A device and method for producing lactide from lactic acid

The continuous operation of lactic acid to lactide preparation was achieved by using a tower reactor loaded with H-beta molecular sieve packing, which solved the problems of catalyst dispersion and stirring, and realized the low-temperature and high-efficiency preparation of lactide, which is suitable for industrial production.

CN117443293BActive Publication Date: 2026-11-24CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311414932.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-27
Publication Date
2026-11-24
Estimated Expiration
2043-10-27

AI Technical Summary

Technical Problem

Existing processes for preparing lactide from lactic acid suffer from problems such as long reaction time, high vacuum requirements, difficulties in mass and heat transfer, high energy consumption, and inconvenient use of catalysts, resulting in high production costs and making them unsuitable for industrialization.

Method used

A tower reactor with H-beta molecular sieve packing material with a silicon-to-aluminum ratio of 35~360:1 and 5~34:1 was used to achieve continuous preparation of lactic acid. The catalyst dispersion and stirring problems were solved by hydrolysis to regenerate the catalyst, thus achieving heterogeneous catalysis.

Benefits of technology

This method enables the preparation of lactide at high yield and low cost at low temperatures, making it suitable for continuous industrial production and reducing energy consumption and equipment complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

This invention provides a production apparatus and method for preparing lactide from lactic acid, comprising a tower reactor 1; a lactic acid inlet is provided on the side of the tower reactor 1, a steam outlet is provided at the top, and a lactic acid oligomer outlet is provided at the bottom; the lactic acid inlet is connected to a lactic acid metering tank, and the tower reactor 1 is packed with H-beta molecular sieves loaded with a silica-to-alumina ratio of 35-360:1; a tower reactor 2 is connected to the lactic acid oligomer outlet; the tower reactor 2 is packed with H-beta molecular sieves loaded with a silica-to-alumina ratio of 5-34:1; the steam outlet at the top of the tower reactor 2 is connected to a U-shaped condenser 1; the U-shaped condenser 1 is connected to a lactide receiving tank 2; and the bottom of the tower reactor 2 is connected to a hydrolysis vessel. This apparatus enables continuous operation of heterogeneous catalytic lactic acid preparation of lactide, solving the problem of molecular sieve dispersion and stirring in the catalytic preparation of lactide from lactic acid; the reaction temperature is low, achieving high yield and low cost of lactide preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of bio-based material synthesis technology, and particularly relates to a production apparatus and method for preparing lactide from lactic acid. Background Technology

[0002] Developing biomass-based biodegradable plastics to replace traditional petroleum-based plastics has become a key research focus and hot topic in the field of polymer materials. Polylactic acid (PLA) is a bio-based biodegradable polyester material with high mechanical strength and good processing properties, suitable for extrusion, injection molding, thermoforming, and other processing methods. After disposal, it degrades into carbon dioxide and water in the natural environment, causing minimal environmental pollution. Currently, PLA has become the most industrially scaled bio-based biodegradable material, and it holds promise for alleviating pollution problems.

[0003] There are two main synthesis processes for polylactic acid (PLA): The first involves a one-step direct condensation polymerization of lactic acid to PLA. Patent (CN 1298764C) utilizes in-situ dehydration with molecular sieves to shorten the reaction cycle, while simultaneously employing polyols for chain extension. This process requires high vacuum and high temperatures, placing high demands on equipment; its industrial application is currently limited. The second process involves a two-step method: lactic acid is prepared by dehydration and oligomerization followed by pyrolysis to produce lactide monomers, and then by ring-opening polymerization of lactide. This process readily yields high molecular weight PLA or copolymers and is currently the primary method for industrial production. As a monomer, the synthesis method of lactide is the core and most challenging aspect of the process. Existing processes use homogeneous catalysts to catalyze the oligomerization and pyrolysis of lactic acid; however, this method suffers from long reaction times, high vacuum requirements, and high viscosity in the later stages of the reaction system, leading to difficulties in mass and heat transfer, resulting in high energy consumption and equipment costs.

[0004] Patent (CN 108610323 A) discloses a method for preparing lactide. Under vacuum conditions, H-beta molecular sieves catalyze the lactic acid reaction at 120-160℃, achieving a solvent-free direct synthesis of lactide from lactic acid. This overcomes the shortcomings of existing lactide synthesis methods, which require oligomerization and high-temperature pyrolysis, resulting in long processes and high reaction temperatures, thus achieving solvent-free production. However, the above method requires the molecular sieve catalyst and raw materials to be catalyzed in equal proportions, leading to a large amount of catalyst needed per reaction stage after scaling up production, resulting in a large-scale equipment. Furthermore, the method uses stirring to disperse the molecular sieve and raw materials, which easily causes wear and high energy consumption. The reaction process is also intermittent, which is not conducive to industrialization. Summary of the Invention

[0005] In view of this, the purpose of this invention is to provide a production apparatus and method for preparing lactide from lactic acid. This apparatus enables continuous preparation of lactide, solves the problems of catalyst catalysis and reuse, and has promising prospects for industrial application. This preparation method achieves a higher conversion rate of lactic acid than existing molecular sieve direct catalysis, realizing high-yield and low-cost lactide preparation.

[0006] This invention provides a production apparatus for preparing lactide from lactic acid, including a tower reactor 1; the tower reactor 1 has a lactic acid inlet on its side, a steam outlet at its top, and a lactic acid oligomer outlet at its bottom; the lactic acid inlet is connected to a lactic acid metering tank, and the tower reactor 1 is filled with packing material containing H-beta molecular sieves with a silica-to-alumina ratio of 35~360:1. A tower reactor 2 is connected to the lactic acid oligomer outlet of the tower reactor 1; the tower reactor 2 is filled with H-beta molecular sieves with a silicon-to-aluminum ratio of 5~34:1. The steam outlet at the top of the tower reactor 2 is connected to the U-shaped condenser 1; the U-shaped condenser 1 is connected to the lactide receiving tank 2; The bottom of the tower reactor 2 is connected to the hydrolysis vessel, which is connected to the lactic acid feeding device.

[0007] Preferably, it further includes a tower reactor 3 connected in parallel to the lactic acid oligomer outlet of the tower reactor 1; the tower reactor 3 is filled with packing material containing H-beta molecular sieves with a silicon-to-aluminum ratio of 5 to 34:1. The steam outlet at the top of the tower reactor 3 is connected to the U-shaped condenser 2; the U-shaped condenser 2 is connected to the lactide receiving tank 1; The bottom of the tower reactor 3 is connected to the hydrolysis vessel, which is connected to the lactic acid metering tank.

[0008] Preferably, the pipe condenser 1 is connected to the steam outlet, and the tube side outlet of the pipe condenser 1 is connected to the lactic acid receiving tank 3 via a pipe; A pipe condenser 2 is connected to the U-shaped condenser 1, and the tube side outlet of the pipe condenser 2 is connected to the lactic acid receiving tank 2 via a pipe.

[0009] Preferably, the pipe condenser 3 is connected to the U-shaped condenser 2, and the tube side outlet of the pipe condenser 3 is connected to the lactic acid receiving tank 1 via a pipe.

[0010] Preferably, the interiors of tower reactor 1, tower reactor 2 and tower reactor 3 are all equipped with heat-conducting oil pipes and baffles; The steam outlets of tower reactors 1, 2, and 3 are all equipped with splash guards.

[0011] Preferably, the shape of the packing material supported on H-beta molecular sieve is strip-shaped, sheet-shaped, or spherical particles.

[0012] This invention provides a method for preparing lactide using the production apparatus described above, comprising the following steps: 1) H-beta molecular sieves with a silicon-to-aluminum ratio of 35~360:1 were loaded into tower reactor 1 using a loading method; 2) Lactic acid is fed into tower reactor 1, where it undergoes molecular sieve catalytic esterification to obtain lactic acid oligomers; 3) The lactic acid oligomer is introduced into tower reactor 2 for further reaction. The generated steam is discharged through the top of the tower and collected to obtain crude lactide. The lactic acid oligomers accumulated at the bottom of the tower reactor 2 are introduced into the hydrolysis vessel for hydrolysis, and the material in the hydrolysis vessel is then introduced into the lactic acid metering tank.

[0013] Preferably, the reaction temperature for catalytic esterification in step 2) is below 110°C, and the vacuum degree is 10~4000Pa; In step 3), the reaction continues at a temperature of 110~240℃ and a vacuum of 10~4000Pa.

[0014] Preferably, after step 3) is repeated multiple times, low-concentration lactic acid is introduced into tower reactor 1 and then transported to tower reactor 2 to hydrolyze the lactic acid oligomers adsorbed on the molecular sieve to obtain lactic acid, which is then transported to the hydrolysis kettle.

[0015] This invention provides a production apparatus for preparing lactide from lactic acid, comprising a tower reactor 1; the tower reactor 1 has a lactic acid inlet on its side, a steam outlet at the top, and a lactic acid oligomer outlet at the bottom; the lactic acid inlet is connected to a lactic acid metering tank; the tower reactor 1 is packed with H-beta molecular sieves with a silica-to-alumina ratio of 35-360:1; a tower reactor 2 is connected to the lactic acid oligomer outlet of the tower reactor 1; the tower reactor 2 is packed with H-beta molecular sieves with a silica-to-alumina ratio of 5-34:1; the steam outlet at the top of the tower reactor 2 is connected to a U-shaped condenser 1; the U-shaped condenser 1 is connected to a lactide receiving tank 2; the bottom of the tower reactor 2 is connected to a hydrolysis vessel, and the hydrolysis vessel is connected to the lactic acid metering tank. This apparatus enables continuous operation of the heterogeneous catalytic lactic acid preparation process for lactide, solving the problem of molecular sieve dispersion and stirring in the lactic acid catalyst preparation of lactide. The apparatus used to prepare lactide has a low reaction temperature, enabling high yield and low cost in the preparation of lactide. Attached Figure Description

[0016] Figure 1 A schematic diagram of the production apparatus for preparing lactide from lactic acid provided by the present invention; Figure 2 This is a schematic diagram of the process flow for preparing lactide using the above-described production apparatus provided by the present invention. Detailed Implementation

[0017] This invention provides a production apparatus for preparing lactide from lactic acid, comprising a tower reactor 1; the tower reactor 1 has a lactic acid inlet on its side, a steam outlet at its top, and a lactic acid oligomer outlet at its bottom; the lactic acid inlet is connected to a lactic acid metering tank, and the tower reactor 1 is filled with packing material containing H-beta molecular sieves with a silica-to-alumina ratio of 35~360:1. A tower reactor 2 is connected to the lactic acid oligomer outlet of the tower reactor 1; the tower reactor 2 is filled with H-beta molecular sieves with a silicon-to-aluminum ratio of 5~34:1. The steam outlet at the top of the tower reactor 2 is connected to the U-shaped condenser 1; the U-shaped condenser 1 is connected to the lactide receiving tank 2; The bottom of the tower reactor 2 is connected to the hydrolysis vessel, which is connected to the lactic acid feeding device.

[0018] The device provided by this invention is simple and can be operated continuously. The catalyst used is loaded on the packing material, which solves the problems of catalyst dispersion and stirring. Through hydrolysis regeneration, the catalyst can be reused and the yield of lactide can be high.

[0019] See Figure 1 , Figure 1 A schematic diagram of the production apparatus for preparing lactide from lactic acid provided by the present invention; The production apparatus includes a lactic acid metering tank, a U-shaped condenser, a tube condenser, a tower reactor 1, a tower reactor 2, a tower reactor 3, a hydrolysis kettle, a metering pump, a centrifugal pump, a vacuum pump, a lactide storage tank, and a lactic acid receiving tank.

[0020] The production apparatus provided by this invention includes a tower reactor 1; the tower reactor 1 has a lactic acid inlet on its side, a steam outlet at the top, and a lactic acid oligomer outlet at the bottom; the lactic acid inlet is connected to a lactic acid metering tank, and the tower reactor 1 is filled with packing material containing H-beta molecular sieves with a silica-to-alumina ratio of 35~360:1; in a specific embodiment, the tower reactor 1 is filled with packing material containing H-beta molecular sieves with a silica-to-alumina ratio of 35~100. All H-beta molecular sieve packing materials are commercially available products.

[0021] The steam outlet at the top of the tower reactor 1 is connected to the tube side of the condenser 1 via a pipe, and the tube side outlet of the condenser 1 is connected to the lactic acid receiving tank 3 via a pipe. The lactic acid receiving tank 3 is connected to the vacuum pump.

[0022] In this invention, the lactic acid oligomer outlet of the tower reactor 1 is connected to the tower reactor 2. Specifically, the bottom of the tower reactor 1 is connected to the nozzle of the tower reactor 2 via a metering pump 3. The top of the tower reactor 2 is provided with a steam outlet, which is connected to the U-shaped condenser 1 via a pipe. The shell outlet of the U-shaped condenser 1 is connected to the pipe condenser 2 via a pipe. The overflow tank of the U-shaped condenser 1 is connected to the lactide receiving tank 2. The tube outlet of the pipe condenser 2 is connected to the lactic acid receiving tank 2 via a pipe. The lactide receiving tank 2 and the lactic acid receiving tank 2 are connected to a vacuum pump.

[0023] The bottom of the tower reactor 2 is connected to the hydrolysis vessel via centrifugal pump 1, and the hydrolysis vessel is connected to the lactic acid metering tank via centrifugal pump 3.

[0024] The production apparatus provided by the present invention further includes a tower reactor 3 connected in parallel to the lactic acid oligomer outlet of the tower reactor 1; the tower reactor 3 is filled with packing material containing H-beta molecular sieve with a silicon-to-aluminum ratio of 5~34:1. The steam outlet at the top of the tower reactor 3 is connected to the U-shaped condenser 2; the U-shaped condenser 2 is connected to the lactide receiving tank 1; the pipe condenser 3 is connected to the U-shaped condenser 2, and the tube side outlet of the pipe condenser 3 is connected to the lactic acid receiving tank 1 through a pipe.

[0025] The bottom of the tower reactor 3 is connected to the hydrolysis vessel via a centrifugal pump 2, and the hydrolysis vessel is connected to the lactic acid metering tank.

[0026] The lactic acid metering tank is connected to the lactic acid inlet of the tower reactor 1 via metering pump 1.

[0027] The U-shaped condensers 1 and 2 described in this invention are equipped with oil inlets and outlets, using oil as the medium for condensation. The pipe condensers 1, 2, and 3 described in this invention are each equipped with a cold water inlet and outlet, using water as the medium for condensation. The tower reactors 1, 2, and 3 described in this invention are each equipped with an oil inlet and outlet.

[0028] In this invention, the packing material supported on H-beta molecular sieve is in the shape of strips, flakes, or spherical particles.

[0029] This invention provides a method for preparing lactide using the production apparatus described above, comprising the following steps: 1) H-beta molecular sieves with a silicon-to-aluminum ratio of 35~360:1 are loaded into tower reactor 1; 2) Lactic acid is fed into tower reactor 1, where it undergoes molecular sieve catalytic esterification to obtain lactic acid oligomers; 3) The lactic acid oligomer is introduced into the tower reactor 2 for further reaction. The generated steam is discharged through the top of the tower and collected to obtain crude lactide. The tower reactor 2 is packed with H-beta molecular sieves with a silica-to-alumina ratio of 5~34:1. The lactic acid oligomers accumulated at the bottom of the tower reactor 2 are introduced into the hydrolysis vessel for hydrolysis, and the material in the hydrolysis vessel is then introduced into the lactic acid metering tank.

[0030] This invention involves loading a catalyst-supported packing material into a tower reactor. The reaction process is regulated by controlling the reaction temperature and the catalyst within the tower. Lactic acid enters the reaction tower, and the reflux temperature at the top of the tower is controlled to separate crude lactide and water. After the reaction is complete, the catalyst is regenerated and unreacted lactic acid polymers are recycled through a hydrolysis reaction. This invention achieves oligomer recycling and catalyst regeneration throughout the entire process, with low energy consumption, making it suitable for large-scale continuous production.

[0031] See Figure 2 , Figure 2 This is a schematic diagram of the process flow for preparing lactide using the above-described production apparatus provided by the present invention.

[0032] The lactic acid introduced into the lactic acid metering tank of this invention can be high-concentration lactic acid, low-concentration lactic acid, or a mixture of low-concentration and high-concentration lactic acid; the concentration of the low-concentration lactic acid is 50-80 wt%, and the concentration of the high-concentration lactic acid is 80-105 wt%. In a specific embodiment, 93% lactic acid is used.

[0033] The lactic acid oligomers obtained by catalytic esterification include one or more of lactic acid dimers, lactic acid trimers, and lactic acid tetramers.

[0034] In this invention, the reaction temperature for catalytic esterification in step 2) is below 110°C, preferably 60~110°C; specifically 80°C or 90°C; the vacuum degree is 10~4000Pa, specifically 500Pa or 1000Pa; and total reflux is used. In step 3), the reaction continues at a temperature of 110~240℃, preferably 130~180℃, specifically 140℃ or 160℃; the vacuum degree is 10~4000Pa; and total reflux is used.

[0035] In this invention, step 3) is preferably repeated multiple times. A low concentration of lactic acid is then introduced into tower reactor 1 (at this point, tower reactor 1 is shut off from heating and vacuum, essentially acting as a pipeline), and transported to tower reactor 2. The lactic acid oligomers adsorbed by the molecular sieve are then desorbed and hydrolyzed to obtain a mixture of lactic acid and lactic acid oligomers, which is then transported to a hydrolysis reactor. This method allows for catalyst regeneration in tower reactor 2, after which the esterification reaction continues.

[0036] A certain amount of water is preferably added to the hydrolysis vessel for hydrolysis; the temperature in the hydrolysis vessel is 50~120℃.

[0037] This invention transfers the lactic acid from the hydrolysis reactor into a lactic acid metering tank.

[0038] The parallel connection of tower reactor 2 and tower reactor 3 in this invention has the advantages of high efficiency in simultaneous production and continuous production under maintenance conditions of one standby and one operation.

[0039] This invention solves the problem of molecular sieve dispersion and stirring in the preparation of lactide by lactic acid catalysis; the method has a low reaction temperature, achieving high-efficiency and low-cost preparation of lactide.

[0040] To further illustrate the present invention, the following detailed description of the production apparatus and method for preparing lactide from lactic acid provided by the present invention is provided in conjunction with embodiments, but these descriptions should not be construed as limiting the scope of protection of the present invention.

[0041] The following examples use Figure 1 The apparatus shown.

[0042] Example 1

[0043] 1) The temperature inside the tower reactor 1 is controlled at 80°C and the vacuum degree is 500Pa. 93wt% lactic acid is introduced into the reactor through a sprayer. The lactic acid is esterified by fixed bed catalysis through molecular sieve (silicon-aluminum ratio 35~100:1). The generated water is removed by vacuum to obtain lactic acid oligomers (mainly composed of lactic acid dimers / trimers / tetramers, etc.). 2) The lactic acid oligomers in step 1) are introduced into another tower reactor 2. The temperature inside the reactor is controlled at 140°C and the vacuum degree is 1000Pa. The fixed-bed molecular sieve (silicon-aluminum ratio 5~34:1) catalyzes the cyclization of lactic acid to generate lactide. 3) After step 2) is completed, the lactic acid oligomers accumulated at the bottom of the tower reactor 2 in step 2) are introduced into the hydrolysis kettle, and a certain amount of water is added for hydrolysis; after the hydrolysis is completed, the lactic acid generated is repeated in step 1) to obtain lactic acid oligomers. 4) Perform the operation in step 2) on the lactic acid from step 3) to obtain lactide (content 98%), with a yield of 95% for lactide.

[0044] Example 2

[0045] 1) The temperature inside the tower reactor 1 is controlled at 90°C and the vacuum degree is 1000Pa. 93wt% lactic acid is introduced into the tower reactor 1 through a sprayer. The lactic acid is catalytically esterified by a fixed bed of molecular sieve (silicon-aluminum ratio 100:1). The generated water is removed by vacuum to obtain lactic acid oligomers (mainly composed of lactic acid dimers / trimers / tetramers, etc.). 2) In step 1), the lactic acid oligomers are introduced into another tower reactor 2. The temperature inside the reactor is controlled at 160°C and the vacuum degree is 1000Pa. The fixed-bed molecular sieve (silicon-aluminum ratio 5-34:1) catalyzes the cyclization of lactic acid to produce lactide.

[0046] 3) After step 2) is completed, the lactic acid oligomers accumulated at the bottom of the tower reactor 2 in step 2) are introduced into the hydrolysis kettle, and a certain amount of water is added for hydrolysis; after the hydrolysis is completed, the lactic acid generated is repeated in step 1) to obtain lactic acid oligomers. 4) Simultaneously, the lactic acid from step 3) is processed in step 2) to obtain lactide (content 98%), with a yield of 96%.

[0047] Comparative Example 1

[0048] 1) The temperature inside the tower reactor 1 is controlled at 80°C and the vacuum degree is 500Pa. 93wt% lactic acid is introduced into the reactor through a sprayer. The lactic acid is esterified by fixed bed catalysis through molecular sieve (silicon-aluminum ratio 35~100:1). The generated water is removed by vacuum to obtain lactic acid oligomers (mainly composed of lactic acid dimers / trimers / tetramers, etc.). 2) In step 1), the lactic acid oligomers are introduced into another tower reactor 2. The temperature inside the reactor is controlled at 140°C and the vacuum degree is 1000Pa. The fixed-bed molecular sieve (silicon-to-aluminum ratio 5~34:1) catalyzes the cyclization of lactic acid to produce lactide (content >98%). The yield of lactide is 85%.

[0049] As can be seen from the above examples, the process of the present invention reacts at a low temperature (80~160℃), resulting in mild reaction conditions; the reaction rate is fast, with a conversion rate of over 60% achieved in approximately 3 hours. The molecular sieve-catalyzed preparation of lactic acid from lactide features mild process conditions, a simple process, rapid reaction, low energy consumption throughout the production process, and low requirements for production equipment. The production equipment designed for the new process is suitable for industrial production, enabling the recycling and reuse of molecular sieves. The equipment is simple to operate and suitable for large-scale production.

[0050] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A production apparatus for preparing lactic acid from lactide, comprising a tower reactor 1; the tower reactor 1 is provided with a lactic acid inlet on its side, a steam outlet at its top, and a lactic acid oligomer outlet at its bottom; the lactic acid inlet is connected to a lactic acid metering tank, and the tower reactor 1 is filled with packing material containing H-beta molecular sieves with a silica-to-alumina ratio of 35~360:

1. A tower reactor 2 is connected to the lactic acid oligomer outlet of the tower reactor 1; the tower reactor 2 is filled with H-beta molecular sieves with a silicon-to-aluminum ratio of 5~34:

1. The steam outlet at the top of the tower reactor 2 is connected to the U-shaped condenser 1; the U-shaped condenser 1 is connected to the lactide receiving tank 2; The bottom of the tower reactor 2 is connected to the hydrolysis vessel, which is connected to the lactic acid metering tank.

2. The production apparatus according to claim 1, characterized in that, It also includes a tower reactor 3 connected in parallel to the lactic acid oligomer outlet of the tower reactor 1; the tower reactor 3 is filled with H-beta molecular sieves with a silicon-to-aluminum ratio of 5~34:

1. The steam outlet at the top of the tower reactor 3 is connected to the U-shaped condenser 2; the U-shaped condenser 2 is connected to the lactide receiving tank 1; The bottom of the tower reactor 3 is connected to the hydrolysis vessel, which is connected to the lactic acid metering tank.

3. The production apparatus according to claim 1, characterized in that, A pipe condenser 1 is connected to the steam outlet of the tower reactor 1, and the tube side outlet of the pipe condenser 1 is connected to the lactic acid receiving tank 3 via a pipe. A pipe condenser 2 is connected to the U-shaped condenser 1, and the tube side outlet of the pipe condenser 2 is connected to the lactic acid receiving tank 2 via a pipe.

4. The production apparatus according to claim 2, characterized in that, A pipe condenser 3 is connected to the U-shaped condenser 2, and the pipe outlet of the pipe condenser 3 is connected to the lactic acid receiving tank 1 via a pipe.

5. The production apparatus according to claim 1, characterized in that, The interiors of tower reactors 1, 2, and 3 are all equipped with heat-conducting oil pipes and baffles. The steam outlets of tower reactors 1, 2, and 3 are all equipped with splash guards.

6. The production apparatus according to claim 1, characterized in that, The packing material supported on H-beta molecular sieves can be in the form of strips, flakes, or spherical particles.

7. A method for preparing lactide using the production apparatus according to any one of claims 1 to 6, comprising the following steps: 1) H-beta molecular sieves with a silicon-to-aluminum ratio of 35~360:1 were loaded into tower reactor 1 using a loading method; 2) Lactic acid is fed into tower reactor 1, where it undergoes molecular sieve catalytic esterification to obtain lactic acid oligomers; 3) The lactic acid oligomer is introduced into the tower reactor 2 for further reaction. The generated steam is discharged through the top of the tower and collected to obtain crude lactide. The tower reactor 2 is packed with H-beta molecular sieves with a silica-to-alumina ratio of 5~34:

1. The lactic acid oligomers accumulated at the bottom of the tower reactor 2 are introduced into the hydrolysis vessel, and the material in the hydrolysis vessel is then introduced into the lactic acid metering tank.

8. The method according to claim 7, characterized in that, In step 2), the reaction temperature for catalytic esterification is below 110℃, and the vacuum degree is 10~4000Pa; In step 3), the reaction continues at a temperature of 110~240℃ and a vacuum of 10~4000Pa.

9. The method according to claim 7, characterized in that, After step 3) is repeated multiple times, low-concentration lactic acid is introduced into tower reactor 1 and then transported to tower reactor 2 to desorb and hydrolyze the lactic acid oligomers adsorbed on the molecular sieve, resulting in a mixture of lactic acid and lactic acid oligomers, which is then transported to the hydrolysis reactor.

Citation Information

Patent Citations

  • Preparation method of lactide

    CN108610323A

  • Method for preparing poly-lactic acid with high molecular weight by polycondensing lactic acid directly

    CN1298764C

  • Preparation method of lactide and reaction device

    CN112876452A

  • Method and device for continuously preparing lactide

    CN116041313A