy using this invention can be applied not only to magnesium but also to lithium, sodium, potassium, aluminum, zinc, and other metals, solving problems such as high impedance, high overpotential, and poor cycle performance associated with the negative electrode side in metal batteries.

[0026] 2. The metal anode treated with the MXene-PEG solution of this invention can be used as a high-energy-density secondary metal battery anode material. The metal anode treated by this method exhibits a longer cycle life, lower overpotential, higher capacity retention, and stronger cycle reversibility. Compared to CN114864858A, this invention applies the protection strategy to full cells, demonstrating its value in practical applications.

[0027] MXene powder exhibits excellent electrical conductivity, hydrophilicity, and good dispersion stability. In this invention, on the one hand, MXene is a fast ion conductor material, which increases the transport efficiency and driving force of metal ions, enabling uniform deposition of the negative electrode while achieving good electrochemical performance; on the other hand, the addition of the organic component PEG allows the SEI to adapt to the large volume changes during the reversible metal deposition / stripping process without breaking, while simultaneously isolating the metal from direct contact with the electrolyte, thus preventing harmful side reactions.

[0028] Compared with CN112111076A, the method for protecting the negative electrode designed in this invention not only utilizes the fast ion conductor MXene, which has better ion conductivity, but also uses flexible PEG material to suppress dendrite growth. The combination of these two complementary advantages makes the negative electrode treated by this method exhibit better performance, enabling the magnesium metal symmetric battery to stably cycle 1000 times.

[0029] 3. This invention uses PEG solutions with different molecular weights, concentrations, and solvents to obtain metal anode sheets with different SEI protection properties. Furthermore, different soaking times can also yield metal anode sheets with different SEI protection thicknesses, or different drop amounts can yield metal anode sheets with different SEI protection thicknesses. Attached Figure Description

[0030] Figure 1 This is a SEM image of the Mg metal anode before the protective layer was coated in Example 1;

[0031] Figure 2 This is a SEM image of the Mg metal anode after the protective layer was coated in Example 1;

[0032] Figure 3 The electrical performance test results of the metal battery obtained in Example 1 are shown.

[0033] Figure 4 The electrical performance test results of the metal battery obtained in Comparative Example 1 are shown.

[0034] Figure 5 The electrical performance test results of the metal battery obtained in Comparative Example 2 are shown.

[0035] Figure 6 The electrical performance test results of the metal battery obtained in Example 17 are shown below.

[0036] Figure 7 The results are the electrical performance test results of the metal battery obtained in Example 18. Detailed Implementation

[0037] The present invention will now be described in detail with reference to the accompanying drawings and embodiments. Obviously, the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0038] Examples 1-9: Preparation of metal-ion batteries after protecting the metal negative electrode

[0039] Examples 1-9 provide methods for protecting different metal anodes and then using them in metal-ion batteries. The preparation methods are basically similar, with the difference being the metal anodes being protected and the raw materials and amounts of the protective materials, as shown in Table 1.

[0040] Table 1

[0041]

[0042]

[0043] Examples 1-9 illustrate methods for preparing metal-ion batteries after protecting different metal anodes:

[0044] (1) Cut the purchased 0.5mm magnesium foil into round pieces with a diameter of about 12mm, and polish them with sandpaper until the surface is smooth and without obvious scratches, and remove all the oxide layer on the surface of the magnesium foil.

[0045] PEG was dissolved in a solvent, and then MXene powder was added. The mixture was stirred on a magnetic stirrer for 12 hours to obtain a PEG@MXene solution. The solvent density was 1.100 g·ml. -1 about.

[0046] The pretreated magnesium sheet is immersed in the prepared PEG@MXene solution and left to stand for 12 hours. After removal, excess solution is wiped off and the sheet is allowed to air dry naturally to obtain the magnesium anode coated with the protective layer.

[0047] (2) Weigh V2O5 powder, conductive carbon black SuperP powder, and PVDF (binder) in a mass ratio of 8:1:1, then add an appropriate amount of NMP to achieve a suitable slurry concentration, and grind evenly in a mortar. Coat the treated solution onto a 12mm diameter nickel foam (0.3mm thick), and dry overnight under vacuum at 100℃ to remove residual NMP solvent. The positive electrode loading (V2O5) is approximately 0.2mg, with the nickel foam serving as the positive electrode current collector.

[0048] (3) Assemble the metal-ion battery in a glove box filled with argon atmosphere (water and oxygen content less than 0.1 ppm). Assemble the positive electrode, glass fiber separator and metal negative electrode prepared in step (2) into a CR2032 button cell. The electrolytes are 0.5 M magnesium bis(trifluoromethanesulfonyl)imide dissolved in a mixed solution of EMIMBF4 and triethylene glycol dimethyl ether (volume ratio 1:9), 1 M zinc sulfate aqueous solution, and 1.3 M aluminum chloride dissolved in 1 M [EMIm]Cl.

[0049] Assemble the battery according to the normal button cell assembly sequence, add 150 μL of electrolyte, and press the components together using a button cell sealing machine to complete the metal-ion battery assembly. Before testing the electrical performance, place the battery on a battery channel rack and let it stand for 8 hours.

[0050] Detection Example 1: Surface Morphology

[0051] The Mg metal anodes prepared in Example 1 before and after the protective coating were examined using SEM images. Figure 1 , Figure 2 As shown in the SEM image, a significant change has occurred on the surface of the magnesium anode: the originally smooth metal surface ( Figure 1 Many needle-like nanosheets grew. Figure 2 As can be seen, after MXene is dispersed into a monolayer sheet by DMSO solvent, it is adsorbed on the magnesium metal surface and together with the molecular weight 600 of PEG, forms a protective layer.

[0052] The morphology of the metal anodes coated with protective layers prepared in Examples 2-8 is similar to that of the others. As the PEG concentration increases, the porosity increases; among them, magnesium metal is the most dense and aluminum metal has the largest porosity.

[0053] Test Example 2: Electrical Performance

[0054] The button batteries prepared in Examples 1-9 were subjected to charge-discharge cycle performance tests at a current density of 1C and a cutoff specific capacity of 300 mAh / g. The test results are shown in Table 2, where the test results for Example 1 are shown in Table 2. Figure 3 As shown.

[0055] Table 2

[0056] Number of cycles Discharge specific capacity Example 1 40 75mAh / g Example 2 40 65mAh / g Example 3 40 57mAh / g Example 4 40 67mAh / g Example 5 40 63mAh / g Example 6 40 61mAh / g Example 7 40 78mAh / g Example 8 40 70mAh / g Example 9 40 64mAh / g

[0057] Comparative Example 1:

[0058] Based on Example 1, only 35% PEG-600 was dissolved in DMSO solution, and the solution was coated onto a Mg metal anode without adding MXene. The results are as follows. Figure 4 As shown in the figure, the capacity retention rate is lower than that of the battery with added MXene, but better than that of the battery without protection (Mg).

[0059] Comparative Example 2:

[0060] The battery was assembled using an unprotected magnesium metal negative electrode, and other experimental procedures were basically the same as in Example 1. Test results are as follows: Figure 5 As shown in the figure, the battery performance is very poor, even lower than that of a battery with protected magnesium.

[0061] Comparative Example 3:

[0062] Based on Example 1, the MXene material Ti3AlC2 was replaced with another type of material MgBr2. After 40 cycles, the discharge specific capacity was only 45mAh / g, which is lower than the performance of the magnesium battery protected by MXene.

[0063] Comparative Example 4:

[0064] Based on Example 1, the MXene material Ti3AlC2 was replaced with another type of material MgF2. After 40 cycles, the discharge specific capacity was only 43 mAh / g, which is lower than the performance of the magnesium battery protected by MXene.

[0065] Example 10:

[0066] Based on Example 1, the molecular weight of PEG was changed from 600 to 200. After 40 cycles, the discharge specific capacity remained at 55 mAh / g, higher than the performance of the unprotected and material-protected magnesium batteries in the comparative examples.

[0067] Example 11:

[0068] Based on Example 1, the 35% PEG-600 was replaced with 35% PEG-1200. The test results were better than those of the unprotected magnesium metal battery. After 40 cycles, the discharge specific capacity was still 56 mAh / g, which is higher than the performance of the unprotected and the material-protected magnesium battery in the comparative example.

[0069] Example 12:

[0070] Based on Example 1, the pretreated magnesium sheet was immersed in the prepared MXene-PEG solution and left to stand for 1 hour. The test results showed that after 40 cycles, the discharge specific capacity was still 65 mAh / g, which was higher than the performance of the unprotected and material-protected magnesium batteries in the comparative example.

[0071] Example 13:

[0072] Based on Example 1, MXene was replaced with Mo2CT instead of Ti3AlC2. x The results showed that after 40 cycles, the discharge specific capacity was still 61 mAh / g, which was higher than the performance of the unprotected and material-protected magnesium batteries in the comparative example.

[0073] Example 14:

[0074] Based on Example 1, MXene was replaced by Ta4C3T instead of Ti3AlC2. x The results showed that after 40 cycles, the discharge specific capacity was still 63 mAh / g, which was higher than the performance of the unprotected and material-protected magnesium batteries in the comparative example.

[0075] Example 15:

[0076] Based on Example 1, the solvent was replaced with DME instead of DMSO. The results showed that after 40 cycles, the discharge specific capacity was still 60 mAh / g, which was higher than the performance of the unprotected and material-protected magnesium batteries in the comparative example.

[0077] Example 16:

[0078] Based on Example 1, the solvent was replaced with TEGDME instead of DMSO. The results showed that after 40 cycles, the discharge specific capacity was still 59 mAh / g, which was higher than the performance of the unprotected and material-protected magnesium batteries in the comparative example.

[0079] Example 17:

[0080] Both the positive and negative electrodes of the battery are made of magnesium metal protected in Example 1, and a symmetrical battery is assembled. Other steps are basically the same as in Example 1. Test results are as follows: Figure 6 As shown, this represents a significant improvement over unprotected magnesium symmetric cells, achieving stable cycling for 600 cycles.

[0081] Example 18:

[0082] Both the positive and negative electrodes of the battery used magnesium metal protected in Example 1, and a Mg-Cu symmetrical battery was assembled. Other steps were basically the same as in Example 1. Test results are as follows: Figure 7 As shown, this is a significant improvement over unprotected magnesium symmetric cells, and it can stably cycle 1000 times.

[0083] Examples 19-27: Preparation of metal-gas batteries after protecting the metal negative electrode

[0084] Examples 19-27 provide methods for protecting different metal anodes and then using them in metal-gas batteries. The preparation methods are basically similar, with the difference being the metal anodes being protected and the raw materials and amounts of the protective materials, as shown in Table 3.

[0085] Table 3

[0086] Metal negative electrode PEG molecular weight PEG concentration MXene types MXene concentration Solvent types Example 19 Magnesium (Mg) 600 35% <![CDATA[Ti3AlC2]]> 5% THF Example 20 Magnesium (Mg) 600 50% <![CDATA[Ti3AlC2]]> 20% THF Example 21 Magnesium (Mg) 600 80% <![CDATA[Ti3AlC2]]> 50% THF Example 22 Aluminum (Al) 600 35% <![CDATA[Ti3AlC2]]> 5% THF Example 23 Aluminum (Al) 600 50% <![CDATA[Ti3AlC2]]> 20% THF Example 24 Aluminum (Al) 600 80% <![CDATA[Ti3AlC2]]> 50% THF Example 25 Zinc (Zn) 600 35% <![CDATA[Ti3AlC2]]> 5% THF Example 26 Zinc (Zn) 600 50% <![CDATA[Ti3AlC2]]> 20% THF Example 27 Zinc (Zn) 600 80% <![CDATA[Ti3AlC2]]> 50% THF

[0087] Examples 19-27 illustrate methods for preparing metal-gas batteries after protecting different metal anodes:

[0088] (1) Cut the purchased 0.5mm magnesium foil into round pieces with a diameter of about 12mm, and polish them with sandpaper until the surface is smooth and without obvious scratches, and remove all the oxide layer on the surface of the magnesium foil.

[0089] PEG was dissolved in a solvent, and then MXene powder was added. The mixture was stirred on a magnetic stirrer for 12 hours to obtain a PEG@MXene solution.

[0090] The prepared PEG@MXene solution was added dropwise onto the pretreated metal sheet and allowed to stand for 12 hours. The excess solution was then wiped off to obtain the magnesium metal anode coated with the protective layer.

[0091] (2) Prepare a mixed material by mixing 5 mg of commercial graphene material and 5 mg of conductive carbon black Super P.

[0092] Mix 10 mg of the above-mentioned mixed material with 50 mg of a 5 wt% polyvinylidene fluoride solution (the solvent of the polyvinylidene fluoride solution is N-methylpyrrolidone), continue to add N-methylpyrrolidone solvent until the catalyst slurry has a suitable consistency, and then grind it thoroughly in an agate mortar until uniform.

[0093] The material was evenly coated onto a pre-cut nickel foam substrate with a thickness of 0.3 mm and a diameter of 12 mm, and then vacuum dried at 100°C for 12 hours to obtain the cathode material.

[0094] The graphene and conductive carbon black Super P are loaded onto sheet-like nickel foam to form a porous conductive network structure with a pore size of 0.23 mm. The open area of ​​the overall electrode accounts for 98% of the total area. The graphene loading is approximately 0.2 mg / cm³. 2 .

[0095] (3) Assemble the batteries in a glove box filled with argon atmosphere, using CR2032 button cell batteries with a 2mm pore diameter and a pore density of 5-8 pores / cm². 2 The negative electrode is the metal negative electrode after treatment in step (1), and the positive electrode is the positive electrode material prepared in step (2). The electrolytes are 0.5M magnesium bis(trifluoromethanesulfonyl)imide dissolved in a mixed solution of EMIMBF4 and triethylene glycol dimethyl ether (volume ratio 1:9), 1M zinc sulfate aqueous solution, and 1.3M aluminum chloride dissolved in 1M [EMIm]Cl. The separator is a glass fiber separator.

[0096] The positive electrode material is placed on one side of the opening in the battery case, and the metal negative electrode processed in step (1) is placed on the other side of the battery case. The assembly can be completed in the normal assembly sequence of a button battery. The above components are pressed together by a button battery sealing machine to complete the battery assembly.

[0097] (4) Place the assembled battery in a 1000ml homemade sealed container, fill it with oxygen, and seal it. Add 40µL of deionized water to the sealed container. Perform a pre-charge and post-discharge test at a current density of 400mA / g and a cutoff specific capacity of 1000mAh / g. The magnesium-oxygen battery can cycle stably for 20 cycles with an overvoltage of only 0.9V.

[0098] Test Example 3: Electrical Performance

[0099] The button batteries prepared in Examples 19-27 were subjected to charge-discharge cycle performance tests at a current density of 200 mA / g and a cutoff specific capacity of 500 mAh / g. The test results are shown in Table 4.

[0100] Table 4

[0101] Number of cycles overvoltage Example 19 20 0.9V Example 20 20 1.0V Example 21 20 1.1V Example 22 20 0.4V Example 23 20 0.6V Example 24 20 0.9V Example 25 20 0.3V Example 26 20 0.4V Example 27 20 0.6V

[0102] Comparative Example 5:

[0103] Based on Example 19, if the protected magnesium metal is replaced with unprotected magnesium metal, the battery can only cycle stably for 4 cycles, and the performance is poor. This is mainly because the magnesium metal does not form a stable SEI.

[0104] Comparative Example 6:

[0105] Based on Example 19, the MXene material Ti3AlC2 was replaced with another type of material MgF2. The battery could cycle stably for 5 cycles with an overvoltage of 1.4V, which is 15 cycles less than the battery protected by Ti3AlC2.

[0106] Comparative Example 7:

[0107] Based on Example 19, the MXene material Ti3AlC2 was replaced with another type of material BiCl3. The battery could cycle stably for 6 cycles with an overvoltage of 1.3V, which is 14 cycles less than the battery protected by Ti3AlC2.

[0108] Example 28:

[0109] Based on Example 19, replacing PEG-600 with PEG-200, the battery can cycle stably for 15 cycles with an overvoltage of 1.0V, which is 11 cycles higher than the unprotected battery.

[0110] Example 29:

[0111] Based on Example 19, replacing PEG-600 with PEG-4000, the battery can cycle stably for 17 cycles with an overvoltage of 1.1V, which is 13 cycles higher than the unprotected battery.

[0112] Example 30:

[0113] Based on Example 19, MXene was replaced with TiNbCT instead of Ti3AlC2. x The battery can cycle stably for 18 cycles with an overvoltage of 1.0V, which is 14 cycles higher than the unprotected battery.

[0114] Example 31:

[0115] Based on Example 19, MXene was replaced by Nb4C3T instead of Ti3AlC2. x The battery can cycle stably for 15 cycles with an overvoltage of 0.75V, which is 11 cycles higher than the unprotected battery.

[0116] Example 32:

[0117] Based on Example 19, the solvent was replaced with DMF instead of THF, and the battery could cycle stably for 12 cycles with an overvoltage of 0.8V, which is 8 cycles higher than the unprotected battery.

[0118] Example 33:

[0119] Based on Example 19, the solvent was replaced with NMP instead of THF, and the battery could cycle stably for 15 cycles with an overvoltage of 0.9V, which is 11 cycles higher than the unprotected battery.

[0120] Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and embodiments. They can be applied to various fields suitable for the present invention. For those skilled in the art, and for those of ordinary skill in the art, various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention. Therefore, the present invention is not limited to the specific details without departing from the general concept defined by the claims and their equivalents.

Claims

1. An application of a material for protecting a metal negative electrode, characterized in that, The material is an MXene-PEG solution, composed of 35-50% PEG, 5-20% MXene powder, and the remaining amount of solvent; the MXene-PEG solution is used to protect the metal anode of the battery, wherein the metal anode is one of magnesium, aluminum, and zinc; The molecular weight of the PEG is 200-4000; The MXene includes Mo2CT x Ta4C3T x Nb4C3T x TiNbCT x Or one of Ti3AlC2; The solvent includes one of DMSO, TEGDME, NMP, DME, DMF, or THF; The specific method for protecting the metal anode of the battery includes soaking or dripping an MXene-PEG solution onto the surface of the metal anode sheet that has been treated with a surface oxide layer, and then drying it to obtain a protective layer.

2. The application according to claim 1, characterized in that, The MXene-PEG solution is prepared by dissolving PEG in a solvent, then adding MXene powder and stirring until homogeneous.

3. The application according to claim 1, characterized in that, The metal anode is used as the anode of a metal-gas battery, which includes, but is not limited to, Al-O2, Zn-O2, Mg-O2 and Al-CO2, Zn-CO2, Mg-CO2 batteries.

4. The application according to claim 1, characterized in that, The metal negative electrode is used as the negative electrode of a metal-ion battery, which includes, but is not limited to, a secondary magnesium metal battery, a secondary aluminum metal battery, and a secondary zinc metal battery.

Citation Information

Patent Citations

  • Surface modification method of metal lithium negative electrode in all-solid-state lithium battery

    CN111509195A

  • Artificial interface protective film, lithium battery negative electrode and preparation method of lithium battery negative electrode

    CN112111076A

  • Zinc battery metal negative electrode with interface protection layer and preparation method and application of zinc battery metal negative electrode

    CN114864858A

  • Ultrathin gel polymer interface modified zinc negative electrode material and preparation method thereof

    CN115763727A

  • Zinc metal negative electrode material based on ion / electron double-conductor interfacial film modification and preparation and application thereof

    CN116154147A