Glass or glass-ceramic sheet comprising a coating arranged on one side and method of manufacturing thereof

By using a single-layer coating of silicone matrix and pigments on glass or glass-ceramic plates, the problems of insufficient scratch resistance and oil penetration resistance of coatings are solved, achieving high adhesion and scratch resistance, while simplifying the manufacturing process and reducing costs.

CN117447090BActive Publication Date: 2026-11-20SCHOTT AG
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202310917513.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-07-25
Filing Date
2023-07-25
Publication Date
2026-11-20
Estimated Expiration
2043-07-25

AI Technical Summary

Technical Problem

Existing coated glass or glass-ceramic panels have insufficient scratch resistance and oil penetration resistance in terms of back coating, and the manufacturing process is complex and costly, making it difficult to simultaneously meet the requirements of high adhesion, scratch resistance and oil resistance.

Method used

A single-layer coating containing an organosilicon matrix and pigments is used, with a coating thickness of at least 10 μm. The coating is fired at 200°C to 400°C using two organosilicon precursors as binders to ensure the coating's scratch resistance and impermeability.

Benefits of technology

It achieves high scratch resistance and oil penetration resistance in a single-layer coating, simplifies the manufacturing process, reduces production costs, and improves mechanical strength and impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117447090B_ABST
    Figure CN117447090B_ABST
Patent Text Reader

Abstract

The present invention relates generally to a coated glass or glass-ceramic plate that can be used as a cover plate of a cooking appliance, for example. In particular, the present invention relates to a glass or glass-ceramic plate comprising a coating arranged on at least one side of a glass or glass-ceramic substrate, and to a method for their manufacture. The coating comprises a silicone matrix and pigments, and has a scratch resistance, and as a single layer a very good scratch resistance as well as a very good oil resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention generally relates to a coated glass or glass-ceramic plate that can be used as a cover for, for example, a cooking utensil. In particular, the invention relates to a glass or glass-ceramic plate comprising a coating disposed on at least one side of a glass or glass-ceramic substrate, and to methods of manufacturing such a plate. The coating comprises a silicone matrix and pigments, and has scratch resistance, exhibiting very good scratch resistance and very good oil resistance as a single layer. Background Technology

[0002] For many years, coated glass or glass-ceramic plates have been used as covers for cooking appliances (e.g., "stovetops" or "oventops"). In recent years, covers incorporating glass or glass-ceramic materials have been developed, consisting of a transparent glass or glass-ceramic material and a coating on one side of the respective glass or glass-ceramic substrate that prevents the material from being seen through. This coating is positioned away from the observer or user of the cooking appliance in its installed state and is often referred to as a bottom coating or back coating.

[0003] These back or bottom coatings are subject to various requirements during assembly and operation; however, their arrangement on the back or bottom of the panel also determines its impact resistance in relation to operation and use. Impact resistance here refers to the strength of the panel to resist mechanical stresses "from above" or "from the front," and the use of coated panels as stovetop covers can be illustrated by placing cookware on the stovetop (even roughly if necessary).

[0004] Because of the so-called "thermal mismatch," that is, the difference in thermal expansion that can occur between the substrate and the coating applied to the substrate, especially in the case of substrates with low expansion, and particularly in the case of coatings on the back side, especially those with good adhesion and / or scratch resistance, cracks are often induced in the substrate (e.g., due to high aging temperatures and mismatch caused when cooling the coated substrate to room temperature). These cracks reduce the mechanical strength of the substrate. It can therefore easily fail due to tensile stresses caused by loads acting on the substrate from above, such as by items placed on the board, such as cookware. Therefore, it is advisable to use glass-based coatings that have particularly good adhesion, scratch resistance, and also meet other requirements of impermeability and cleanability, and are not defined as "back coatings" or "bottom coatings," especially when using substrates with relatively low elongation, such as certain glass ceramics or glass.

[0005] Therefore, coatings with lower adhesion than conventional glass-based coatings are particularly suitable for use as back or bottom coatings. For example, coatings based on silicone or silicone-based sol-gel binders have been proposed. Such coatings do not lead to the formation of molten reaction zones like conventional glass-based coatings, and therefore, for this reason alone, the risk of cracking is lower. However, they also have the disadvantage of lower adhesion. To ensure the strength of a board covered with such a coating, it is generally advantageous if the coating is porous against the substrate. However, this porosity is disadvantageous because the back or bottom surface of the cover is frequently in contact with fluid media, whether adhesive residues, water vapor, or oil, or, in the case of a cover in a gas stove-driven stove, spilled food reaching the bottom surface of the cover through holes in the stove. Another disadvantage of porous layers is generally their low scratch resistance. A corresponding coating is described, for example, in German patent application DE 10 2008 031 428 A1.

[0006] For this reason, another coating, also known as a "sealing," is usually applied over the first layer, which is actually colored and visible to the user through the substrate. This second coating typically has a different composition than the first coating and may require different firing conditions. It is also possible that the first and second coatings have different chromaticity coordinates. This is particularly disadvantageous when the first coating is shallow and the second coating is deep. In this case, the first coating must be applied particularly thickly, otherwise the second coating will seep through the first coating and alter its chromaticity coordinates. A similar coating is described, for example, in German patent application DE 10 2008 031 426 A1.

[0007] The combination of coloring and sealing layers also implies additional coating and tempering steps, and is therefore disadvantageous from both an economic and CO2 balance perspective.

[0008] For example, European patent document EP 1 730 085 B1 describes a plate composed of glass or glass-ceramic and having a colored coating in at least one region on at least one side, wherein the coating comprises at least one polysiloxane resin, which is a virtually carbon-free material, and wherein the filler content of the coating is between 10% and 60% by volume. Its disadvantage is the virtually carbon-free coating according to this patent document, because a sufficiently dense coating cannot be obtained in this way, particularly in terms of resistance to oil penetration.

[0009] International patent application WO 2005 / 092810 A2 describes a method for increasing the strength of glass or glass-ceramic plates. It does not describe a colored coating with high oil penetration resistance.

[0010] Japanese patent application JP 2011 / 216457 A1 describes a plate comprising a substrate made of glass or glass-ceramic, wherein the plate has a bottom coating comprising various coatings. Specifically, the structure of the coloring coating 3 differs from that of the heat-resistant resin layer 4, and a further resin layer 5 may be coated to further improve the performance of the first resin layer 4. The described plate therefore has a very complex layer structure, in which methods such as sputtering or glass-based coatings can be used.

[0011] Japanese Patent JP 6 231 066 B2 describes a product in which a coating of silicone resin is applied to a glass or glass-ceramic substrate, the silicone resin having branched alkyl chains. This process is disadvantageous because the organic components must be burned at very high temperatures, such as approximately 350°C. However, it is impossible to produce a dense and scratch-resistant coating simultaneously in this manner. When the organic components burn off, a porous layer is formed.

[0012] Furthermore, Japanese Patent 206 024B2 describes a coated glass plate comprising two different composite coatings: a decorative coating and a light-shielding coating. The decorative coating, in addition to SiO2 as an essential component, also includes another metal oxide such as MnO and / or CoO.

[0013] Japanese patent application JP 2019 / 519458 A1 describes a coating on a glass or glass-ceramic plate comprising a silicone binder and nano-pigments. No description is made regarding the coating's scratch resistance or sealing properties.

[0014] European patent application EP 3 511 631 A1 also describes a multilayer structure comprising a first decorative layer and a second heat-resistant resin layer. This layer comprises pigments with very small particle sizes. The resin layer can also be applied directly to the substrate. There is no description regarding the oil resistance of the coating.

[0015] European application EP 3 222 595 A1 describes a stovetop appliance comprising a partially translucent layer element. There is no mention of oil tightness or scratch resistance.

[0016] International patent application WO 2020 / 122069 A1 describes a cooking plate comprising a heat-resistant resin layer. It includes flake-like inorganic fillers, particularly alumina. No description is made regarding oil resistance.

[0017] In other words, the manufacturing of existing back-coated glass or glass-ceramic panels is demanding and expensive. Therefore, there is a need for glass or glass-ceramic panels that at least partially mitigate the aforementioned weaknesses of the prior art. Furthermore, there is a need for methods for their manufacture. Summary of the Invention

[0018] The object of the present invention is to provide a glass or glass-ceramic plate and a method for manufacturing the same, the glass or glass-ceramic plate comprising at least one coating disposed on at least one side, the coating at least partially mitigating the weaknesses of the prior art.

[0019] The objective is addressed by the subject matter of the independent claims. Preferred and specific embodiments are the subject matter of the dependent claims, as well as the description and drawings of the invention.

[0020] Therefore, the present invention relates to a glass or glass-ceramic plate comprising a glass or glass-ceramic substrate and a coating disposed on at least one side of the glass or glass-ceramic substrate, the coating comprising an organosilicon matrix and a pigment. The coating has a thickness of at least 10 μm and preferably at most 80 μm. The coating has scratch resistance and oil resistance greater than 7N and preferably at most 30N in the area of ​​the glass or glass-ceramic plate where the coating is disposed only on the glass or glass-ceramic substrate, as tested according to DIN-ISO 1518-1, wherein the chromaticity coordinate change ΔE determined through the glass or glass-ceramic substrate is less than 1, preferably less than 0.5, particularly preferably less than 0.3, very particularly preferably less than 0.2, and most preferably less than 0.1, wherein the chromaticity coordinate change ΔE is determined in the L*a*b* system and given by the following formula:

[0021]

[0022] Here, chromaticity coordinate 1 refers to the chromaticity coordinate of the glass or glass-ceramic substrate before the colored oil is applied, and chromaticity coordinate 2 refers to the chromaticity coordinate after the colored oil is applied.

[0023] The testing is preferably conducted as follows:

[0024] The oil is preferably colored with a blue dye, such as the one sold under the trade name Orasol Blue 855. This dye is generally made from a copper phthalocyanine complex, also known as CI Solvent Blue 70 (CAS No. 12237-24-0). For this purpose, 0.5 g of the powdered dye is first dissolved in 10 ml of isopropanol. Then, a commercially available oil, such as sunflower oil, is used to bring the solution to a final volume of 50 ml.

[0025] The composition range of commercially available sunflower seed oil suitable for this test can be found in the following list (see also de.wikipedia.org / wiki / ). (Date: May 4, 2022):

[0026]

[0027] Then provide test samples. The minimum size here is 80*80mm. 2The sample is made of coated glass or glass-ceramic plate. Preferably, the sample consists only of the substrate and the coating to be tested. The chromaticity coordinates of the coating are determined before loading, particularly through the substrate. Then, 2 ml of the colored edible oil, preferably commercially available sunflower oil, is added to the coating as described above, and the sample with the colored oil is then heated in an oven at 150°C for 3 hours. The chromaticity coordinates of the coating are then determined again through the substrate. The chromaticity coordinates are determined separately using a colorimetric device and in the CIE-L*a*b* system. The chromaticity coordinate change ΔE is then determined based on the measurements before and after loading. It is also possible, and preferably preferred, in the case of large samples, to determine the chromaticity coordinates at untreated and oil-treated points on the sample, and thereby determine the chromaticity coordinate change. This is feasible because the heat treatment temperature of 150°C is too low to cause a change in the chromaticity coordinates of the coating itself. Therefore, the chromaticity coordinates of the untreated points correspond to the chromaticity coordinates before treatment within the range of measurement accuracy. To eliminate any errors and human factors (Artefakt), the reference sample can also be tempered to avoid human factors, such as if the sample was contaminated in the furnace itself.

[0028] Generally, it is advantageous to proceed in the following manner:

[0029] A ring, preferably made of commercially available stainless steel or comprising commercially available stainless steel, with an inner diameter of 40 mm, is preferably placed on the coated side of the plate / substrate. For example, the outer diameter may be 57 mm, where the exact dimensions of the outer diameter are understood only as an example. This ring specifically serves as a limit to prevent uncontrolled leakage of oil. 2 ml of colored oil is then added to the ring, preferably by dropwise addition using a pipette. The ring is then capped, for example, with a clock glass cap, to prevent rapid evaporation of the oil. The colored oil sample is then placed in a laboratory oven and heated to 150°C. It is maintained at 150°C for three hours. After the sample cools, the ring and cap are removed, and any remaining oil on the coated surface is wiped away with a cloth such as cellulose.

[0030] If the oil remains liquid and not sticky after temperature treatment, it may indicate that the oven temperature is too high.

[0031] The sample is then flipped and evaluated from the substrate side. First, a visual evaluation is performed. Furthermore, the chromaticity coordinates in the CIEL*a*b* system are determined using a colorimeter. For this purpose, the chromaticity coordinates are determined in the untreated and treated areas of the sample, and the chromaticity coordinate change ΔE is calculated based on the sample described above. Additionally, an untreated reference sample is preferably also recorded.

[0032] Chromaticity coordinates are preferably determined using a spectrophotometer from Konica-Minolta, specifically a CM 700d instrument, with a D65 light source and a 10° viewing angle. Measurement aperture (MAV) and measurement settings (SCI) can be used. Due to the high level of opacity of the test sample, the measurement is background-independent, meaning it is irrelevant whether the measurement is against a black (falle) or white background.

[0033] In the context of this invention, "plate" is understood to refer to a molded body whose thickness is at least an order of magnitude smaller than its length and width. Furthermore, within the scope of this invention, "glass or glass-ceramic plate" is understood to refer to a product comprising a glass or glass-ceramic substrate, wherein the glass or glass-ceramic substrate itself is plate-shaped. Unlike a glass or glass-ceramic substrate, a glass or glass-ceramic plate also includes at least one coating layer and can therefore also be understood as a refined substrate. The spatial dimensions and the glass or glass-ceramic substrate and the side surfaces of the glass or glass-ceramic plate largely correspond to each other, where it should be noted that the thickness of the glass or glass-ceramic plate is strictly greater than the thickness of the coating layer than the thickness of the (uncoated) glass or glass-ceramic substrate. However, the typical thickness of the glass plate / substrate or glass-ceramic plate / substrate considered herein is in the range of mm, which is negligible within the range of measurement accuracy.

[0034] This design scheme for glass or glass-ceramic panels, as described above, has many advantages.

[0035] In the present case, the coating is designed as a coating comprising an organosilicon matrix and pigments, i.e., as a cover layer or at least a partial cover layer. Within the scope of this invention, a cover or at least a partially cover coating (or layer) is understood to represent a coating that at least reduces light transmission through it. On the one hand, this is because the coating contains pigments, i.e., colorants, preferably temperature-stable and / or ceramic colorants, which reduce light transmission by absorption and / or scattering. On the other hand, the covering effect of the coating is also attributed to its thickness, as the coating has a thickness of at least 10 μm. In the context of this invention, colorants are understood to mean not only coloring pigments but also functional pigments, which are not necessarily colored themselves but can also be formed, for example, as pure silver pigments (e.g., corresponding to so-called "pearlescent pigments"). Generally, as described, these functional pigments do not necessarily have color due to their own absorption and are included under the general term "colorant" in the context of this invention.

[0036] In this way, an opaque effect can be achieved even when using pigments or coatings that do not inherently possess strong opacity, such as functional pigments based on transparent flakes (e.g., pearlescent pigments, such as those commercially available under the trademark "Iriodin") or coatings containing a large amount of such pigments. Here, a layer thickness of at least 10 μm, together with one or more pigments included in the coating, has an advantageous effect, thereby ensuring adequate coverage.

[0037] Pearlescent pigments are generally understood to refer to functional pigments based on mica. Specifically, the mica can be in the form of flakes and coated, where the coating itself can be a non-absorbent coating, such as a coating made of TiO2 or a coating containing TiO2. In this way, for example, a matte silver sheen can be achieved. It is also possible for such pearlescent pigments to contain multiple layers, thereby producing an interference effect. For example, a certain color impression can be achieved here through reflection. Coating materials that have an inherent color, such as Fe2O3, can also be used. In this case, the resulting pearlescent pigment has a slight color cast, but is still not an opaque absorbing pigment. For example, pearlescent pigments with yellow or gold chromaticity coordinates are known. In principle, other chromaticity coordinates are also possible, such as purple.

[0038] In the context of this invention, pearlescent pigments are also referred to as mica pigments.

[0039] In addition to at least one pigment, the coating also comprises a silicone matrix. The silicone matrix is ​​understood as the coating matrix, which can be referred to as the "binder," and is obtained from silicone precursor materials. Known silicone precursor materials include, for example, TEOS (tetraethyl orthosilicate), TMOS (tetramethyl orthosilicate), or their organically modified derivatives (m-TEOS, triethyl orthosilicate, DMDEOS, dimethyl diethyl orthosilicate, triethyl orthosilicate, etc.). Within the scope of this invention, silicone and polysiloxanes are also considered possible components of silicone binders. The silicone binder according to the invention can particularly comprise a variety of precursor materials. In particular, the binder can comprise a sol-gel component and a polysilsesquioxane or silicone resin component.

[0040] The coating itself is scratch-resistant, meaning that as a single layer on a glass or glass-ceramic substrate, it has a scratch resistance of over 7N in tests according to DIN-ISO1518-1.

[0041] Generally, within the scope of this invention, a material layer applied to a substrate by a coating step is referred to as a coating or layer.

[0042] Within the scope of this invention, a single layer is understood to refer to a coating or a layer having the same composition. This coating may be applied in multiple coating steps or in a single coating step. For example, within the scope of this invention, a single layer can also be obtained by two or more coating processes that are consecutive to each other, such as by double printing. This can be advantageous, for example, when the coating is only slightly opaque and results in only a small layer thickness in a single coating process, such as in screen printing. Such a coating can also be understood to comprise two partial layers of the same composition. Advantageously, at least one or more coating processes may be performed after the first coating process, such as the first printing, to obtain a sufficiently thick coating overall. It is also possible, but not absolutely necessary, to perform intermediate steps after the coating processes, such as heat setting of the previous coating.

[0043] In contrast to a single layer, within the scope of this invention, a layer (or coating) comprising layers of materials with different compositions is proposed, for example, relating to the type of one or more pigments used or the adhesive used. Within the scope of this invention, the adhesive may also be referred to as an adhesive phase or matrix, particularly when referring to a cured coating rather than a paste.

[0044] The coating of this invention on glass or glass-ceramic plates also exhibits excellent resistance in oil tests.

[0045] In the context of this invention, oil testing is understood to refer to a test that examines the permeability of a coating to oil. The visibility of fluid permeation through a coating and then through the coated substrate is a complex issue, especially when functional pigments are involved. This is because it has been shown that, depending on the exact composition of the coating, particularly when the coating contains functional pigments, fluid permeation can sometimes only be fully visible at certain angles. This differs from, for example, coatings designed as purely "body color," i.e., with little or no functional pigments. For example, water seeping into the coating pores is very easily seen here because the color appears darker as the pores are filled.

[0046] Therefore, the inventors developed the above-described test method to test the impermeability of the coating using the colored oil. If the coating is not dense enough, the oil, along with the added dye, will penetrate into the pores of the coating, and this can also be visually perceived on the "other side," i.e., the side where the coating is adjacent to the substrate, i.e., in the form of a color change, measured using chromaticity coordinates before and after the application of the colored oil. In the case of the coating according to the embodiment, the chromaticity coordinate change ΔE is not greater than 2, preferably even smaller; in other words, the chromaticity coordinate change ΔE is particularly preferably imperceptible. Therefore, the coating is considered sufficiently dense.

[0047] This configuration, in which a single layer is both scratch-resistant and impermeable, was previously unknown. Instead, it was previously assumed that at least two coatings were required, with different compositions, for example, due to different pigment or binder contents or different firing conditions. The first coating, directly disposed on the substrate, is porous, particularly due to firing at elevated temperatures, while the second coating disposed on top of the first is dense, where, in particular, hot firing at temperatures exceeding 300°C or 350°C is abandoned. Therefore, these known glass or glass-ceramic plates of the prior art comprise what is called a double layer, where the first and second coatings must be harmonized in terms of their composition, firing conditions, and, if applicable, the resulting color impression. Only in this way can it be ensured that the resulting glass or glass-ceramic plate possesses sufficient scratch resistance, sufficient impermeability, and sufficient mechanical strength under conditions of use.

[0048] The inventors suspect that the disclosed single-layer scratch resistance and simultaneous impermeability are due to the special design of the adhesive used. Therefore, the coating composition used to produce glass or glass-ceramic plates according to the embodiments comprises an adhesive containing at least two silicone precursors. One silicone precursor is a silicone resin, particularly a commercially available silicone resin, while the other silicone precursor is a sol-gel hydrolysis product. In addition to the adhesive, the coating composition also includes at least one pigment.

[0049] This configuration is highly advantageous. The advantageous properties of the colored coating, which are not too strong but sufficiently adhesive, can be set very simply by using the sol-gel hydrolysis products of organosilicon compounds or mixtures of organosilicon compounds. However, as has already been shown, such coatings are not suitable for forming separate layers on glass or glass-ceramic substrates for use as back or bottom coatings. This is because these layers are either fired too deeply, resulting in excessive porosity that prevents self-sealing (i.e., according to the invention, they exhibit very good oil resistance), or they are not fired but merely dried, thus lacking sufficient thermal stability. This is because it will burn under heat load when subsequently used with the equipped cooking utensils, thus reducing the coating's impermeability over time. Furthermore, unfired coatings do not have good adhesion and therefore lack sufficient scratch resistance.

[0050] However, it is now possible to provide coated glass or glass-ceramic sheets in a very simple way, with a coating that is scratch-resistant and sealing even when designed as a single layer.

[0051] According to one embodiment of the glass or glass-ceramic plate, its flexural strength, determined using the double-ring method according to EN 1288-5, is at least 140 MPa and preferably at most 250 MPa (determined as the arithmetic mean of at least two samples in total). This advantageously supports the mechanical stability of the glass or glass-ceramic plate. According to one embodiment, the 5th percentile of the flexural strength of the glass or glass-ceramic plate is at least 100 MPa, wherein preferably at least 18 samples should be used to determine the 5th percentile.

[0052] According to one embodiment, the glass or glass-ceramic plate has impact resistance determined in a drop ball test according to UL 858 to be at least 45 cm, preferably at least 60 cm, preferably at least 70 cm, preferably at least 80 cm, and particularly preferably at least 90 cm, as the arithmetic mean of the total number of samples from at least two samples, wherein the impact resistance is determined for a coating disposed on the bottom surface of the glass or glass-ceramic plate. Furthermore, according to one embodiment, the glass or glass-ceramic plate has an impact resistance of at least 35 cm, preferably at least 40 cm, and particularly preferably at least 45 cm or higher, determined in a drop ball test according to UL 858 at the 5th percentile. The coating is also disposed on the underside of the specimen for determining impact resistance, i.e., the upper side of the specimen or glass or glass-ceramic plate is subjected to impact (or ball drop in the test), and the coating, according to the embodiment, is disposed on the reverse side of the specimen / glass or glass-ceramic plate.

[0053] As mentioned above, the bottom surface of the glass or glass-ceramic plate is understood to refer to the side of the plate that is furthest from the operator / observer / user when the plate is being operated. For example, it is possible, and even preferred, to design a bottom surface with bumps, as this allows for adjustment of the plate's particularly high strength, especially its shock resistance. However, it is also possible to configure the plate to be smooth on both sides, as this makes it easier to integrate display elements under the plate as part of the operating elements of the device equipped with the plate.

[0054] According to another embodiment of the glass or glass-ceramic plate, the glass or glass-ceramic plate has a light transmittance of less than 0.08%, preferably less than 0.04%, and particularly preferably less than 0.02% in the area where the coating is disposed, as determined according to Part 1 of DIN 5036. The transmittance specification preferably pertains only to the area on the glass or glass-ceramic substrate where the coating according to the embodiment is disposed.

[0055] In other words, the coating is designed to be almost opaque or opaque.

[0056] This can be advantageously supported by a suitable ratio of pigment to binder in the coating. According to one embodiment of the glass or glass-ceramic plate, the weight ratio of pigment to binder in the coating is 0.8 to 1.3, preferably 1:1 to 1:2.5, and particularly preferably 1:1.3 to 1:2. In this way, good coverage of the coating is advantageously ensured. Furthermore, this method allows the glass or glass-ceramic plate to be designed to produce a coating with high strength while maintaining sufficient adhesive strength.

[0057] Whenever the term "pigment to binder" is mentioned in the context of this invention, it always refers to the total amount of pigments contained in the coating. Here, "pigment" should be understood to mean a colorant, particularly an inorganic colorant, preferably a ceramic, i.e., an inorganic-nonmetallic colorant containing particles. For example, to set a specific color and / or one of the other properties of the coating, it may be possible and necessary for the coating to contain multiple pigments, such as pigments with different colors or hues. In this case, the specification of the pigment-binder ratio refers to the total amount of pigments contained in the coating, i.e., the total pigment content.

[0058] According to another embodiment, the coating comprises functional pigments, wherein the functional pigments constitute a proportion of 50% to 100% by weight, preferably 70% to 100% by weight, and particularly preferably 88% to 98% by weight in the total pigments.

[0059] The coating's construction allows it to include at least one functional pigment, typically used to set a specific appearance ("metallic coating"). However, it has been shown that functional pigments can also perform other functions in the coating. This is because many functional pigments, such as so-called pearlescent pigments, are typically formed in flake form, which can further support the coating's advantageous properties, such as high abrasion resistance. Therefore, it can be advantageously specified that the functional pigment constitutes a proportion of not less than, and for example, at least 50% by weight, preferably at least 70% by weight, and particularly preferably at least 88% by weight.

[0060] Coatings can typically contain only one functional pigment as a colorant, or, in special cases, as an "effect pigment," such that the functional pigment can constitute 100% by weight of the total pigment content. However, a lower content, such as only 98% by weight, may be advantageous and preferred. This can be particularly advantageous when the effect pigment itself is not colored but is, for example, a pure "silver-white" pearlescent pigment. In this case, to achieve a sufficiently high coating gloss density, in other words, to design the coating to be "opaque," only a very high layer thickness can be achieved. Therefore, it may be advantageous to add at least one other pigment that colors by absorption and / or scattering, or, if necessary, several other pigments to increase the opacity of the coating. To obtain a particular color impression, especially a dark color, it is also advantageous if, in addition to the effect pigment, at least one other pigment, particularly an absorbing pigment or a white pigment, is included in the coating.

[0061] Of course, the coating may also not contain any functional pigments.

[0062] As described above, according to the embodiment, the coating is designed as a single layer, and as a single layer, it has been designed to be both scratch-resistant and sealing.

[0063] The formation of a single layer does not imply that only a single coating is permitted on the side of a glass or glass-ceramic plate, on which a coating is also disposed, according to the embodiment. Conversely, it is possible, and may be preferred, if one or more additional coatings are disposed on that side. However, these additional coatings are not decisive for the performance of the first coating, but can be applied, for example, as functional layers for operating electronic components, etc. The advantageous characteristics of the coating can be determined here in areas of the glass or glass-ceramic plate where only the coating itself is disposed, without any other coating disposed between the substrate and the coating, or on the coating itself.

[0064] Therefore, the inventors have pioneered a method for providing a coating suitable as a bottom or back coating even when it already has a single layer. As explained, this can be advantageously achieved by a special configuration of the coating composition containing two silicone precursors. The inventors here assume that the addition of silicone resin is responsible for ensuring sufficient sealing.

[0065] Therefore, according to one aspect, the present invention also relates to a method for manufacturing a glass or glass-ceramic plate according to an embodiment of the present invention, comprising the following steps:

[0066] - Provide glass or glass-ceramic substrates.

[0067] - A coating composition comprising pigments and a binder is provided, wherein the binder comprises two silicone precursors, one of which is a silicone resin and the other is a sol-gel hydrolysis product.

[0068] - The coating composition is applied to one side of a glass or glass-ceramic substrate to form a coating, preferably by a printing method.

[0069] - Bake the coating at a temperature of at least 200°C and at most 400°C for at least 10 minutes and at most 120 minutes, preferably at a temperature of at least 250°C and at most 330°C for at least 30 minutes and at most 90 minutes, especially at most 60 minutes, and particularly preferably at a temperature of at least 300°C and at most 320°C for at least 30 minutes and at most 60 minutes.

[0070] This method not only allows for the manufacture of glass or glass-ceramic plates according to the embodiments, but also offers the advantage of simplified processes. In particular, the method according to the invention significantly reduces the logistical work associated with this production process because a single layer is now applied, eliminating the need for different pastes in logistics. If the desired chromaticity coordinates of the coating are very light, it is no longer necessary to change the chromaticity coordinates from above, i.e., through the substrate; a darker but sealing layer can be applied over the lighter first coating. It is precisely in this combination that, if the first layer is not sufficiently opaque or translucent, the chromaticity coordinates of the first coating may change due to darker printing on the back side.

[0071] According to another aspect of the invention, the invention also relates to a glass or glass-ceramic plate which is manufactured or at least capable of being manufactured by a method according to one embodiment.

[0072] Example

[0073] The table below provides examples of the compositions of three coating compositions or pastes for glass or glass-ceramic plates obtained according to embodiments.

[0074] Color scheme 1 [wt%] 2 [wt%] 3 [wt%] silicone resin 53.72 48.15 48.15 Sol-gel hydrolysis products 1.96 4.76 4.76 solvent 10.64 12.93 12.93 Defoamer 0.52 0.52 0.52 White pigment 3.84 0.00 0.00 Pearlescent Pigment 1 (Interference Pigment) 2.88 3.08 0.00 graphite 0.48 0.87 0.87 Pearl pigment 2 (yellow / brown) 0.00 0.00 14.91 Pearl pigment 3 (silver white) 15.06 11.83 17.39 Pearl pigment 4 (silver white) 10.65 17.39 0.00 Filler material 0.24 0.46 0.46

[0075]

[0076] According to the table above, the composition of the example paste, in addition to fillers, includes several pearlescent pigments, as well as a white pigment and graphite as a dark-colored component as a solid component. The proportions of these components are variable and have been used here to achieve particularly preferred chromaticity coordinates. Therefore, other pigments or only one pigment may also be used. For example, TiO2 can be used as a white pigment. The general compositional range of coating compositions or pastes used to manufacture glass or glass-ceramic plates according to the embodiments is summarized below:

[0077] The composition range of the disclosed coating material compositions

[0078] Composition / Color System weight% silicone resin 40-60 Sol-gel hydrolysis products 0.5-10 solvent 5-20 Defoamer 0.1-1.5 White pigment 0-5 Pearl pigments 0-53.9 Other pigments (such as spinel) 0-25 graphite 0.5-5 Filler material 0-3

[0079] Regarding pigments, the totals for white pigments, pearlescent pigments, and other pigments (particularly including absorbing pigments such as spinel, i.e., oxidizing pigments particularly stable at high temperatures) are given separately. That is, a paste or coating composition may contain only one or more pearlescent pigments, in which case the total amount of all pearlescent pigments contained in the coating composition is at most 53.9% by weight. Correspondingly, the coating composition may contain one or more white pigments, wherein the total amount of all white pigments is within the aforementioned range; the same applies to other pigments.

[0080] In addition to pearlescent pigments, other functional pigments may be present. However, the total amount of pearlescent pigments and other functional pigments must not exceed 53.9% by weight. Other functional pigments may exist, for example, on Al2O3, SiO2, or borosilicate glass sheets with different coatings. Using such functional pigments, color appearance and other effects, such as shimmer or metallic effects, can be achieved.

[0081] Find examples of compositions for producing sol-gel hydrolysis products in the table below:

[0082] Preparation of sol-gel hydrolysis products

[0083] 104.16g Tetraethoxysilane 0.500 mol 178.3g Methyltriethoxysilane 1.000 mol 1.78g p-Toluenesulfonic acid 0.0093 mol 9.01g <![CDATA[H2O]]> 0.500 mol

[0084] First, silane is introduced, then p-toluenesulfonic acid is dissolved in water and added. After stirring for 1 hour, the resulting ethanol is distilled off.

[0085] Comparative example

[0086] Composition / Color System V4 [weight %] V5 [weight %] V6 [weight %] silicone resin 62.00 35.00 45.00 Sol-gel hydrolysis products 0.00 20.00 11.00 solvent 11.00 12.93 10.05 Defoamer 0.52 0.52 0.52 White pigment 3.81 0.00 0.00 Pearlescent Pigment 1 (Interference Pigment) 0.00 3.08 0.00 graphite 0.48 0.87 0.87 Pearl pigment 2 (yellow / brown) 0.00 0.00 14.71 Pearl pigment 3 (silver white) 11.30 11.83 17.39 Pearl pigment 4 (silver white) 10.65 15.31 0.00 Filler material 0.24 0.46 0.46

[0087] Attached Figure Description

[0088] The invention will now be explained in more detail with reference to the accompanying drawings. In the drawings:

[0089] Figure 1 Scanning electron micrographs of glass or glass-ceramic plates with coatings are shown.

[0090] Figure 2 Photographic views of glass or glass-ceramic plates are shown to illustrate oil resistance, and Figure 3 Photographs of glass or glass-ceramic plates are shown to illustrate scratch resistance. Detailed Implementation

[0091] Figure 1Figure a shows a scanning electron microscope image of a prior art glass or glass-ceramic plate 10, which includes a coating 2 constructed as a double layer. In the present case, the glass or glass-ceramic plate 10 is designed as a glass-ceramic plate, i.e., including a substrate 1 containing glass ceramic herein. It can be clearly seen that the coating 2 comprises two distinct layers (or partial layers) 22, 21, one layer 21 disposed as a colored layer facing the substrate 2, and the other layer 22 disposed on the first layer 21. A dividing line (or interface) 23 between the first layer 21 and the second layer 22 is schematically drawn on... Figure 1 From a. Figure 1 As can be seen from the scanning electron micrograph of a, the second sealing layer 22 has a different fine structure, such as matrix 221, which is finer than matrix 211 of layer 21.

[0092] In contrast, a glass or glass-ceramic plate 10 according to one embodiment of the invention, also designed here as a glass-ceramic plate, comprises a substrate 1 containing glass ceramic and a coating 2. The coating 2 is here designed as a double layer, such that a paste having the same composition is printed twice, resulting in a coating comprising two partial layers. As mentioned above, this coating 2 is referred to as a single layer within the scope of the invention because the two partial layers constituting it have the same composition. Due to the identical composition, the two partial layers with the same composition have very good adhesion to each other and can only adhere to each other in... Figure 1 They are very difficult to distinguish from each other in the scanning electron micrographs of b.

[0093] In contrast, there are two layers, such as Figure 1 As shown in the example in a, layers 21 and 22 have different compositions.

[0094] Figure 2 Photographs of 10 glass or glass-ceramic plates are shown to illustrate oil resistance. Figure 2 Figure b shows the back side of the coating 2 of different plates 10. Figure 2 Figure a shows the same plate 10, but the plate shown here has a substrate 1 facing upwards, i.e., towards the observer.

[0095] exist Figure 2 In sample b, the residue of colored oil on the back of the sample is still clearly visible (blue spots, shadows in the black and white photograph). Figure 2 In a, the order in which the samples are shown is the same as Figure 2The images in Figure a are identical, although there are significant differences in oil visibility: the sample on the left has a clearly discernible spot, which also implies a corresponding large change in chromaticity coordinates, while a spot in the middle sample is barely visible. In the sample on the far right, no spots are visible through the substrate, compared to the other two samples. This is also evidenced by the corresponding measurements of chromaticity coordinates in the comparison between treated and untreated samples, showing a chromaticity coordinate point difference ΔE of less than 2, and in this case, even only 0.22.

[0096] Figure 3 Two photographs are shown of specimens undergoing a scratch test, i.e., DIN-ISO 1518-1. For this purpose, a test probe with defined contact (defined by contact force) is pulled to one side of the coating, preferably in an area where only the coating is applied to the substrate.

[0097] Within the scope of this invention, it is understood through testing as follows:

[0098] - If the test probe trajectory is not visible when viewed from above, i.e., through the substrate, or

[0099] -If the coating does not peel off.

[0100] Preferably, the probe trail is not visible from above, i.e., through the substrate. This is especially important for coatings containing functional pigments. Because from... Figure 3 As can be seen from the test track in example a, the coating can exhibit a so-called "metallic effect" under these conditions, and coating damage can occur even before obvious peeling, which can be visually perceived through the substrate. The inventors suspect this may be due to the functional pigments being "crushed together," thus creating a difference in visual impression between the unloaded coating and the coating area with the test track through the substrate. However, in the case of the board according to the embodiment, this only occurs after a load of 7N or greater, unlike the boards of the prior art.

[0101] Therefore, the coating on the glass or glass-ceramic plate has a scratch resistance greater than 7N, preferably not greater than 30N, in the test according to DIN-ISO 1518-1, in the area where the coating is applied only on the glass or glass-ceramic substrate.

[0102] Preferably, the scratch resistance can also be greater than 16N, for example up to 17N or even 18N, especially when delamination is taken into account. Thus, according to one embodiment, the scratch resistance may be 16N or even higher, meaning that according to this embodiment, no delamination occurs under the load mentioned in the scratch test.

[0103] However, excessively high scratch resistance is associated with excellent layer adhesion, which is detrimental to coatings intended for application on the user-facing side of a board (bottom or back coating) as this can significantly reduce the board's mechanical resistance. Therefore, according to one embodiment, the maximum scratch resistance of the coating is specified to be 30 N.

[0104] In the context of this invention, the phrase "in the area of ​​the glass or glass-ceramic plate where only the coating is disposed on the glass or glass-ceramic substrate" is generally understood to refer to the side where the coating is disposed in this case. On the other side of the plate, for example, a further coating may be applied, such as a ceramic decoration for marking cooking areas. However, as will be apparent to those skilled in the art, what is important for the scratch and oil resistance of the coating is only the adhesion of the coating to the substrate or its inherent sealing properties, and of course, no further coating disposed on the opposite side of the plate, such as a top-side decoration.

[0105] List of reference numerals

[0106] 1 Glass or glass-ceramic substrate 10 Glass or glass-ceramic plate 2 coating 21、22 Partial layer of 2 23 The separator line / interface between 21 and 22 211 21 matrix and binding phase 221 22 matrix and binding phase

Claims

1. A method for manufacturing glass or glass-ceramic plates, the method comprising the following steps: - Provide glass or glass-ceramic substrates, - A coating composition comprising an inorganic pigment and a binder, the binder comprising two silicone precursors, one of which is a silicone resin and the other is a sol-gel hydrolysis product. - The coating composition is applied to one side of a glass or glass-ceramic substrate to form a coating. - Bake the coating at a temperature of at least 250°C and at most 400°C for at least 10 minutes and at most 120 minutes.

2. The method according to claim 1, wherein, The coating composition is applied to one side of a glass or glass-ceramic substrate by a printing method to form a coating.

3. The method according to claim 1, wherein, Bake the coating at at least 250°C and at most 330°C for at least 30 minutes and at most 90 minutes.

4. The method according to claim 1, wherein, Bake the coating at at least 250°C and at most 330°C for at least 30 minutes and at most 60 minutes.

5. The method according to claim 1, wherein, Bake the coating at at least 300°C and at most 320°C for at least 30 minutes and at most 60 minutes.

6. The method according to any one of claims 1 to 5, wherein, The weight ratio of the sol-gel hydrolysis product to the silicone resin in the coating composition is between 1:0.2 and 1:0.

02.

7. The method according to any one of claims 1 to 5, wherein, The weight ratio of the sol-gel hydrolysis product to the silicone resin in the coating composition is between 1:0.09 and 1:0.

035.

8. A glass or glass-ceramic plate manufactured by the method according to any one of claims 1 to 7, comprising a glass or glass-ceramic substrate and a coating disposed on at least one side of the glass or glass-ceramic substrate, the coating comprising an organosilicon matrix and an inorganic pigment, wherein the coating has a thickness of at least 10 μm and at most 80 μm, and wherein the coating has scratch resistance and oil resistance greater than 7N and at most 30N according to DIN-ISO 1518-1 in the region of the glass or glass-ceramic plate where the coating is disposed only on the glass or glass-ceramic substrate, wherein the chromaticity coordinate change ΔE determined through the glass or glass-ceramic substrate is less than 1, wherein the chromaticity coordinate change ΔE is within L a b The system is defined and given by the following formula: , in , , It refers to the chromaticity coordinates of a glass or glass-ceramic substrate before the colored oil is applied. , , It refers to the chromaticity coordinates of a glass or glass-ceramic plate after a colored oil has been applied to it.

9. The glass or glass-ceramic plate according to claim 8, wherein, The chromaticity coordinate change ΔE is less than 0.

5.

10. The glass or glass-ceramic plate according to claim 8, wherein, The chromaticity coordinate change ΔE is less than 0.

3.

11. The glass or glass-ceramic plate according to claim 8, wherein, The chromaticity coordinate change ΔE is less than 0.

2.

12. The glass or glass-ceramic plate according to claim 8, wherein, The chromaticity coordinate change ΔE is less than 0.

1.

13. The glass or glass-ceramic plate according to any one of claims 8 to 12, having a flexural strength of at least 140 MPa, determined in the double-ring method according to EN 1288-5, and determined as the arithmetic mean of the total number of samples of at least two samples.

14. The glass or glass-ceramic plate according to claim 13, wherein, The maximum bending strength is 250 MPa.

15. The glass or glass-ceramic plate according to any one of claims 8 to 12, having an impact resistance of at least 45 cm, determined in a drop ball test according to UL 858, and determined as the arithmetic mean of the total number of samples of at least two samples, wherein the impact resistance is determined for a coating disposed on the underside of the glass or glass-ceramic plate.

16. The glass or glass-ceramic plate according to claim 15, wherein, Impact resistance is at least 60cm.

17. The glass or glass-ceramic plate according to claim 15, wherein, Impact resistance is at least 70cm.

18. The glass or glass-ceramic plate according to claim 15, wherein, Impact resistance is at least 80cm.

19. The glass or glass-ceramic plate according to claim 15, wherein, Impact resistance is at least 90cm.

20. The glass or glass-ceramic plate according to any one of claims 8 to 12, wherein, The glass or glass-ceramic plate has a light transmittance of less than 0.08% in the area where the coating is applied, as determined according to DIN 5036 Part 1.

21. The glass or glass-ceramic plate according to claim 20, wherein, The glass or glass-ceramic plate has a light transmittance of less than 0.04% in the area where the coating is applied.

22. The glass or glass-ceramic plate according to claim 20, wherein, The glass or glass-ceramic plate has a light transmittance of less than 0.02% in the area where the coating is applied.

23. The glass or glass-ceramic plate according to any one of claims 8 to 12, wherein, The weight ratio of pigment to binder in the coating is from 1:0.8 to 1:

3.

24. The glass or glass-ceramic plate according to any one of claims 8 to 12, wherein, The weight ratio of pigment to binder in the coating is from 1:1 to 1:2.

5.

25. The glass or glass-ceramic plate according to any one of claims 8 to 12, wherein, The weight ratio of pigment to binder in the coating is from 1:1.3 to 1:

2.

26. The glass or glass-ceramic plate according to any one of claims 8 to 12, wherein, The coating comprises functional pigments, wherein the proportion of the functional pigments in the total pigment content is between 50% by weight and 100% by weight.

27. The glass or glass-ceramic plate according to claim 26, wherein, The functional pigment accounts for a proportion of 70% to 100% by weight in the total pigment content.

28. The glass or glass-ceramic plate according to claim 26, wherein, The functional pigment accounts for a proportion of 88% to 98% by weight in the total pigment content.

Citation Information

Patent Citations

  • Method for producing a sealing layer for decorative layers, glass or glass-ceramic articles and its use

    DE102008031426A1

  • Decorative coating of glass or glass-ceramic articles

    DE102008031428A1

  • Glass-ceramic and glass plates, heating plates, and preparation

    EP1730085B1

  • Hotplate device

    EP3222595A1

  • Cooking device top plate and manufacturing method for same

    EP3511631A1