Aerogel beads and preparation method thereof
By introducing thiol functional groups into the aerogel and using the gel-vacuum freeze-drying method to prepare PVA-SA/CS-SH aerogel beads, the existing aerogels have low mechanical strength and acid resistance when removing uranyl ions. Weak problem, achieving efficient and economical uranyl ion adsorption effect and good reusability.
Patent Information
- Application Number
- CN202311413466.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-10-30
Smart Images

Figure CN117443359B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chemistry, and in particular relates to an aerogel bead and a preparation method thereof. Background Art
[0002] In recent years, nuclear energy has been used all over the world as a safe, stable and efficient clean energy. In the large-scale use of nuclear energy, the mining of uranium mines and the discharge of nuclear fuels have caused a large amount of uranium-containing wastewater to enter nature. The uranium in nuclear wastewater generally exists in a hexavalent form, which can cause radiation in the human body and damage various organs of the human body, and even cause cancer. Uranium existing in nature can cause serious harm to the environment and humans due to its radioactivity and heavy metal toxicity. Therefore, it is very necessary to develop a safe and efficient method to remove uranium from wastewater.
[0003] At present, there are several main methods for removing uranium from aqueous solutions, such as photocatalysis, solvent extraction, membrane separation, bioremediation, electrochemistry and adsorption. Among these methods, adsorption has become a common and effective method because of its simple equipment, convenient operation, low cost and large adsorption capacity. Commonly used adsorbents include polymer adsorbents, bioadsorbents and porous materials. Among them, porous materials are widely used in the adsorption field because of their excellent pore structure and active sites that are conducive to adsorption. For example, layered double metal hydroxides, organic covalent materials and aerogels. Aerogel is a new type of three-dimensional macroscopic porous material with high surface area, high porosity, good expansion and fast mass transfer. It is suitable for removing pollutants and impurities in aqueous solutions, so it can be used as an effective and efficient adsorbent. Natural polymers represented by polysaccharides are widely used in the preparation of aerogels because of their long chains carrying rich functional groups and cross-linkable properties. Chitosan (CS) and sodium alginate (SA) are both natural polysaccharides with abundant active functional groups, biodegradability and good biocompatibility, and are widely used in the field of adsorption. However, pure chitosan aerogel and pure sodium alginate aerogel have low mechanical strength, weak acid resistance and poor stability, which greatly limits their application in the adsorption of heavy metal ions in wastewater.
[0004] Y.-R.He et al. published the paper "Aerogel based on melamine-formaldehyde and alginate: Simply removing of uranium from aqueous solutions" in Journal of Molecular Liquids in 2019, which announced the preparation of a melamine-formaldehyde / alginate (MF-A) aerogel, obtained a block structure of a porous network, and good mechanical stability, and was used to adsorb U (VI) from an aqueous solution. Therefore, chitosan can be used as a polycation component and sodium alginate as a polyanion component, and the two can be cross-linked to form gel beads, which not only obtains a large number of active groups, but also obtains a porous internal space structure. Other functional groups can also be modified and grafted on the surface of chitosan and sodium alginate to enrich active sites. Moreover, the cross-linked prepared gel beads are also easier to separate from the solution after the adsorption is completed, and can be recycled after adsorption-desorption. However, the preparation cost of the aerogel is high, and the adsorption performance of the aerogel for uranyl ions is not high enough.
[0005] Therefore, there is a need in the art for a new aerogel bead and a method for preparing the same. Summary of the invention
[0006] The invention uses chitosan and sodium alginate as raw materials, grafts (3-mercaptopropyl) trimethoxysilane to introduce mercapto functional groups, uses polyvinyl alcohol, and adopts a gel-vacuum freeze-drying method to prepare polyvinyl alcohol-sodium alginate / mercapto functionalized chitosan aerogel beads (PVA-SA / CS-SH).
[0007] The invention firstly provides an aerogel bead, wherein the aerogel bead is a polyvinyl alcohol-sodium alginate / thiol functionalized chitosan aerogel bead, namely a PVA-SA / CS-SH aerogel bead.
[0008] In a specific embodiment, the method comprises the following steps:
[0009] Step A: firstly prepare benzaldehyde-chitosan, i.e. BCS, using benzaldehyde and chitosan;
[0010] Step B: preparing benzaldehyde-thiol functionalized chitosan, namely BCS-SH;
[0011] Step C: Then preparing thiol-functionalized chitosan, i.e., CS-SH;
[0012] Step D: using polyvinyl alcohol and sodium alginate as well as the CS-SH prepared in step C, polyvinyl alcohol-sodium alginate / thiol functionalized chitosan aerogel beads, namely PVA-SA / CS-SH, were prepared.
[0013] In a specific embodiment, the deacetylation degree of the chitosan is above 90%, preferably above 95%; the alcoholysis degree of the polyvinyl alcohol is above 95 mol%, preferably 98-99 mol%.
[0014] In a specific embodiment, in step A, chitosan is dissolved in an acetic acid solution, and methanol is added. After the chitosan is completely dissolved, a mixture of benzaldehyde and methanol is added; the mixture is fully reacted at room temperature to obtain a light yellow gel; the gel is fully washed several times with methanol and anhydrous ethanol respectively to wash away unreacted benzaldehyde, and then dried to obtain amino-protected chitosan, namely BCS.
[0015] In a specific embodiment, in step A, the concentration of the acetic acid solution is 1-3%, the reaction time for fully reacting at room temperature to obtain a light yellow gel is more than 24 hours, the drying temperature of the gel is 60-70°C, and the drying time is more than 10 hours.
[0016] In a specific embodiment, in step B, the BCS prepared in step A is dispersed in toluene, (3-mercaptopropyl)trimethoxysilane is added to obtain a mixture, the mixture is ultrasonically dispersed, and then a hydrothermal reaction is performed; after the reaction is completed, the mixture is naturally cooled to room temperature, and the obtained solid reactant is washed several times with toluene and anhydrous ethanol, respectively, and BCS-SH is obtained after drying.
[0017] In a specific embodiment, in step B, the ultrasonic dispersion time of the mixture is more than 10 minutes, the hydrothermal reaction includes charging the mixture into a hydrothermal reactor with a polytetrafluoroethylene liner, reacting at 105-120°C for more than 12 hours, and the drying is carried out at 60-70°C, and the drying time is more than 6 hours.
[0018] In a specific embodiment, in step C, the BCS-SH prepared in step B is hydrolyzed with hydrochloric acid to remove the benzaldehyde used to protect the amino group and the chitosan that has not been successfully grafted with the thiol group, and then washed with anhydrous ethanol and deionized water for several times, and then dried to obtain CS-SH.
[0019] In a specific embodiment, in step C, the concentration of hydrochloric acid is 0.2-1 mol / L, the temperature of hydrolysis with hydrochloric acid is 50-70°C, the hydrolysis time is more than 6 hours, and the drying is carried out at 60-70°C, and the drying time is more than 6 hours.
[0020] In a specific embodiment, in step D, polyvinyl alcohol and sodium alginate are first dissolved in deionized water, heated and stirred to form a uniform mixed solution; then transferred to a low-temperature water bath, CS-SH prepared in step C is added and stirred, and after being completely dissolved, the mixed solution is naturally cooled to room temperature to obtain a mixed solution; the mixed solution is added dropwise to a calcium chloride solution, cross-linked to form gel beads; the gel beads are immersed in the calcium chloride solution, and then washed with deionized water for several times to remove uncross-linked calcium chloride; the gel beads are then frozen and vacuum freeze-dried to obtain the PVA-SA / CS-SH. H; preferably, a water bath is used for heating and stirring, and the water bath heating temperature is 85-95°C, and the time is more than 1 hour; the temperature of the low-temperature water bath is 75-82°C, the time of adding CS-SH and stirring is more than 3 hours, preferably a syringe is used to drop the mixed solution into the calcium chloride solution, the concentration of the calcium chloride solution is 2-5wt%, the gel beads are immersed in the calcium chloride solution for more than 5 hours, preferably the freezing temperature is -35°C to -25°C, the freezing time is more than 2 hours, and the vacuum freeze-drying temperature is -55°C to -45°C, and the time is more than 6 hours.
[0021] The PVA-SA / CS-SH aerogel beads provided by the present invention have a strong adsorption capacity and can remove up to 350.33 mg g of uranyl ions. -1 , showing excellent adsorption performance. The PVA-SA / CS-SH provided by the present invention has good reusability and adsorption selectivity, is low in cost, economical and affordable, and is expected to become a new and efficient uranium removal adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The macroscopic and microscopic structures of the PVA-SA / CS-SH gel beads prepared in Example 1 are shown. Figure 1 a is the gel beads before vacuum freeze drying. Figure 1 b is the gel beads after vacuum freeze drying. Figure 1 c is the SEM image of gel beads. Figure 1 d is the SEM image characterizing the internal structure of the gel beads.
[0023] Figure 2 The EDX analysis results of PVA-SA / CS-SH and PVA-SA / CS-SH+U are shown in Figure 1. Figure 2 a is the gel beads before uranium adsorption, Figure 2 b shows the gel beads after uranium adsorption.
[0024] Figure 3 This is the thermogravimetric curve (TGA) of PVA-SA / CS-SH gel beads.
[0025] Figure 4The isotherms and pore size distribution of PVA-SA / CS-SH gel beads are shown. Figure 4 a is the adsorption-desorption isotherm of gel beads, Figure 4 b is the pore size distribution of gel beads.
[0026] Figure 5 XRD spectra of CS, BCS, BCS-SH, CH-SH and PVA-SA / CS-SH.
[0027] Figure 6 FTIR spectra of CS, BCS, BCS-SH, CH-SH and PVA-SA / CS-SH.
[0028] Figure 7 The adsorption effect of gel beads on uranium under different pH conditions and its Zeta potential diagram. Figure 7 a is the adsorption effect of PVA-SA / CS-SH gel beads and sodium alginate / chitosan gel beads (SA / CS) on uranium under different pH conditions. Figure 7 b is the Zeta potential diagram of PVA-SA / CS-SH gel beads under different pH conditions.
[0029] Figure 8 Schematic diagram of the adsorption of U(VI) by PVA-SA / CS-SH at different contact times. Figure 8 a shows the effect of contact time on the change of the adsorption rate of U(VI) on PVA-SA / CS-SH. Figure 8 b is the linear fit of the intra-particle diffusion curve.
[0030] Fig. 9 Effect of coexisting ions on uranium adsorption experiments on PVA-SA / CS-SH aerogel beads.
[0031] Fig.10 Structural diagram of five cycles of adsorption-desorption experiments on PVA-SA / CS-SH.
[0032] Fig.11 The EDS mapping and EDS characterization images of PVA-SA / CS-SH aerogel beads after uranium adsorption. Fig.11 a is the EDS mapping diagram, Fig.11 b is the EDS characterization diagram.
[0033] Fig.12 It is the full spectrum of FTIR spectrum and XPS spectrum of PVA-SA / CS-SH before and after uranium adsorption. Fig.12 a is the FTIR spectrum, Fig.12 b is the XPS spectrum. DETAILED DESCRIPTION
[0034] Example 1
[0035] This example is about preparing PVA-SA / CS-SH aerogel beads.
[0036] Materials: Chitosan (deacetylation degree: 95%), acetic acid, hydrochloric acid and benzaldehyde were purchased from Sinopharm Chemical Reagent Beijing Co., Ltd. Polyvinyl alcohol (alcoholysis degree: 98.0-99.0 mol%, viscosity: 3.2-3.8 mPa.s), sodium alginate (90%), (3-mercaptopropyl) trimethoxysilane, methanol and anhydrous ethanol were purchased from Shanghai MacLean Biochemical Technology Co., Ltd. Toluene was purchased from Tianjin Tianli Technology Co., Ltd. Uranyl nitrate hexahydrate (UO 2 (NO 3 ) 2 6H 2 O) was purchased from Hubei Chushengwei Chemical Co., Ltd. All reagents were analytical grade. Deionized water was prepared in the laboratory. The preparation method of the PVA-SA / CS-SH aerogel beads comprises the following steps.
[0037] 1. Preparation of benzaldehyde-chitosan (BCS)
[0038] Dissolve 5.0g chitosan (CS) in 160mL 2% acetic acid solution, and add 100mL methanol. After the chitosan is completely dissolved, add a mixture of 40mL benzaldehyde and 100mL methanol. Fully react at room temperature for 24h to obtain a light yellow gel. Wash the gel several times with methanol and anhydrous ethanol to wash away the unreacted benzaldehyde, and then dry it at 65°C for 12h to obtain amino-protected chitosan - benzaldehyde-chitosan (BCS). This can prevent the amino groups in chitosan from being consumed in large quantities during the reaction of grafting thiol groups.
[0039] 2. Preparation of benzaldehyde-thiol functionalized chitosan (BCS-SH)
[0040] 1.5 g of benzaldehyde-chitosan (BCS) was dispersed in 30 mL of toluene, and 3 mL of (3-mercaptopropyl) trimethoxysilane was added. The mixture was ultrasonically dispersed for 15 min, and then placed in a polytetrafluoroethylene-lined hydrothermal reactor and reacted at 110 ° C for 24 h. After cooling naturally to room temperature, the reactants were washed several times with toluene and anhydrous ethanol, respectively, and dried at 65 ° C for 12 h to obtain benzaldehyde-thiol functionalized chitosan (BCS-SH).
[0041] 3. Preparation of thiol-functionalized chitosan (CS-SH)
[0042] 1.0g of thiolated benzaldehyde-chitosan (BCS-SH) was hydrolyzed with 50mL 0.5mol / L hydrochloric acid at 60℃. After 12h of hydrolysis, the benzaldehyde used to protect the amino groups and the chitosan that was not successfully grafted with thiol groups were removed. After washing with anhydrous ethanol and deionized water several times, it was dried at 65℃ for 12h to obtain thiol-functionalized chitosan (CS-SH).
[0043] 4. Preparation of polyvinyl alcohol-sodium alginate / thiol-functionalized chitosan aerogel beads (PVA-SA / CS-SH)
[0044] 1) Dissolve 2.0 g polyvinyl alcohol (PVA) and 0.5 g sodium alginate (SA) in 60 mL deionized water and heat in a water bath at 90°C for 2 h to form a uniform mixture. Then transfer to a water bath at 80°C, add 0.5 g thiol-functionalized chitosan (CS-SH), and stir magnetically for 6 h. After complete dissolution, cool naturally to room temperature.
[0045] 2) The mixed solution was added dropwise to 100 mL of 3w% calcium chloride solution by syringe to form gel beads by cross-linking. The gel beads were soaked in 3w% calcium chloride solution overnight, and then washed several times with deionized water to remove the uncross-linked calcium chloride. The gel beads were frozen at -30°C for 4 hours, and finally vacuum freeze-dried at -51°C for 12 hours to obtain polyvinyl alcohol-sodium alginate / thiol-functionalized chitosan aerogel beads (PVA-SA / CS-SH).
[0046] Example 2
[0047] This example is to characterize the PVA-SA / CS-SH aerogel beads prepared in the above Example 1.
[0048] 1. Characterization methods and equipment:
[0049] The morphology and microstructure of the aerogel beads were observed using a field emission scanning electron microscope (SEM, Apreo 2). X-Max EDS instrument (Oxford, UK) was used for elemental analysis of the aerogel beads. Fourier transform infrared spectra of the aerogel beads were obtained on a Nicolet-iS10 FTIR spectrometer (Thermo Fisher Scientific, USA) at 4000–400 cm -1The aerogel beads were measured on the surface. The aerogel beads were subjected to XRD analysis using a smartlab9 X-ray diffractometer (Kα radiation, copper target, Rigaku Corporation, Japan). The specific surface area of the aerogel beads was measured using Brunauer-Emmett-Teller (BET, Micro for TriStar IIPlus 3030). The surface potential of the aerogel beads was detected using ZS-90 (Malvern, UK). The aerogel beads were subjected to thermogravimetric analysis using a NETZSCH STA 449F3 instrument (Netzsch, Germany). The XPS spectrum of the aerogel beads was measured by a USA Thermo Fisher Scientific Escalab 250Xi spectrometer. The concentration of uranium in the solution was determined using a double-beam UV-visible spectrophotometer (Shanghai Youke Instrument Co., Ltd.).
[0050] Figure 1 The macroscopic and microscopic structures of the PVA-SA / CS-SH gel beads prepared in Example 1 are shown. Figure 1 a is the gel beads before vacuum freeze drying. Figure 1 b is the gel beads after vacuum freeze drying. Figure 1 c is the SEM image of gel beads. Figure 1 d is the SEM image characterizing the internal structure of the gel beads.
[0051] from Figure 1 As can be seen in the figure, PVA-SA / CS-SH is a white colloidal sphere with a uniform size and a diameter of about 2 mm ( Figure 1 a). After vacuum freeze drying, the appearance of PVA-SA / CS-SH was basically unaffected, the volume was slightly smaller, and the surface roughness increased ( Figure 1 b) SEM image of PVA-SA / CS-SH Figure 1 As shown in c, the surface of the gel beads is rough. Figure 1 d is an electron microscope image characterizing the internal structure of the gel beads. It can be observed that there are a large number of groove structures inside the gel beads, resulting in a wrinkled and curved surface inside, which is conducive to the multi-channel diffusion of uranium solution. This structure provides sufficient contact positions, increases the adsorption surface area, improves the adsorption capacity, and helps the PVA-SA / CS-SH gel beads to quickly adsorb U(VI).
[0052] Figure 2 The EDX analysis results of PVA-SA / CS-SH and PVA-SA / CS-SH+U are shown in Figure 1. Figure 2 a is the gel beads before uranium adsorption, Figure 2 b is the gel beads after uranium adsorption. The sample was subjected to elemental analysis. The EDX analysis results of PVA-SA / CS-SH and PVA-SA / CS-SH+U are shown in Figure 2 shown. Figure 2 The analysis of PVA-SA / CS-SH in a shows Si and S elements, indicating that (3-mercaptopropyl)trimethoxysilane grafting was successful and the mercapto functional group was introduced into the material. In addition, Ca elements also appeared, indicating that Ca 2+ with Na + Ion exchange occurs and the material is successfully cross-linked to form gel beads. Figure 2 b is the EDX characterization result after PVA-SA / CS-SH adsorbed U(VI). It can be seen that the U element was detected in the characterization result, and this analysis shows that PVA-SA / CS-SH successfully adsorbed U(VI) during the adsorption process.
[0053] Figure 3 This is the thermogravimetric curve (TGA) of PVA-SA / CS-SH gel beads. Figure 3 The middle horizontal axis is temperature, the left vertical axis is weight, corresponding to the solid curve, and the right vertical axis is DTG, corresponding to the dotted curve. The solid curve is mainly divided into three stages. The first stage is the decomposition of crystal water and the evaporation of adsorbed water, which occurs at 30-170°C; the second stage occurs at 214.45-308.22°C, and the mass loses sharply, which is mainly attributed to the bond breaking of organic reagents and the loss of organic functional groups; the mass continues to decrease in the third stage (308.22-501.06°C), which may be the chain breaking decomposition of SA and CS structures and the large-scale thermal decomposition of the polymer main chain. The remaining residue is mainly inorganic salts of sodium alginate.
[0054] Figure 4 The isotherms and pore size distribution of PVA-SA / CS-SH gel beads are shown. Figure 4 a is the adsorption-desorption isotherm of gel beads, Figure 4 b is the pore size distribution of gel beads. Figure 4 In a, the horizontal axis is the relative pressure and the vertical axis is the adsorption volume. Figure 4 In b, the horizontal axis is the pore diameter in nm, and the vertical axis is the pore volume in cm 3 / g. The BET surface area of PVA-SA / CS-SH gel beads was calculated by nitrogen adsorption / desorption isotherms. Figure 4 It can be seen that the PVA-SA / CS-SH gel beads belong to the type IV isotherm and show the H3 type hysteresis loop. A monomolecular adsorption layer is formed in the low pressure zone, and then the monomolecular layer gradually reaches saturation and begins to adsorb multiple molecular layers. The H3 type hysteresis loop indicates that the pore structure of the material is formed by the accumulation of layered structures. The specific surface area of the PVA-SA / CS-SH gel beads is 5.0680m 2 / g, and the total pore volume calculated by the single-point method is 0.0159 cm 3 / g, the pore size distribution is between 2-10nm, and the average pore size is 7.4747nm. This shows that PVA-SA / CS-SH gel beads are mainly mesoporous adsorption materials, providing a good mass transfer environment for the adsorption of U(VI).
[0055] Figure 5 XRD spectra of CS, BCS, BCS-SH, CH-SH and PVA-SA / CS-SH. Figure 5 The horizontal coordinate is 2θ degrees, and the vertical coordinate is intensity. The five curves from top to bottom in the figure are the XRD spectra of CS, BCS, BCS-SH, CH-SH and PVA-SA / CS-SH. Among them, the characteristic peak of CS appears at 20.3°, but there is no obvious characteristic peak near 10°. The reason is that this experiment uses chitosan with a high degree of deacetylation (95%). This corresponds to the Form Ⅱ crystal form of chitosan, which reflects strong crystallinity. BCS is chitosan grafted with benzaldehyde. The characteristic peak near 20° is broadened and the intensity decreases. This is because the -NH 2 The reaction with benzaldehyde caused a decrease in the hydrogen bond content and a decrease in the crystallinity of the material. Compared with the XRD spectra of CS, BCS, BCS-SH and CH-SH, the XRD spectrum of PVA-SA / CS-SH changed greatly, with small characteristic peaks appearing at 2θ=32.04° and 45.82°. Other peaks disappeared, and the main characteristic peak shifted from 20° to 22°, which can be attributed to the characteristic peak of sodium alginate. Moreover, the characteristic peak became broader and the intensity decreased, which may be due to the reaction of part of the sodium alginate with Ca 2+ The other part is cross-linked with CS. The XRD pattern of PVA-SA / CS-SH shows a new configuration, and the interaction between polyvinyl alcohol, sodium alginate and mercapto chitosan forms a new structure.
[0056] Figure 6 FTIR spectra of CS, BCS, BCS-SH, CH-SH and PVA-SA / CS-SH. Figure 6 In the figure, the horizontal axis is the wave number and the vertical axis is the transmittance. From bottom to top, the curves of CS, BCS (or BACS), BCS-SH (or BACS-SH), CH-SH and PVA-SA / CS-SH are shown. The functional groups of CS, BCS, BCS-SH, CH-SH and PVA-SA / CS-SH gel beads were further analyzed by FTIR spectroscopy. -1 The broad peak at corresponds to the stretching vibration of -OH and -NH 2 The superposition peaks of stretching vibrations. At 2923 and 2876 cm -1 The absorption peaks at 1653 and 1596 cm are due to the symmetric and asymmetric stretching vibrations of CH.-1 The characteristic peaks at 758 and 690 cm-1 correspond to the amide-Ⅰ (C=O stretching vibration) and amide-Ⅱ (NH bending vibration) groups. -1 The characteristic peak corresponding to the benzene ring appeared at 1598cm -1 The characteristic peak at corresponds to C=N, which indicates that the C 2 -NH 2 The characteristic peaks of benzaldehyde also appear in the spectrum of BCS-SH, and BCS-SH, CH-SH and PVA-SA / CS-SH are at 484 cm -1 New characteristic peaks appeared at 2349 cm-1, corresponding to the bending vibration of Si-O-Si, among which CH-SH and PVA-SA / CS-SH were at 2349 cm-1. -1 The characteristic peaks at 758, 690 and 1598 cm-1 correspond to the stretching vibration peaks of -SH. These results show that -SH was successfully grafted onto the material. -1 The characteristic peaks at 1000 nm have disappeared, indicating that the benzaldehyde protecting the amino group has been successfully removed. The above analysis shows that the PVA-SA / CS-SH gel beads were successfully prepared.
[0057] Example 3
[0058] This example is to conduct a uranium adsorption experiment on the PVA-SA / CS-SH aerogel beads prepared in the above Example 1, and specifically examine the effect of pH.
[0059] Dissolve 2.1091 g of uranyl nitrate hexahydrate in deionized water and add 10 mL of 0.1 mol / L HNO 3 , dilute to 1L with deionized water to obtain a 1g / L uranium original solution. In subsequent experiments, the uranium original solution was diluted to 50mg / L and 0.1MHNO 3 Or NaOH to adjust the pH of the solution (2-10). A certain amount of PVA-SA / CS-SH was added to a conical flask containing U(VI) solution. All adsorption experiments were carried out in a reciprocating water bath shaker at 130 rpm. After reaching adsorption equilibrium, a 0.22 μm microfiltration membrane was used to separate the solid phase and the liquid phase. Arsenazo (III) was used as a color developer, and the absorbance of the supernatant was measured at 652 nm using a UV-visible spectrophotometer to calculate the U(VI) concentration. The amount of U(VI) removed by the adsorbent q e (mg / g) and removal rate R are calculated by the following two formulas:
[0060]
[0061]
[0062] Among them C 0 and C e are the initial concentration and equilibrium concentration of U(VI) ions (mg L -1 ). V is the volume of U(VI) solution (L), and m is the amount of adsorbent (g).
[0063] Figure 7 The adsorption effect of gel beads on uranium under different pH conditions and its Zeta potential diagram. Figure 7 a is the adsorption effect of PVA-SA / CS-SH gel beads and sodium alginate / chitosan gel beads (SA / CS) on uranium under different pH conditions. The upper curve is the curve of PVA-SA / CS-SH gel beads, and the lower curve is the curve of SA / CS gel beads. The pH value of the initial solution is the most important factor in the adsorption process of U(VI) on PVA-SA / CS-SH gel beads. To this end, the present invention explores the adsorption capacity of PVA-SA / CS-SH for U(VI) when the pH value of the initial solution is in the range of 2-10, and compares it with sodium alginate / chitosan gel beads (SA / CS). V from Figure 7 aIt can be seen that the adsorption amount of U(VI) by cross-linking SA and CS without group modification and material modification is not high. In contrast, PVA-SA / CS-SH has excellent adsorption effect on U(VI). It can be seen that PVA-SA / CS-SH has the strongest adsorption capacity for U(VI) at pH=6, with an adsorption amount of 340.51 mg / g. The adsorption amount of PVA-SA / CS-SH is relatively low in the high acid region, and the adsorption amount increases with the increase of pH, and reaches the maximum value at pH=6.
[0064] Figure 7 b is the Zeta potential diagram of PVA-SA / CS-SH gel beads under different pH conditions, and its ordinate is the Zeta potential value. Figure 7 b It can be seen that the Zeta potential of PVA-SA / CS-SH in the pH range of 2-7 is positive, which indicates that the surface of PVA-SA / CS-SH gel beads is positively charged. This phenomenon can be attributed to the presence of a large amount of H + , resulting in the -NH 2 Protonation occurs In this pH range, uranium is mainly present as UO 2 2+ exists in the form of PVA-SA / CS-SH and UO 2 2+ Electrostatic repulsion occurs, affecting its adsorption capacity. As the pH increases, -NH3 + Deprotonation occurs and it turns back to -NH 2 , at this time, OH in the solution - The content increases and forms complexes with uranyl ions, such as UO 2 (OH) + ,(UO 2 ) 2 (OH) 2 2+ and (UO 2 ) 3 (OH) 5 + , the adsorption capacity increases. When the pH value continues to increase, the uranyl ion complex changes again and becomes a negatively charged group, such as UO 2 (OH) 3 - and (UO 2 ) 3 (OH) 7 - The Zeta of PVA-SA / CS-SH gradually changes to a negative potential, and the surface of the gel beads begins to carry a negative charge, which electrostatically repels uranyl ions, resulting in a low adsorption amount in the high alkaline region.
[0065] Example 4
[0066] This example is to conduct a uranium adsorption experiment on the PVA-SA / CS-SH aerogel beads prepared in the above Example 1, and specifically examine the effect of contact time.
[0067] Figure 8 Schematic diagram of the adsorption of U(VI) by PVA-SA / CS-SH at different contact times. Figure 8 a shows the effect of contact time on the change of the adsorption rate of U(VI) on PVA-SA / CS-SH. Figure 8 b is the linear fit of the intra-particle diffusion curve. Figure 8 The multiple dots in a represent experimental data. At the inflection point of the curve at around 80 min, the curves from top to bottom represent the pseudo-first-order kinetic model, pseudo-second-order kinetic model, Elovich model, and intraparticle diffusion kinetic model. The reaction conditions are: C 0 =50mg / L, m / V=0.125g / L, pH=6.0, T=313K.
[0068] Contact time is a key factor affecting the adsorption rate of U(VI) by adsorbents. Various kinetic models were established to analyze the adsorption process and explore the mass transfer rate-limiting step in the adsorption process. Figure 8a It can be seen that within 0-2h, the adsorption amount of U(VI) by PVA-SA / CS-SH increases rapidly, because the concentration of U(VI) in the solution is high in the initial stage, which can diffuse rapidly on the surface of the adsorbent, and the surface of the adsorbent can also provide sufficient adsorption active centers, so the adsorption amount increases significantly. With the increase of contact time, U(VI) is constantly captured by the adsorbent, causing the concentration of U(VI) to decrease, reducing the diffusion rate. The adsorption active centers of the adsorbent gradually decrease and cannot provide enough sites. The gel beads stay in the solution for a long time, and the steric hindrance increases, thereby increasing the mass transfer resistance, resulting in a slowdown in the adsorption rate and a decline. The reaction equilibrium is almost reached at about 6h. In order to explain the effect of contact time on the adsorption process of PVA-SA / CS-SH, the pseudo-first-order (Eq.3), pseudo-second-order (Eq.4), intraparticle diffusion kinetic model (Eq.5) and Elovich model (Eq.6) are established to simulate the adsorption kinetic data:
[0069]
[0070]
[0071]
[0072]
[0073] In the formula, q t (mg / g) is the adsorption capacity at adsorption time t (min), q e is the adsorption capacity at adsorption equilibrium. 1 (min -1 ) and k 2 (g mg -1 min -1 ) are the rate constants of pseudo-first-order and pseudo-second-order kinetic equations, respectively. ip is the intraparticle diffusion rate constant (mg g –1 min –0.5 ), C i is the boundary layer constant. α(mg g -1 -min) is the initial adsorption rate, β(g mg -1 ) is related to the degree of surface coverage and the activation energy of chemical adsorption.
[0074] The fitting results are as follows Figure 8 shown. Figure 8In a, the comparison of pseudo-first-order, pseudo-second-order, intraparticle diffusion kinetic models and Elovich simulation shows that the fitting coefficient of the pseudo-second-order kinetic model is 0.996, which is the highest among the four models. The theoretical equilibrium adsorption capacity simulated by the pseudo-second-order kinetic model is 358.76 mg / g, which is closer to the actual equilibrium adsorption capacity (350.33 mg / g). This shows that the pseudo-second-order kinetic model is more suitable for describing the adsorption process of U(VI) by PVA-SA / CS-SH. The results show that chemical adsorption is the rate-limiting step of the adsorption process, and the functional groups on PVA-SA / CS-SH undergo complexation with U(VI). Figure 8 b is the linear fit of the intraparticle diffusion curve, which can visually observe the steps of intradiffusion. Three linear components appeared in the fitting results, indicating that there are three stages in the adsorption process. The three straight lines from left to right in the figure represent the first stage, the second stage and the third stage respectively. In the first stage, U(VI) undergoes a rapid diffusion process on the adsorbent surface, and the adsorption rate is the fastest. In the second stage, the intraparticle diffusion process occurs. As the adsorption proceeds, the active sites of the adsorbent are gradually occupied. The diffusion rate of this process is lower than that of the first stage. The third stage represents the dynamic adsorption equilibrium of adsorption and desorption between U(VI) and PVA-SA / CS-SH gel beads, and the adsorption reaction almost reaches equilibrium. The fitting curve is not a straight line passing through the origin of the coordinate axis, indicating that the adsorption process is not controlled by a single factor of intraparticle diffusion, and there are other processes involved in the rate control of the adsorption process.
[0075] Example 5
[0076] This example is to conduct a uranium adsorption experiment on the PVA-SA / CS-SH aerogel beads prepared in the above Example 1, and specifically examine the adsorption isotherm and the maximum adsorption amount of uranium by the aerogel beads.
[0077] The use of isotherm models can facilitate the study of the bonding mode between the adsorbent and the adsorbate, as well as the adsorption behavior and mechanism of the adsorbent in the solid and liquid phases. Three models, Langmuir, Freundlich and Dubinin-Raduschkevich (DR) isotherm models, were established to explore the adsorption behavior and mechanism of PVA-SA / CS-SH in the range of uranium initial concentration of 10-100 mg / L.
[0078] Among the three isotherm models, the Langmuir model has the highest average fitting coefficient of 0.996, which is much larger than the average fitting coefficients of the Freundlich model (0.975) and the DR model (0.763). The theoretical maximum adsorption capacity simulated by the Langmuir model is also more consistent with the actual adsorption results, so it is the most suitable model for describing the adsorption process of PVA-SA / CS-SH on U(VI).
[0079] Combining the fitting data of Langmuir, Freundlich and DR isotherm models, it is shown that the adsorption process of PVA-SA / CS-SH on U(VI) belongs to the chemical adsorption of homogeneous monolayer. At 313K, the maximum adsorption amount of PVA-SA / CS-SH on U(VI) simulated by the Langmuir isotherm model is 664.56 mg / g, indicating that PVA-SA / CS-SH is a potential and excellent adsorption material.
[0080] Example 6
[0081] This example is to conduct a uranium adsorption experiment on the PVA-SA / CS-SH aerogel beads prepared in the above Example 1, and specifically examine the adsorption temperature and adsorption thermodynamics.
[0082] In order to further explore the adsorption mechanism, the thermodynamic analysis of PVA-SA / CS-SH on U(VI) was carried out in the range of 303-323 K to explore the change of its adsorption capacity. The experimental results show that increasing the temperature based on 313 K does not significantly increase the adsorption amount. From the perspective of energy saving and environmental protection, 313 K is selected as the optimal reaction temperature.
[0083] Example 7
[0084] This example is to conduct a uranium adsorption experiment on the PVA-SA / CS-SH aerogel beads prepared in the above Example 1, and specifically examine the influence of coexisting ions and the reusability of PVA-SA / CS-SH.
[0085] Fig. 9 The effect of coexisting ions on uranium adsorption experiments on PVA-SA / CS-SH aerogel beads. The adsorption conditions in the figure are: m / V = 0.125g / L, pH = 6.0, T = 313K, t = 300min. In order to explore the effect of other ions on the adsorption of U(VI) by the material, experiments with coexisting ions of different concentrations were conducted. Uranium wastewater is generally an acidic environment, containing a large amount of Cl - and SO 4 2- In addition, there are other anions and cations, so the following ions are selected for exploration experiments. Fig. 9 As shown. In the anion Cl - and NO 3 - It has almost no effect on the adsorption process. 3 2- and SO 4 2- The presence of SO reduces the adsorption effect of the material. This is because SO 4 2-It will form complexes with uranyl ions, such as (UO 2 ) 4 (OH) 7 (SO 4 ) 4 7- , and can also form insoluble complexes such as UO 2 SO 4 (aq), cannot be adsorbed by the adsorbent, resulting in a decrease in the adsorption amount. + and Na + The adsorption of U(VI) is not affected much because the ionic radius of the above ions is quite different from that of uranyl ions and they cannot compete with uranyl ions for adsorption. 2+ and Fe 3+ The biggest influence on the adsorption effect is Cu 2+ The ionic radius of Fe is similar to that of uranyl ion, and the two form competitive adsorption, which interferes with the adsorption process. 3+ The amino and thiol groups on PVA-SA / CS-SH can easily react with Fe 3+ The coordination complexation occurred, and the active centers of the adsorbent were occupied, which inhibited the adsorption of U(VI). In general, PVA-SA / CS-SH has good selective adsorption for U(VI).
[0086] Fig.10 The structure diagram of five cycles of adsorption-desorption experiment on PVA-SA / CS-SH. The adsorption conditions in the figure are: C 0 =50mg / L, m / V=0.125g / L, pH=6.0, T=313K, t=300min. The horizontal axis in the figure is the number of cycles, the vertical axis on the left is the amount of uranium removed by the adsorbent, corresponding to the bar graph, and the vertical axis on the right is the desorption rate, corresponding to the dot line.
[0087] The reuse performance of the material was explored as a consideration for environmental protection and economic benefits. 3 The solution was used as the desorbent of PVA-SA / CS-SH to test its repeatability. Fig.10 As shown in the figure, with the increase of adsorption-desorption times, the adsorption capacity of the material gradually decreased. In the fifth cycle adsorption-desorption experiment, the removal rate of U(VI) can still reach 81.19%. In multiple cyclic adsorption-desorption experiments, part of the material itself may undergo acid hydrolysis, thus affecting the overall adsorption effect. Uranyl ions will also combine with the adsorbent to consume part of the active sites, resulting in a decrease in adsorption capacity. The results show that PVA-SA / CS-SH has excellent reusability and good recyclability.
[0088] Example 8
[0089] This example is a characterization of the PVA-SA / CS-SH aerogel beads prepared in the above Example 1 before and after being used for uranium adsorption and an analysis of the adsorption mechanism.
[0090] Fig.11 The EDS mapping and EDS characterization images of PVA-SA / CS-SH aerogel beads after uranium adsorption. Fig.11 a is the EDS mapping diagram, Fig.11 b is the EDS characterization diagram. The sample after adsorption of U(VI) was characterized and analyzed using two-dimensional elemental analysis (EDS-Mapping). Fig.11 In a, we can clearly see the presence of uranium in the material. Fig.11 The uranium ray peak can also be observed in b, indicating that U(VI) is successfully adsorbed by the material. In addition, the presence of sulfur, calcium and other elements can be observed in the EDS mapping and EDS characterization, further indicating that the modified material was successfully prepared.
[0091] Fig.12 It is the full spectrum of FTIR spectrum and XPS spectrum of PVA-SA / CS-SH before and after adsorption. Fig.12 a is the FTIR spectrum, Fig.12 b is the XPS spectrum. Fig.12 The upper curve in a is the aerogel beads before uranium adsorption, and the lower curve is the aerogel beads after uranium adsorption. The horizontal axis in the figure is the wave number, and the vertical axis is the transmittance. Fig.12 The upper curve in b is the aerogel beads after uranium adsorption, and the lower curve is the aerogel beads before uranium adsorption. The horizontal axis is the binding energy and the vertical axis is the intensity. In order to explore the adsorption mechanism of PVA-SA / CS-SH on U(VI), X-ray photoelectron spectroscopy (XPS) and Fourier transform infrared spectroscopy (FT-IR) were used to characterize and analyze PVA-SA / CS-SH before and after adsorption of U(VI). Fig.12 In a, the curve after adsorption is at 896cm -1 A new characteristic peak appears at 2349 cm, corresponding to the antisymmetric stretching vibration of O=U=O, indicating that U(VI) is successfully adsorbed by PVA-SA / CS-SH. -1 The characteristic absorption peak corresponding to -SH shifts to a lower wave number after adsorption, and the characteristic absorption peak changes from a sharp peak to a smooth broad peak. This indicates that -SH participates in the adsorption reaction during the adsorption of U(VI) and plays an important role. Fig.12In b, the XPS spectrum after adsorption showed a characteristic peak corresponding to U 4f, which once again confirmed that PVA-SA / CS-SH successfully adsorbed U(VI). In addition to U4f, S2p, N 1s, C 1s, and O1s also appeared in the full XPS spectrum of PVA-SA / CS-SH, further indicating that the material was successfully prepared.
[0092] In addition, PVA-SA / CS-SH was compared with other highly efficient U(VI) adsorbents, such as MWCA, aMSP / SA, ZnNiA1-LDHs, PCG, and CS / AL-AP reported in the literature. The removal capacity of U(VI) by PVA-SA / CS-SH was as high as 350.33 mg g -1 , showing excellent adsorption performance.
[0093] In summary, the present invention uses sodium alginate and chitosan as raw materials, successfully introduces thiol functional groups by grafting (3-mercaptopropyl) trimethoxysilane, uses calcium chloride as a cross-linking agent, and adopts gel-vacuum freeze-drying method to prepare polyvinyl alcohol-sodium alginate / thiol functionalized chitosan aerogel beads (PVA-SA / CS-SH). Specifically, the present invention first uses benzaldehyde to react with the amino group in chitosan to produce a Schiff base, synthesizes amino-protected benzaldehyde-chitosan (B-CS), and reacts with (3-mercaptopropyl) trimethoxysilane to introduce thiol functional groups, and then removes benzaldehyde to obtain thiol-chitosan (CS-SH). The mixed solution of thiol-chitosan and polyvinyl alcohol and sodium alginate is cross-linked by calcium chloride solution, and polyvinyl alcohol-sodium alginate / thiol functionalized chitosan aerogel beads (PVA-SA / CS-SH) are prepared by gel-vacuum freeze-drying. The present invention also provides the application of the aerogel beads in the treatment of uranium-containing wastewater.
[0094] The characterization results show that there are a large number of groove structures and stacked cavities inside the PVA-SA / CS-SH gel beads, which provide excellent mass transfer conditions for the adsorption of U(VI). At pH = 6, T = 313K, m / V = 0.125 g / L (solid-liquid ratio), C 0 =50mg L -1Under the experimental conditions, the adsorption reaction reached equilibrium at 300 min, and the maximum adsorption amount of PVA-SA / CS-SH for U(VI) was 350.33 mg / g. The adsorption process was more consistent with the Langmuir isotherm adsorption model and the pseudo-second-order kinetic model. The adsorption isotherm, adsorption kinetics and adsorption thermodynamic parameters showed that the adsorption was a monolayer homogeneous, spontaneous endothermic process dominated by chemical adsorption. The intraparticle diffusion model showed that the adsorption process was divided into three steps. In the first stage, a rapid diffusion process occurred on the surface; in the second stage, an intraparticle diffusion process occurred; in the third stage, the adsorption rate slowed down and entered a dynamic adsorption equilibrium state. The adsorption effect of PVA-SA / CS-SH on U(VI) was mainly the coordination / chelation of amino, hydroxyl and thiol groups.
[0095] PVA-SA / CS-SH has good reusability and adsorption selectivity, low cost and economical performance, and is expected to become a new type of efficient uranium removal adsorbent.
[0096] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.
Claims
1. Application of aerogel beads in adsorbing uranium, It is characterized in that The aerogel beads are polyvinyl alcohol-sodium alginate / thiol-functionalized chitosan aerogel beads, namely PVA-SA / CS-SH aerogel beads; and the preparation method of the aerogel beads comprises the following steps: Step A: first use benzaldehyde and chitosan to prepare benzaldehyde-chitosan, namely BCS; specifically, in step A, dissolve chitosan in acetic acid solution, add methanol, and after chitosan is completely dissolved, add a mixed solution of benzaldehyde and methanol; fully react at room temperature to obtain a light yellow gel; wash the gel with methanol and anhydrous ethanol for several times to wash away unreacted benzaldehyde, and then dry it to obtain amino-protected chitosan, namely BCS; Step B: preparing benzaldehyde-thiol functionalized chitosan, namely BCS-SH; specifically, in step B, taking the BCS prepared in step A and dispersing it in toluene, adding (3-mercaptopropyl)trimethoxysilane to obtain a mixture, ultrasonically dispersing the mixture, and then performing a hydrothermal reaction; after the reaction is completed, naturally cooling to room temperature, washing the obtained solid reactant with toluene and anhydrous ethanol for several times, respectively, and drying to obtain BCS-SH; Step C: Then prepare thiol-functionalized chitosan, i.e., CS-SH; specifically, in step C, the BCS-SH prepared in step B is hydrolyzed with hydrochloric acid to remove the benzaldehyde used to protect the amino group and the chitosan that is not successfully grafted with the thiol group, and then washed with anhydrous ethanol and deionized water for several times, and then dried to obtain CS-SH; Step D: using polyvinyl alcohol and sodium alginate as well as the CS-SH prepared in step C and adopting a gel-vacuum freeze-drying method to prepare polyvinyl alcohol-sodium alginate / thiol functionalized chitosan aerogel beads, namely PVA-SA / CS-SH; specifically, in step D, a mixed solution containing polyvinyl alcohol, sodium alginate and CS-SH is added dropwise to a calcium chloride solution to form gel beads by cross-linking; the gel beads are immersed in the calcium chloride solution and then washed several times with deionized water to remove uncross-linked calcium chloride; the gel beads are then frozen and vacuum freeze-dried to obtain the PVA-SA / CS-SH.
2. Use of the aerogel beads according to claim 1 in adsorbing uranium, It is characterized in that The deacetylation degree of the chitosan is above 95%; and the alcoholysis degree of the polyvinyl alcohol is 98-99 mol%.
3. Use of the aerogel beads according to claim 1 in adsorbing uranium, It is characterized in that In step A, the concentration of the acetic acid solution is 1-3%, the reaction time for fully reacting at room temperature to obtain a light yellow gel is more than 24 hours, the drying temperature of the gel is 60-70° C., and the drying time is more than 10 hours.
4. Use of the aerogel beads according to claim 1 in adsorbing uranium, It is characterized in that In step B, the ultrasonic dispersion time of the mixture is more than 10 minutes, the hydrothermal reaction includes charging the mixture into a hydrothermal reactor with a polytetrafluoroethylene liner, reacting at 105-120° C. for more than 12 hours, and the drying is carried out at 60-70° C. for more than 6 hours.
5. Use of the aerogel beads according to claim 1 in adsorbing uranium, It is characterized in that In step C, the concentration of hydrochloric acid is 0.2-1 mol / L, the temperature of hydrolysis with hydrochloric acid is 50-70° C., the hydrolysis time is more than 6 hours, and the drying is carried out at 60-70° C., and the drying time is more than 6 hours.
6. Use of the aerogel beads according to any one of claims 1 to 5 in adsorbing uranium, It is characterized in that In step D, polyvinyl alcohol and sodium alginate are first dissolved in deionized water, heated and stirred to form a uniform mixed solution; then transferred to a low-temperature water bath, CS-SH prepared in step C is added and stirred, and after being completely dissolved, naturally cooled to room temperature to obtain a mixed solution; the mixed solution is added dropwise to a calcium chloride solution to cross-link to form gel beads; the gel beads are immersed in the calcium chloride solution, and then washed with deionized water for several times to remove uncross-linked calcium chloride; the gel beads are then frozen and vacuum freeze-dried to obtain the PVA-SA / CS-SH.
7. Use of the aerogel beads according to claim 6 in adsorbing uranium, It is characterized in that In step D, a water bath is used for heating and stirring, and the water bath heating temperature is 85-95° C., and the time is more than 1 hour; the temperature of the low-temperature water bath is 75-82° C., the CS-SH is added and stirred for more than 3 hours, and the mixed solution is added dropwise to the calcium chloride solution using a syringe, the concentration of the calcium chloride solution is 2-5wt%, the gel beads are immersed in the calcium chloride solution for more than 5 hours, the freezing temperature is -35° C. to -25° C., the freezing time is more than 2 hours, and the vacuum freeze-drying temperature is -55° C. to -45° C., and the time is more than 6 hours.