Silicone emulsion for additives

By optimizing the combination of hydroxyl-terminated polysiloxane, silicone rubber compound, polyether-modified silicone emulsifier, and nonionic emulsifier, the dilution and storage stability issues of silicone emulsion were solved, and the gloss and abrasion resistance of the coating film were improved.

CN117440990BActive Publication Date: 2026-11-24KCC SILICONE CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202280036388.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-17
Filing Date
2022-05-03
Publication Date
2026-11-24
Estimated Expiration
2042-05-03

AI Technical Summary

Technical Problem

Existing silicone emulsions have shortcomings in terms of dilution and storage stability, and the resulting coatings have poor gloss and abrasion resistance.

Method used

A composition comprising hydroxyl-terminated polysiloxane, silicone rubber compound, polyether-modified organosilicon emulsifier, nonionic emulsifier and water is used to improve the dispersibility and stability of the emulsion by optimizing the weight-average molecular weight, degree of polymerization and content of each component.

Benefits of technology

Excellent dilution and storage stability of silicone emulsions in organic solvents and water were achieved, and the gloss and abrasion resistance of the prepared coatings were significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004557928610000021
    Figure BDA0004557928610000021
  • Figure BDA0004557928610000041
    Figure BDA0004557928610000041
Patent Text Reader

Abstract

This invention relates to an organosilicon emulsion for additives, comprising a polysiloxane, a polyether-modified organosilicon emulsifier, a nonionic emulsifier, and water. The polysiloxane comprises a hydroxyl-terminated polysiloxane and a silicone rubber compound. The weight-average molecular weight of the hydroxyl-terminated polysiloxane is 30,000 to 110,000 g / mol, and the weight-average molecular weight of the silicone rubber compound is 400,000 to 1,000,000 g / mol.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an organosilicon emulsion for additives that exhibits excellent dilution and storage stability, as well as superior gloss and abrasion resistance in the resulting coating. Background Technology

[0002] Silicone emulsions are emulsions in which silicone polymers are dispersed in organic solvents or water. They are typically prepared as oil / water (O / W) emulsions by adding high-viscosity silicone polymers, emulsifiers, preservatives, and water. These silicone emulsions are added as additives to leather coatings or paints to impart gloss and abrasion resistance. In particular, to meet requirements for slip resistance or abrasion resistance, these silicone emulsions often contain highly polymerized polydimethylsiloxanes.

[0003] To disperse this highly polymerized polydimethylsiloxane in organic solvents or water, it is necessary to emulsify the polydimethylsiloxane using emulsifiers. Various emulsifiers, such as organosilicon-based or organic compound-based emulsifiers, are used as emulsifiers. Specifically, Japanese Patent No. 4822305 (Patent Document 1) discloses an organosilicon emulsion composition containing (A) organosilicon, (B) a nonionic surfactant, and (C) water. However, the organosilicon emulsion composition in Patent Document 1 has limitations due to the high viscosity of polydimethylsiloxane, resulting in poor emulsification and instability.

[0004] Therefore, there is a need to research and develop silicone emulsions for additives that exhibit excellent dilution and storage stability, and produce coatings with excellent gloss and abrasion resistance. Summary of the Invention

[0005] (The problem the invention aims to solve)

[0006] Therefore, the present invention aims to provide an additive silicone emulsion with excellent dilution stability and storage stability, and excellent gloss and abrasion resistance of the resulting coating.

[0007] (The measures taken to solve the problem)

[0008] The present invention provides an organosilicon emulsion for additives, the organosilicon emulsion comprising polysiloxane, polyether-modified organosilicon emulsifier, nonionic emulsifier and water.

[0009] The polysiloxane comprises hydroxyl-terminated polysiloxane and silicone gum.

[0010] The weight-average molecular weight of the hydroxyl-terminated polysiloxane is 30,000 to 110,000 g / mol.

[0011] The weight-average molecular weight of the silicone rubber compound is 400,000 to 1,000,000 g / mol.

[0012] (The effect of the invention)

[0013] The silicone emulsion used as an additive according to the present invention exhibits excellent dilution stability and storage stability against organic solvents and water. Furthermore, coatings prepared using paint or leather coating compositions containing the silicone emulsion exhibit excellent appearance properties, particularly excellent gloss and abrasion resistance. Therefore, the silicone emulsion is usefully applicable as an additive in paint or leather coatings. Detailed Implementation

[0014] The present invention will be described in detail below.

[0015] The “weight-average molecular weight” used in this specification is determined by conventional methods known in the art, such as gel permeation chromatography (GPC).

[0016] Furthermore, the content of functional groups, such as "hydroxyl content," can be determined using methods known in the art, such as calculations by structural analysis including H-NMR and C-NMR.

[0017] The silicone emulsion for additives according to the present invention comprises polysiloxane, polyether-modified silicone emulsifier, nonionic emulsifier and water.

[0018] Polysiloxane

[0019] Polysiloxanes include hydroxyl-terminated polysiloxanes and silicone gum.

[0020] The silicone emulsion of the present invention uses both hydroxyl-terminated polysiloxane and silicone rubber compound. However, when silicone rubber compound with a high degree of polymerization is used alone, it has the disadvantages of difficult dispersion and long dispersion time. But when it is used in combination with hydroxyl-terminated polysiloxane with a lower viscosity, the silicone rubber compound is easy to disperse and the dispersion time is shortened.

[0021] Hydroxyl-terminated polysiloxane

[0022] Hydroxyl-terminated polysiloxanes can improve the dispersibility of silicone rubber compounds and enhance the abrasion resistance of the resulting coatings.

[0023] The hydroxy-terminated polysiloxane can be represented by the following chemical formula 1.

[0024] [Chemical Formula 1]

[0025]

[0026] In the chemical formula 1, R 1 and R 2 C is independently substituted or unsubstituted. 1-10 Alkyl group. In this case, the alkyl group can be a straight-chain or branched alkyl group.

[0027] Specifically, R 1 and R 2 C can be substituted or unsubstituted, respectively. 1-5 Alkyl, or C 1-3 Alkyl group, wherein the alkyl group may be a straight-chain alkyl group.

[0028] At this point, m is a value that satisfies the weight-average molecular weight described later.

[0029] For example, the hydroxyl-terminated polysiloxane may be a hydroxyl-terminated polydimethylsiloxane, i.e., R 1 and R 2 It can be methyl.

[0030] The weight-average molecular weight of the hydroxyl-terminated polysiloxane can be 30,000 to 110,000 g / mol, 40,000 to 100,000 g / mol, or 60,000 to 100,000 g / mol. When the weight-average molecular weight of the hydroxyl-terminated polysiloxane is lower than the range described above, the viscosity of the polysiloxane is low, resulting in insufficient abrasion resistance and dilution stability after coating on a substrate; when it exceeds the range described above, a long dispersion time may occur.

[0031] Furthermore, the degree of polymerization of the hydroxyl-terminated polysiloxane can be 500 to 2000, 600 to 1500, or 1100 to 1400. When the degree of polymerization of the hydroxyl-terminated polysiloxane is lower than the specified range, the viscosity of the polysiloxane is low, resulting in insufficient abrasion resistance and dilution stability after coating on the substrate; when it exceeds the specified range, a longer dispersion time may occur.

[0032] Relative to the total weight of the hydroxyl-terminated polysiloxane, the hydroxyl content in the hydroxyl-terminated polysiloxane is 0.001 to 0.1% by weight or 0.002 to 0.08% by weight. When the hydroxyl content of the hydroxyl-terminated polysiloxane is lower than the range, there is a problem of poor coating effect on the substrate; when it exceeds the range, it may contain excessive low molecular weight hydroxyl-terminated polysiloxane, resulting in low viscosity of the silicone emulsion, which may lead to insufficient wear resistance and dilution stability after coating on the substrate.

[0033] Furthermore, the viscosity of the hydroxyl-terminated polysiloxane at 25°C can be 4000 to 100000 cP, 4500 to 90000 cP, or 70000 to 90000 cP. When the viscosity of the hydroxyl-terminated polysiloxane at 25°C is lower than the specified range, insufficient abrasion resistance and dilution stability may occur after coating on the substrate; when it exceeds the specified range, a longer dispersion time may occur.

[0034] Based on 100 parts by weight of the silicone emulsion, the hydroxyl-terminated polysiloxane can be included in the silicone emulsion at a content of 1 to 10 parts by weight, preferably 2 to 8 parts by weight. When the content of the hydroxyl-terminated polysiloxane is lower than the specified range, there are problems such as long dispersion time and insufficient storage stability; when it exceeds the specified range, the prepared silicone emulsion may have low viscosity, resulting in insufficient abrasion resistance and dilution stability after coating on the substrate.

[0035] <Silicone Rubber Compound>

[0036] Silicone gum can improve the low-temperature flexibility, high-temperature stability, weather resistance and wear resistance of silicone emulsions.

[0037] The silicone rubber compound can be represented by the following chemical formula 2.

[0038] [Chemical Formula 2]

[0039]

[0040] In the chemical formula 2, R 3 and R 4 C is independently substituted or unsubstituted. 1-10 Alkyl group. In this case, the alkyl group can be a straight-chain or branched alkyl group.

[0041] Specifically, R 3 and R 4 C can be independently substituted or unsubstituted. 1-5 Alkyl or C 1-3 Alkyl group, wherein the alkyl group may be a straight-chain alkyl group.

[0042] At this point, n is a value that satisfies the weight-average molecular weight described later.

[0043] For example, the silicone rubber compound can be hydroxyl-terminated polydimethylsiloxane, i.e., R 3 and R 4 It can be methyl.

[0044] The weight-average molecular weight of the silicone rubber compound can be 400,000 to 1,000,000 g / mol, 500,000 to 800,000 g / mol, or 600,000 to 800,000 g / mol. When the weight-average molecular weight of the silicone rubber compound is lower than the specified range, the viscosity of the polysiloxane is low, resulting in insufficient wear resistance after coating on the substrate. When the weight-average molecular weight exceeds the specified range, the dispersion and emulsification of the silicone rubber compound are also difficult, which may lead to poor storage stability and dilution stability of the prepared silicone emulsion.

[0045] Furthermore, the degree of polymerization of the silicone rubber compound can be 6000 to 13000, 7000 to 11000, or 8000 to 11000. When the degree of polymerization of the silicone rubber compound is lower than the specified range, the viscosity of the polysiloxane is low, resulting in insufficient abrasion resistance after coating on the substrate; when it exceeds the specified range, the dispersion and emulsification of the silicone rubber compound are also difficult, and the storage stability and dilution stability of the prepared organosilicon emulsion will decrease.

[0046] The viscosity of the silicone rubber compound at 25°C can be 20 million to 90 million cP, 30 million to 80 million cP, or 50 million to 80 million cP. When the viscosity of the silicone rubber compound at 25°C is lower than the specified range, due to the low viscosity of polysiloxane, insufficient wear resistance occurs after coating on the substrate; when it exceeds the specified range, the dispersion and emulsification of the silicone rubber compound are also difficult, and the storage stability and dilution stability of the prepared organosilicon emulsion will decrease.

[0047] Based on 100 parts by weight of the silicone emulsion, the silicone rubber compound can be included in the silicone emulsion at a content of 50 to 60 parts by weight or 52 to 58 parts by weight. If the content of the silicone rubber compound is lower than the range, the prepared coating film will have insufficient abrasion resistance; if it exceeds the range, the dispersion and emulsification of the silicone rubber compound will be difficult, and the storage stability and dilution stability of the silicone emulsion will also be problematic.

[0048] Polyether modified silicone emulsifier

[0049] Polyether-modified silicone-based emulsifiers can improve the emulsifying properties, storage stability, and dilution stability of polysiloxanes.

[0050] Water and oil are immiscible and opposing components, requiring emulsifiers to form a dispersed emulsion. Polyether-modified silicone emulsifiers, by simultaneously possessing polyvinyl and polypropylene groups, can mix well with water due to their hydrophilicity, and possess polysiloxane structures with substituted or unsubstituted alkyl groups as lipophilic groups, thereby achieving oil miscibility and stabilizing the emulsion. Specifically, in the oil / water (O / W) emulsion structure, the emulsifier forms a micelle morphology where the hydrophilic groups face outwards towards the water and the lipophilic groups face outwards towards the oil, thus stabilizing the emulsion.

[0051] The polyether-modified silicone emulsifier may be a polyethylene glycol (PEG)-polypropylene glycol (PPG)-terminated silicone emulsifier. Specifically, the polyether-modified silicone emulsifier can be represented by the following chemical formula 3.

[0052]

Chemical Formula 3

[0053]

[0054] In the chemical formula 3,

[0055] R 10 To R 13 C is independently substituted or unsubstituted. 1-10 alkyl.

[0056] a / b ranges from 1 to 5, and a+b ranges from 20 to 100.

[0057] y is an integer between 15 and 150.

[0058] Specifically, R 10 To R 13 C can be independently substituted or unsubstituted. 1-5 Alkyl, C 1-3 Alkyl, or methyl, ethyl, or n-propyl. In this case, the alkyl group can be a straight-chain or branched alkyl group.

[0059] Additionally, a / b can be 1 to 5 or 1.5 to 3; a+b can be 20 to 100 or 40 to 80. When a / b and a+b are below these ranges, the silicone emulsion is difficult to emulsify, and the dilution stability and wear resistance of the prepared coating are insufficient. If they exceed these ranges, problems may arise with the gloss of the prepared coating, insufficient storage stability of the silicone emulsion, and insufficient dilution stability.

[0060] Furthermore, the weight-average molecular weight of the polyether-modified silicone emulsifier can be from 4500 to 30000 g / mol or from 6500 to 25000 g / mol. When the weight-average molecular weight of the polyether-modified silicone emulsifier is lower than the specified range, the silicone emulsion suffers from difficulties in emulsification, dilution stability, and insufficient wear resistance of the prepared coating film; when it exceeds the specified range, the prepared silicone emulsion exhibits poor workability and insufficient dilution stability during use.

[0061] The viscosity of the polyether-modified silicone emulsifier at 25°C can be 50,000 to 200,000 cP or 95,000 to 150,000 cP. When the viscosity of the polyether-modified silicone emulsifier at 25°C is lower than the specified range, the silicone emulsion is difficult to emulsify, and the dilution stability and wear resistance of the prepared coating are insufficient; when it exceeds the specified range, the prepared silicone emulsion will have problems with poor workability and insufficient dilution stability during use.

[0062] Furthermore, the degree of polymerization (y in the chemical formula 3) of the polyether-modified silicone emulsifier can be an integer from 15 to 150 or from 30 to 120. When the degree of polymerization of the polyether-modified silicone emulsifier is lower than the specified range, the silicone emulsion suffers from problems such as difficulty in emulsification, dilution stability, and insufficient wear resistance of the prepared coating film; when it exceeds the specified range, the prepared silicone emulsion will exhibit problems such as poor workability and insufficient dilution stability during use.

[0063] The hydrophilic-lipophilic balance (HLB) of the polyether-modified silicone emulsifier can be 6 to 9 or 7 to 8. When the HLB of the polyether-modified silicone emulsifier is below the specified range, the emulsification stability of the silicone emulsion may be compromised; when it exceeds the specified range, the dilution stability of the silicone emulsion and the abrasion resistance of the prepared coating film may be compromised.

[0064] Furthermore, based on 100 parts by weight of the silicone emulsion, the polyether-modified silicone emulsifier can be included in the silicone emulsion at a content of 10 to 20 parts by weight or 11 to 17 parts by weight. When the content of the polyether-modified silicone emulsifier is lower than the specified range, problems such as poor dispersion of polysiloxane, making emulsification difficult, and insufficient storage and dilution stability of the silicone emulsion occur; when the content exceeds the specified range, problems such as insufficient dilution stability of the silicone emulsion and insufficient wear resistance of the prepared coating film occur.

[0065] Nonionic emulsifiers

[0066] Nonionic emulsifiers can improve the emulsification, storage stability and dilution stability of polysiloxanes, and also improve the abrasion resistance of the prepared coating film.

[0067] The nonionic emulsifier may comprise a first polyoxyethylene-modified alkyl ether and a second polyoxyethylene-modified alkyl ether with different modification rates. Using two polyoxyethylene-modified alkyl ethers with different modification rates as nonionic emulsifiers allows for adjustment to an appropriate HLB value, thereby improving the emulsification stability of the silicone emulsion and the abrasion resistance of the prepared coating. However, if only one polyoxyethylene-modified alkyl ether is used, adjusting the HLB value to the target value is not easy, and the storage stability, dilution stability, and abrasion resistance of the prepared silicone emulsion may be insufficient.

[0068] At this point, the first polyoxyethylene modified alkyl ether may contain 10 to 20 mol% or 12 to 17 mol% polyoxyethylene (EO) relative to the total molar number. Furthermore, the second polyoxyethylene modified alkyl ether may contain 25 to 40 mol% or 26 to 35 mol% polyoxyethylene (EO) relative to the total molar number.

[0069] The nonionic emulsifier can be represented by the following chemical formula 4.

[0070] [Chemical Formula 4]

[0071]

[0072] In chemical formula 4,

[0073] o+p is 5 to 15.

[0074] q is the polyoxyethylene modification rate.

[0075] Specifically, o+p can be 8 to 13 or 9 to 13.

[0076] For example, the nonionic emulsifier may contain a first polyoxyethylene modified alkyl ether and a second polyoxyethylene modified alkyl ether in a weight ratio of 1:0.5 to 3 or 1:0.5 to 2. When the weight ratio of the first polyoxyethylene modified alkyl ether to the second polyoxyethylene modified alkyl ether is lower than the specified range, i.e., when the content of the second polyoxyethylene modified alkyl ether is lower than the content of the first polyoxyethylene modified alkyl ether, the HLB of the silicone emulsion is low, resulting in problems with dilution stability and insufficient abrasion resistance of the resulting coating. When the ratio exceeds the specified range, i.e., when the content of the second polyoxyethylene modified alkyl ether is higher than the content of the first polyoxyethylene modified alkyl ether, the HLB of the silicone emulsion is high, and problems may occur with the storage stability after emulsification.

[0077] Furthermore, the nonionic emulsifier can be included in the silicone emulsion at a content of 1 to 12 parts by weight or 3 to 10 parts by weight, based on 100 parts by weight of the silicone emulsion. When the content of the nonionic emulsifier is lower than the range, the emulsification stability of the silicone emulsion is poor; if it exceeds the range, the dilution stability of the silicone emulsion and the abrasion resistance of the resulting coating may be insufficient.

[0078] water

[0079] The water is a dispersion medium for polysiloxane dispersion, which has the function of adjusting the viscosity of organosilicon emulsion and improving workability.

[0080] At this time, the water may be one or more selected from the group consisting of deionized water, pure water, ultrapure water and distilled water.

[0081] Furthermore, the water can be included in the composition at a content of 5 to 30 parts by weight or 10 to 25 parts by weight, based on 100 parts by weight of the silicone emulsion. If the water content is below the range, the viscosity of the silicone emulsion will be too high, causing problems with packaging and use; if it exceeds the range, the storage stability, dilution stability, and abrasion resistance of the silicone emulsion and the resulting coating may be insufficient.

[0082] additive

[0083] The silicone emulsion may further contain preservatives and pH adjusters, which are typically included in silicone emulsions.

[0084] The additive, based on 100 parts by weight of the silicone emulsion, may be included in the composition in amounts of 0.01 to 2 parts by weight or 0.01 to 0.5 parts by weight, respectively.

[0085] The preservative serves to prevent the silicone emulsion from being contaminated and deteriorating by microorganisms, thus preventing a decrease in stability. In this case, any preservative commonly used for silicone emulsions can be used without particular restriction, such as isothiazolone preservatives.

[0086] The pH adjuster serves to adjust the pH value of the silicone emulsion. Furthermore, the pH adjuster can be any pH adjuster commonly used for silicone emulsions without particular restriction; for example, it can be an aqueous solution of sodium hydroxide.

[0087] The viscosity of the silicone emulsion at 25°C can be between 250,000 and 900,000 cP or between 300,000 and 650,000 cP. When the viscosity of the silicone emulsion at 25°C is lower than the specified range, the silicone emulsion exhibits insufficient dilution stability and storage stability; when it exceeds the specified range, the viscosity of the silicone emulsion is too high, which may lead to problems with packaging and use.

[0088] Furthermore, the particle size of the silicone emulsion can be 2.0 to 9.0 μm or 3.0 to 8.5 μm. If the silicone emulsion particle size is smaller than the range described above, the resulting coating will have insufficient gloss and abrasion resistance; if it exceeds the range described above, the silicone emulsion will have insufficient dilution stability and storage stability.

[0089] As described above, the silicone emulsion according to the present invention exhibits excellent dilution stability and storage stability against organic solvents and water. Furthermore, coatings prepared using paint or leather coating compositions containing the silicone emulsion exhibit excellent appearance characteristics, particularly excellent gloss and abrasion resistance. Therefore, the silicone emulsion can be usefully used as an additive in paint or leather coatings.

[0090] (Method for carrying out the invention)

[0091] The present invention will now be described in more detail through the following embodiments. However, the descriptions in the following embodiments are only for illustrating specific implementations of the present invention, and are not intended to limit or restrict the scope of the present invention to the contents described in these embodiments.

[0092] Example 1: Preparation of Organosilicon Emulsion

[0093] 14 parts by weight of polyether-modified silicone emulsifier-1 (degree of polymerization (y): 75, chemical formula 3, a / b(EO / PO) = 50 / 20, R) 10 To R 13Four parts by weight of Nippon Shokubai Softanol 150 (15% mol of ethylene oxide (EO)) as the first polyoxyethylene modified alkyl ether and four parts by weight of Nippon Shokubai Softanol 300 (30 mol% mol of ethylene oxide (EO)) as the second polyoxyethylene modified alkyl ether were added to a reactor and mixed for 20 minutes. Then, 55 parts by weight of silicone rubber compound-1 (HG-H) and 5 parts by weight of hydroxyl-terminated polysiloxane-1 (HEP-80K) were added, and the mixture was stirred at 1000 rpm for 2 hours. Afterward, 5 parts by weight of water were added and stirred for 30 minutes, and the particle size of the emulsion was measured. After adding 12.85 parts by weight of water and stirring for 60 minutes, 0.1 parts by weight of a mixture of methylchloroisothiazolinone and methylisothiazolinone in a 3:1 weight ratio (KATHON CG) as a preservative was added and stirred for 30 minutes. Then, 0.05 parts by weight of a 20% by weight sodium hydroxide aqueous solution (pH adjuster) was added to prepare the silicone emulsion.

[0094] Examples 2 to 20 and Comparative Examples 1 to 5

[0095] Except for the compositions described in Tables 1 to 3, silicone emulsions were prepared using the same method as in Example 1.

[0096] Table 1

[0097]

[0098]

[0099]

[0100] Table 2

[0101]

[0102]

[0103] Table 3

[0104]

[0105]

[0106] The components and product names of the elements used in the following examples and comparative examples are listed in Table 4 below, where EO is polyethylene oxide and PO is polypropylene oxide.

[0107] Table 4

[0108]

[0109]

[0110]

[0111] Test examples and physical property evaluation

[0112] The physical properties of the silicone emulsions of the Examples and Comparative Examples were determined by the following methods, and the results are shown in Table 5.

[0113] (1) Whether or not emulsified

[0114] Whether the prepared silicone emulsion is emulsified or not can be confirmed by observing whether there is phase separation and whether it is evenly dispersed.

[0115] (2) Average particle size of dispersed particles

[0116] The average particle size (μm) of the dispersed particles in the silicone emulsion was measured using a Malvern Master Size 3000.

[0117] (3) Viscosity

[0118] The viscosity of the silicone emulsion at 25°C was determined using a Brookfield viscometer and a helipath stand #93 while stirring at 2.5 rpm.

[0119] (4) Storage stability (at room temperature)

[0120] The silicone emulsion was placed at 25℃±5℃ for 7 days. The appearance of the silicone emulsion was observed to determine whether the water layer and oil layer were separated, thereby evaluating its room temperature stability.

[0121] (5) Storage stability (high temperature)

[0122] The silicone emulsion was placed in a 50°C oven for 7 days. The appearance of the silicone emulsion was observed to determine whether the water layer and oil layer separated, thereby evaluating its high-temperature stability.

[0123] (6) Ethanol dilution stability

[0124] Add ethanol to dilute the silicone emulsion to a concentration of 20% by weight, and then visually confirm whether the oil has separated and / or the time point of layer separation under static conditions.

[0125] (7) Dilution stability of dimethylfluorene (DMF)

[0126] After adding dimethylfluorene (DMF) to dilute the silicone emulsion to a concentration of 10% by weight, visually confirm whether oil separation occurs and / or the time point of layer separation under static conditions.

[0127] (8) Stability under water dilution

[0128] After diluting the silicone emulsion with water to a concentration of 20% by weight, visually confirm whether water separation has occurred and / or the time point of stratification under static conditions.

[0129] (9) Abrasion resistance

[0130] A waterborne polyurethane solution was prepared by mixing and dispersing 30% by weight of waterborne polyurethane resin (manufacturer: KCC, solids content 30% by weight, viscosity (25°C): 70 cP), 2% by weight of curing agent (CX-100_Aziridine), 0.5% by weight of silicone emulsion from the examples or comparative examples, and 67.5% by weight of water. The waterborne polyurethane solution was then coated onto synthetic leather to a thickness of 10 μm and dried at 120°C for 10 minutes to prepare a test piece.

[0131] Afterwards, the test piece was subjected to 3000 abrasion tests with a load of 1kg using a Taber Abrasion Tester (CS10). The abrasion degree of the synthetic leather on the test piece was evaluated from 1 (high abrasion) to 5 (low abrasion).

[0132] (10) Gloss

[0133] An aqueous polyurethane solution was prepared using the same method as in Project (9), then coated onto synthetic leather and dried to prepare a test piece. The gloss of the test piece was then evaluated visually, with a relative rating of 1 (low gloss) to 5 (high gloss).

[0134] Table 5

[0135]

[0136]

[0137]

[0138] As shown in Table 5, the silicone emulsion of the example has suitable viscosity and average particle size of dispersed particles at 25°C, excellent storage stability at room temperature and high temperature, and excellent dilution stability to ethanol, DMF and water. The prepared coating film has excellent gloss and wear resistance.

[0139] Conversely, in Comparative Example 1, which does not contain silicone rubber, the dispersion viscosity is low, and the dilution stability to ethanol and the abrasion resistance of the prepared coating are poor.

[0140] Furthermore, in Comparative Example 2, which does not contain hydroxyl-terminated polysiloxane, the average particle size of the dispersed particles is large, with a value of more than 10 μm. It has high viscosity at 25°C, poor high-temperature storage stability, and poor dilution stability with ethanol and water.

[0141] Comparative Example 3, in which polyoxyethylene glycol trimethyl nonyl ether emulsifier was used instead of polyether-modified silicone emulsifier, and Comparative Example 5, in which anionic emulsifier was used, were both not emulsified.

[0142] Furthermore, Comparative Example 4, which uses a cationic emulsifier, exhibits poor storage stability at both room temperature and high temperature, and poor stability to dilution with ethanol and water.

Claims

1. An additive silicone emulsion, comprising polysiloxane, polyether-modified silicone emulsifier, nonionic emulsifier, and water. The polysiloxane comprises hydroxyl-terminated polysiloxane and silicone rubber compound. The hydroxyl-terminated polysiloxane has a weight-average molecular weight of 30,000 to 110,000 g / mol and a viscosity of 4,000 to 100,000 cP at 25°C. The weight-average molecular weight of the silicone rubber compound is 400,000 to 1,000,000 g / mol. in, Based on 100 parts by weight of silicone emulsion, it contains 50 to 60 parts by weight of silicone rubber compound, 1 to 10 parts by weight of hydroxyl-terminated polysiloxane, 10 to 20 parts by weight of polyether-modified silicone emulsifier, 1 to 12 parts by weight of nonionic emulsifier and 5 to 30 parts by weight of water.

2. The silicone emulsion for additives according to claim 1, wherein, The polyether-modified silicone emulsifier has a weight-average molecular weight of 4,500 to 30,000 g / mol, a viscosity of 50,000 to 200,000 cP at 25°C, and a degree of polymerization of 15 to 150.

3. The silicone emulsion for additives according to claim 1, wherein, The polyether-modified silicone emulsifier is represented by the following chemical formula 3. [Chemical Formula 3] ; In the chemical formula 3, R 10 To R 13 C is independently substituted or unsubstituted. 1-10 alkyl, a / b ranges from 1 to 5, and a+b ranges from 20 to 100. y is an integer between 15 and 150.

4. The silicone emulsion for additives according to claim 1, wherein, The nonionic emulsifier comprises a first polyoxyethylene-modified alkyl ether and a second polyoxyethylene-modified alkyl ether, each with different polyoxyethylene modifications.

5. The silicone emulsion for additives according to claim 4, wherein, The first polyoxyethylene modified alkyl ether and the second polyoxyethylene modified alkyl ether are contained in a weight ratio of 1:0.5 to 3.

6. The silicone emulsion for additives according to claim 1, wherein, The additive is a silicone emulsion used as an additive in paint or leather coatings.

Citation Information

Patent Citations

  • Method for preparing silicone emulsions

    KR100684668B1

  • KR20200090065A