Process for the selective hydrogenation of acetylenes
By introducing palladium and silver supported on an organic cage structure into the catalyst, the size and distribution of the active centers are controlled, solving the problem of green oil and coking in the selective hydrogenation catalyst of C2 fraction. This achieves high selectivity and activity, reduces the formation of by-products during hydrogenation, and extends the catalyst life.
Patent Information
- Application Number
- CN202210855861.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-19
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-07-19
AI Technical Summary
Existing selective hydrogenation catalysts for C2 fractions are prone to producing green oil and coking, leading to decreased catalyst activity and shortened lifespan, especially in reactions involving CO.
Catalysts using an organic cage structure to support palladium and silver, with palladium located within the organic cage and silver located in the middle or at the bottom of the palladium active center, reduce internal diffusion restriction and the occurrence of hydroformylation reaction by controlling the size and composition distribution of the active center.
It improves the selectivity and activity of the catalyst, reduces the amount of green oil generated and the coking rate, extends the catalyst life, reduces the generation of by-products, and lowers equipment investment and operating costs.
Smart Images

Figure BDA0003753304140000131 
Figure BDA0003753304140000141 
Figure BDA0003753304140000171
Abstract
Description
Technical Field
[0001] This invention relates to a selective hydrogenation method for alkynes in C2 fractions, and more particularly to a selective hydrogenation method for post-hydrogenation of C2 fractions involving CO. Background Technology
[0002] Ethylene, obtained through steam cracking of petroleum hydrocarbons such as ethane, naphtha, diesel, and hydrotreated tail oil, contains 0.2% to 2.5% acetylene by mass. During polymerization, the acetylene in ethylene reduces the activity of the polymerization catalyst and affects the physical properties of the polymer; therefore, it must be removed. Currently, selective hydrogenation is commonly used industrially to remove acetylene from ethylene, primarily employing noble metal catalysts such as Pd, Pt, and Au. To ensure that the ethylene produced by acetylene hydrogenation and the original ethylene in the feedstock do not undergo further hydrogenation to form ethane, thus preventing ethylene loss, a high hydrogenation selectivity of the catalyst is essential for achieving good economic benefits.
[0003] Post-hydrogenation of C2 catalysts involves calculating the required hydrogen based on the acetylene content and adding it to the hydrogenation feedstock. The molar ratio of hydrogen to acetylene is generally no more than 2. Due to the low hydrogen content, acetylene readily undergoes hydrogenation dimerization, producing a C4 fraction. This C4 fraction further polymerizes to form oligomers with a wider molecular weight range, commonly known as "green oil." This green oil adsorbs onto the catalyst surface and further forms coke, blocking the catalyst pores and preventing reactants from diffusing to the active sites, thus reducing catalyst activity.
[0004] Noble metal catalysts exhibit high activity, but they are prone to generating green oil during use, leading to coking and deactivation, which affects catalyst stability and lifespan. Patent CN200810119385.8 discloses a non-noble metal supported selective hydrogenation catalyst, its preparation method, and its application. The catalyst includes a support and a main active component and a co-active component supported on that support. The main active component is Ni, and the co-active component is selected from at least one of Mo, La, Ag, Bi, Cu, Nd, Cs, Ce, Zn, and Zr. Both the main active component and the co-active component exist in amorphous form with an average particle size <10 nm. The support is a non-oxidizing porous material. Furthermore, the catalyst is prepared using a microemulsion method.
[0005] US4404124 describes a selective hydrogenation catalyst with a shell distribution of active components prepared via a stepwise impregnation method. This catalyst can be applied to the selective hydrogenation of C2 fractions to eliminate acetylene from ethylene. US5587348 describes a high-performance C2 hydrogenation catalyst prepared using alumina as a support, with the addition of silver and palladium co-catalysts, and the addition of fluorine chemically bonded to alkali metals. This catalyst exhibits characteristics such as reduced green oil formation, improved ethylene selectivity, and reduced formation of oxygen-containing compounds.
[0006] Patent CN1736589 reports a Pd / γ-Al2O3 selective hydrogenation catalyst prepared by a complete adsorption impregnation method, but the catalyst generates a large amount of green oil during use. Patent CN200810114744.0 discloses an unsaturated hydrocarbon selective hydrogenation catalyst and its preparation method. This catalyst uses alumina as a support and palladium as the active component. The addition of rare earth and alkaline earth metals and fluorine improves the catalyst's resistance to impurities and coking, but its selectivity is not ideal.
[0007] The catalysts prepared by the above methods all use catalysts with a single pore size distribution. In fixed-bed reactions, the selectivity of the catalyst is poor due to the influence of internal diffusion. Supports with a bimodal pore distribution can improve catalyst selectivity while ensuring high activity, as the presence of large pores can reduce the influence of internal diffusion. ZL971187339 discloses a hydrogenation catalyst with a honeycomb support, which is a large-pore support and effectively improves the catalyst selectivity. CN1129606A discloses a hydrocarbon conversion catalyst, whose support catalyst includes alumina, nickel oxide, iron oxide, etc. This catalyst includes two types of pores: one to improve the catalytic reaction surface and the other to facilitate diffusion. Patent CN101433842A discloses a hydrogenation catalyst with a bimodal pore distribution. The most probable radius of the small pores is 2–50 nm, and the most probable radius of the large pores is 100–500 nm. Due to the bimodal pore distribution, the catalyst has both good hydrogenation activity and good selectivity, resulting in a large increase in ethylene production.
[0008] In the C2 hydrogenation reaction, the formation of green oil and coking of the catalyst are important factors affecting catalyst lifespan. The catalyst's activity, selectivity, and lifespan constitute its overall performance. While the methods listed above offer good pathways to improve catalyst activity and selectivity, they do not solve the problem of catalyst coking, or they address the issues of green oil formation and coking but not selectivity. Although macroporous supports can improve selectivity, the larger molecules generated by polymerization and chain growth reactions can easily accumulate in the macropores of the support, causing catalyst coking and deactivation, thus affecting catalyst lifespan.
[0009] CN201910988247.1 discloses a selective hydrogenation method for C2 fractions. This method uses a catalyst support with a bimodal pore distribution. During catalyst preparation, active components are loaded via two methods: solution and microemulsion. In the solution method, a portion of Pd is loaded into the micropores as the main active component for the reaction. Additionally, a W / O type microemulsion with a particle size larger than the support pores is prepared. This microemulsion contains nickel and copper salts, distributing these components in the macropores of the support, forming Ni-Cu active centers. The catalyst prepared using this method allows the selective hydrogenation reaction to primarily occur in the micropores. The green oil generated during the reaction enters the macropores and undergoes saturated hydrogenation at the Ni-Cu active centers, reducing catalyst coking. While this method reduces the catalyst coking rate, it does not solve the problem of green oil formation, especially when CO is involved in the reaction. Due to the hydroformylation reaction, oxygen-containing compounds are generated, which have a stronger adsorption capacity on the catalyst, making them more prone to coking and causing catalyst deactivation.
[0010] In the selective hydrogenation of C2, when Pd is the main active component, in the traditional impregnation process for catalyst preparation, Pd is used as the active component. 2+ Or [PdCl4] 2- Pd is ionicly bound to the support, and during activation, it aggregates to become active sites. Since the aggregation of Pd during activation is a kinetically governed stochastic process, the size of each active site is difficult to control beforehand.
[0011] Previous studies have found that the selective hydrogenation process of acetylene involves the following steps: first, an acetylene molecule combines with one hydrogen atom to form a vinyl group; the vinyl group then combines with another hydrogen atom to form ethylene; or two vinyl groups couple to form butadiene. Since butadiene can undergo a series of polymerization reactions to form green oil and then coke, inhibiting butadiene formation becomes crucial to preventing coking of C2 selective hydrogenation catalysts.
[0012] Clearly, if two vinyl groups form simultaneously on a single catalyst active site, the probability of butadiene formation increases significantly. Studies have also found that larger active site sizes lead to higher butadiene yields. To prevent large active site sizes, there are generally two approaches: reducing the amount of active component and expanding the dispersion region of the active component. However, reducing the loading of the active component may result in insufficient active sites, leading to inadequate hydrogenation activity, incomplete acetylene removal, and substandard hydrogenated products. Expanding the active component loading region means that some active sites are not located near the catalyst surface, resulting in poor catalyst selectivity and significant ethylene loss during hydrogenation.
[0013] To reduce the formation of green oil during C2 hydrogenation, the key is to prevent the simultaneous formation of two or more vinyl groups on a single active site. To this end, much research has been conducted on noble metal single-atom catalysts for hydrogenation reactions. However, currently, there is still a considerable gap between this research and practical applications. This is because the active site for hydrogenation requires two processes: first, the activation of the alkyne molecule, where the electron pair of the alkyne double bond enters the empty orbitals of the active site atom, and the active site atom feeds the electron pair back to the antibonding orbitals of the alkyne molecule, causing the double bond energy to decrease, thus activating and breaking the double bond; simultaneously, the hydrogen molecule also requires the same process to be activated into hydrogen atoms. For single-atom active sites, due to the limited physical size of a single atom, completing both processes simultaneously is challenging, resulting in a slow reaction process that is difficult to meet the requirements of practical applications. Therefore, it is natural that active neutrals need to have a certain physical size. In fact, for palladium catalysts, since their stacked structure can absorb a large amount of hydrogen, the activation of hydrogen and the transfer of hydrogen atoms are completed within the palladium stacked structure. Therefore, their activity is higher than that of active components that can only adsorb hydrogen on the surface.
[0014] To prepare catalysts with narrow particle size distributions, researchers have recently synthesized a series of three-dimensional organic cages. These organic cages, with fixed sizes, can be used to immobilize metals, thereby preparing catalysts with highly dispersed metal clusters. Qiang Song et al. synthesized three-dimensional organic cages, reporting in "Three-dimensional hydrophobic porous organic polymers confined Pd nanoclusters for phase-transfer catalytic hydrogenation of nitroarenes in water," that an organic cage with a size of 1.4-1.8 nm was synthesized using two organic monomers, tris(4-formylphenyl)amine and phenylenediamine. After loading active palladium into these organic cages, hydrogenation of nitrobenzene can be achieved in the liquid phase. Currently, these three-dimensional organic cages, after loading the active component, are either in solution or uniformly distributed on a support, thus limiting their application to hydrogenation without considering selectivity or homogeneous hydrogenation. For selective hydrogenation, not only does the size of the active center affect the reaction, but the distribution of the active component in the catalyst also has a significant impact on the reaction results. Therefore, catalysts with uniformly distributed active components prepared by organic cages are not suitable for selective hydrogenation reactions, especially for selective hydrogenation reactions in the gas phase such as acetylene.
[0015] If the hydrogenation feedstock contains CO, a hydroformylation reaction will occur during the hydrogenation process, generating aldehydes, ketones, acids, etc. These fractions are more easily adsorbed on the alumina support, accelerating the coking process of the green oil. Since the hydroformylation reaction involves hydrogen, CO, and olefins, these three molecules need to be simultaneously adsorbed at the catalyst's active site, especially CO and olefins, for the hydroformylation reaction to occur. Therefore, preventing the simultaneous adsorption of these two components is crucial for effectively reducing the coking rate of C2 hydrogenation catalysts involving CO. Summary of the Invention
[0016] The main objective of this invention is to provide a selective hydrogenation method for alkynes to overcome the defects of existing selective hydrogenation methods, such as low catalyst activity, poor selectivity, and easy coking.
[0017] This invention provides a selective hydrogenation method for alkynes, wherein the hydrogenation feedstock is a C2 fraction. The C2 fraction enters a reactor for gas-phase hydrogenation to remove acetylene. The process conditions for this gas-phase hydrogenation are: reactor inlet temperature 45–120°C, pressure 1.5–3.0 MPa, and gas hourly space velocity 1000–6000 h⁻¹. -1 The hydrogen required for this gas-phase hydrogenation comes from crude hydrogen, which contains 0.1-1% CO by volume and 20-95% hydrogen by volume. The catalyst used for this gas-phase hydrogenation has an alumina support or is mainly alumina, and the active components are Pd and Ag. Based on the mass of the support (100%), the mass content of Pd is 0.045-0.075%, and the mass content of Ag is 0.06-0.12%. Palladium is located in an organic cage on the outer surface of the catalyst, and the size of the organic cage is 2.7-3.6 nm. Silver is located in the middle or bottom of the palladium active center.
[0018] The selective hydrogenation method for alkynes of the present invention is wherein the reactor is an adiabatic reactor or an isothermal reactor; the reactor is a single-stage reactor or a two-stage reactor.
[0019] In the selective hydrogenation method for alkynes of the present invention, when the reactor is a fixed-bed single-stage reactor, the hydrogen / alkyne molar ratio at the reactor inlet is 1.3 to 2.0;
[0020] Alternatively, the reactor may be a fixed-bed two-stage reactor, with the hydrogen / acetylene molar ratio at the inlet of the first-stage reactor being 1.1 to 1.3 and the hydrogen / acetylene molar ratio at the inlet of the second-stage reactor being 1.4 to 2.0.
[0021] In the selective hydrogenation method for alkynes of the present invention, the ethylene volume content in the C2 fraction is 60-90%, and the acetylene volume content is 0.1-1.5%.
[0022] The selective hydrogenation method for alkynes according to the present invention, wherein the catalyst has a specific surface area of 15-30 m².2 / g.
[0023] The selective hydrogenation method for alkynes according to the present invention, wherein the catalyst is prepared by means of:
[0024] (1) A hydrophilic polymerizable monomer is mixed with a calcined support and polymerized at a certain temperature to obtain a semi-finished catalyst A, wherein the volume of the polymer synthesized from the hydrophilic polymerizable monomer is 80-95% (preferably 85-95%) of the pore volume of the support.
[0025] (2) Mix tris(4-formylphenyl)amine with haloacetic acid, dissolve in haloalkane, then mix with semi-finished catalyst A, stir and add dropwise a mixed solution of aromatic diamine compound and haloalkane, let the mixture stand, and after the reaction is complete, pour off the residual liquid, wash with alcohol and deionized water respectively, and dry to obtain semi-finished catalyst B.
[0026] The molar ratio of aromatic diamine compounds to tris(4-formylphenyl)amine is 1.2-2.5:1, and the mass ratio of tris(4-formylphenyl)amine to haloacetic acid is 2000-6000:1.
[0027] (3) Dissolve the organic palladium compound in an organic solvent to obtain the first solution of the palladium precursor;
[0028] The semi-finished catalyst B is immersed in an alcohol solution. The first solution of palladium precursor is added dropwise to the mixture of semi-finished catalyst B and alcohol while stirring. Then, a reducing agent is added dropwise, and the mixture is heated and stirred. When the surface of semi-finished catalyst B no longer changes color, the solution is poured off, washed with deionized water, dried, and calcined at a temperature at which the polymer formed in step (1) can be decomposed to obtain semi-finished catalyst C.
[0029] (4) Dissolve soluble silver salt in deionized water or organic solvent to obtain silver impregnation solution. The total amount of silver impregnation solution is equivalent to the pore volume of the carrier. Immerse the semi-finished catalyst C in the silver impregnation solution. After complete absorption, let stand, add reducing agent dropwise to reduce silver, pour off the solution, wash with deionized water, and dry to obtain semi-finished catalyst D.
[0030] (5) Dissolve the organopalladium compound in an organic solvent. After the organopalladium is completely dissolved, a second solution of palladium precursor is obtained. Immerse the semi-finished catalyst D in an alcohol solution. Add the second solution of palladium precursor dropwise to the mixture of semi-finished catalyst D and alcohol while stirring.
[0031] Add the reducing agent dropwise to the above solution, heat and stir. When the surface of the semi-finished catalyst D no longer changes color, pour off the solution, wash and dry to obtain the catalyst. Alternatively, without reduction, pour off the solution, wash with deionized water, dry, and calcine to obtain the catalyst.
[0032] Preferably, in steps (3) and (5), the total mass ratio of palladium to tris(4-formylphenyl)amine is 2-14:1.
[0033] The selective hydrogenation method for alkynes according to the present invention includes a hydrophilic polymerizable monomer comprising a carbonyl group, a carboxyl group, or a carbon-carbon double bond; the hydrophilic polymerizable monomer can undergo polymerization or condensation reaction at temperatures below 420°C; and the hydrophilic polymerizable monomer can decompose at temperatures below 450°C after polymerization.
[0034] The selective hydrogenation method for alkynes of the present invention comprises the following: the tetraphenyldiamine compound is tetraphenyldiamine or tetraphenyldiamine with a substituent on the benzene ring, preferably p-tetraphenyldiamine or p-tetraphenyldiamine with a substituent on the benzene ring, wherein the substituent is an alkyl group or a halogen; the organopalladium compound is palladium acetate or palladium acetylacetonate; the silver-containing compound is a soluble silver salt; and the reducing agent is methanol, formaldehyde, formic acid, ethanol, acetaldehyde, or hydrazine hydrate.
[0035] The selective hydrogenation method for alkynes of the present invention, wherein the mass ratio of palladium contained in the partial organopalladium compound and the remaining organopalladium compound is 0-1:0.36-2.12.
[0036] The beneficial effects of this invention are:
[0037] 1. This invention synthesizes an organic cage structure of a specific size on a carrier, allowing the active component palladium to be loaded within the organic cage. Limited by the physical size of the organic cage, the maximum size of the active center (cluster) composed of palladium is equal to the size of the cage. This size satisfies the requirements for acetylene selectivity and activity, while significantly reducing the probability of forming two vinyl groups simultaneously in one active center.
[0038] 2. Furthermore, in the preparation of the catalyst of the present invention, an organic polymer is first synthesized to seal the inner pores of the support, and an organic cage is synthesized on the outer pores of the support. Therefore, the active component palladium is supported on the outer surface of the catalyst. Then, the organic polymer is calcined off to obtain the catalyst of the present invention. The gas-phase hydrogenation reaction is an internally diffusion-limited reaction. The organic cage structure is located on the outer surface of the catalyst, which avoids the influence of internal diffusion limitation on the catalytic reaction, resulting in good selectivity of the catalyst.
[0039] 3. Furthermore, in this invention, the active component silver is loaded in the middle or bottom of the palladium active center, which reduces the adsorption intensity of olefins on the catalyst surface, reduces the probability of a palladium active center simultaneously adsorbing CO and olefins, greatly reduces the yield of green oil, and greatly reduces the coking rate of the catalyst.
[0040] 4. When using the catalyst of this invention for the selective hydrogenation of alkynes, the amount of byproducts is significantly reduced, thus the catalyst may not even require regeneration. Furthermore, even if regeneration is necessary, it can be performed at temperatures below 450°C without damaging the organic cage structure, thereby significantly extending the catalyst's lifespan.
[0041] 5. Due to the improved selectivity and reduced green oil formation of the hydrogenation method of this invention, when the acetylene content at the reactor inlet exceeds 1.5% (V / V), a single-stage hydrogenation process can completely remove the acetylene. In conventional C2 fraction hydrogenation processes, a three-stage hydrogenation process is required when the acetylene content exceeds 1.4% (V / V). Therefore, the hydrogenation method of this invention can effectively reduce the number of reactors, thereby reducing equipment investment and operating costs. Detailed Implementation
[0042] The following provides a detailed description of the embodiments of the present invention. These embodiments are implemented based on the technical solution of the present invention and provide detailed implementation methods and processes. However, the scope of protection of the present invention is not limited to the following embodiments. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions.
[0043] This invention discloses a selective hydrogenation method for alkynes, wherein the hydrogenation feedstock is a C2 fraction. The C2 fraction enters a reactor for gas-phase hydrogenation to remove acetylene. The process conditions for this gas-phase hydrogenation are: reactor inlet temperature 45–120°C, pressure 1.5–3.0 MPa, and gas hourly space velocity 1000–6000 h⁻¹. -1 The hydrogen required for this gas-phase hydrogenation comes from crude hydrogen, which contains 0.1-1% CO by volume and 20-95% hydrogen by volume. The catalyst used for this gas-phase hydrogenation has an alumina support or is mainly alumina, and the active components contain at least Pd and Ag. Based on 100% of the support mass, the mass content of Pd is 0.045-0.075%, the mass content of Ag is 0.06-0.12%, palladium is located in an organic cage on the outer surface of the catalyst, and the size of the organic cage is 2.7-3.6 nm. Silver is located in the middle or bottom of the palladium active center.
[0044] The selective hydrogenation method for alkynes of this invention is mainly applicable to the selective hydrogenation of C2 fractions, that is, the selective hydrogenation of alkynes in the C2 fraction to produce olefins. In one embodiment, the C2 fraction contains 60-90% (v / v) ethylene and 0.1-1.5% (v / v) acetylene, with the above contents calculated based on 100% of the total volume of the C2 fraction. This invention does not particularly limit the source of the C2 fraction, for example, it can be from the top of a pre-deethaner column.
[0045] The present invention does not impose any particular limitation on the reactor, such as an adiabatic reactor or an isothermal reactor. In one embodiment, the reactor of the present invention can be a single-stage hydrogenation reactor or a two-stage hydrogenation reactor. In yet another embodiment, the reactor of the present invention is a fixed-bed reactor.
[0046] The process conditions for gas-phase hydrogenation in this invention are: reactor inlet temperature 45–120°C, operating pressure 1.5–3.0 MPa, and gas hourly space velocity 1000–6000 h⁻¹. -1 In one embodiment, the reactor inlet temperature is 50–120°C, the operating pressure is 1.5–3.0 MPa, and the gas hourly space velocity is 1000–6000 h⁻¹. -1 .
[0047] In one embodiment, the reactor of the present invention is a fixed-bed single-stage reactor, and the hydrogen / acetylene molar ratio (i.e., the molar ratio of hydrogen to alkynes in the hydrogenation feedstock) at the reactor inlet is 1.3 to 2.0. In another embodiment, the reactor of the present invention is a fixed-bed two-stage reactor, and the hydrogen / acetylene molar ratio at the inlet of the first-stage reactor is 1.1 to 1.3, and the hydrogen / acetylene molar ratio at the inlet of the second-stage reactor is 1.4 to 2.0.
[0048] The catalyst used in the gas-phase hydrogenation of this invention has the following characteristics: the support is alumina or mainly alumina catalyst; the active components contain at least Pd and Ag; based on 100% of the support mass, the Pd content is 0.045–0.075%, and the Ag content is 0.06–0.012%; palladium is located within an organic cage on the outer surface of the catalyst, and the size of the organic cage is 2.7–3.6 nm; silver is located in the middle or at the bottom of the palladium active center. "Silver in the middle or at the bottom of the palladium active center" means that silver can be at the bottom or center of the palladium active center, i.e., covered or surrounded by palladium atoms. The size of the organic cage in this invention is determined by the PET method.
[0049] In this invention, an organic cage is formed on the catalyst support, with the active component palladium located within the organic cage. The size of the organic cage effectively limits the size of the palladium active center clusters formed. This specific size satisfies the requirements for selective hydrogenation of acetylene and reduces the probability of a single palladium active center simultaneously adsorbing two vinyl groups, thereby reducing side reactions, decreasing the catalyst coking rate, and extending the catalyst's lifespan. Furthermore, the organic cage is formed on the outer surface of the catalyst, avoiding the influence of internal diffusion limitations on the catalytic reaction, resulting in excellent catalyst selectivity.
[0050] The hydrogen required for gas-phase hydrogenation in this invention can be derived from crude hydrogen, which typically contains CO. In one embodiment, the CO content in the crude hydrogen is 0.1-1% (v / v), and the hydrogen content is 20-95% (v / v). Due to the presence of CO, a hydroformylation reaction will occur during the hydrogenation process, generating aldehydes, ketones, acids, etc. These substances are more easily adsorbed on the alumina support, accelerating the coking process of the green oil. Since the hydroformylation reaction involves hydrogen, CO, and olefins, these three molecules need to be simultaneously adsorbed at the catalyst active site, especially CO and olefins, for the hydroformylation reaction to occur. The catalyst of this invention introduces the active component silver, which reduces the adsorption strength of olefins on the catalyst surface, reduces the probability of a palladium active site simultaneously adsorbing CO and olefins, greatly reduces the yield of green oil, and thus greatly reduces the coking rate of the catalyst.
[0051] Furthermore, the adsorption principle of CO on palladium atoms is as follows: the lone pair electrons in the CO molecule enter the empty orbitals in the outer shell of the palladium atom, and CO is adsorbed onto the palladium atom by chemical adsorption. This adsorption occurs in various ways; strong adsorption involves one CO molecule binding to multiple palladium atoms, making desorption difficult. When silver is covered or surrounded by palladium atoms, its outer electrons can more easily enter the empty orbitals of palladium. The partial occupation of these empty orbitals prevents the lone pair electrons of CO from entering, reducing the probability of strong adsorption between CO molecules and multiple palladium atoms, and thus reducing the probability of CO undergoing a formylation reaction. Therefore, in this invention, the active component silver is located in the middle or at the bottom of the palladium active center, which can reduce the probability of CO undergoing a formylation reaction.
[0052] The present invention does not specifically limit the raw materials and formation method of the organic cage on the catalyst support, but the size of the organic cage to be formed should be between 2.7 and 3.6 nm.
[0053] The catalyst support of this invention is alumina or mainly alumina, and the Al2O3 crystal form is preferably θ, α, or a mixture thereof. The alumina content in the catalyst support is preferably above 80% (wt), and the support may also contain other metal oxides such as magnesium oxide, titanium oxide, etc. This invention does not particularly limit the shape of the catalyst support; for example, it can be spherical, cylindrical, clover-shaped, four-leaf clover-shaped, etc. In one embodiment, the support used in step 1 is a calcined support.
[0054] This invention does not specifically limit the type of hydrophilic polymerizable monomer in step 1. The hydrophilic polymerizable monomer of this invention only needs to be capable of polymerization or condensation reactions below 420°C, and decompose after polymerization below 450°C. In one embodiment, the hydrophilic polymerizable monomer in step 1 contains a carbonyl group, a carboxyl group, or a carbon-carbon double bond, and the hydrophilic polymerizable monomer can, for example, undergo polymerization or condensation reactions. In another embodiment, the volume of the hydrophilic polymerizable monomer after polymerization is 80-95% of the pore volume of the carrier.
[0055] In step 1, the "certain temperature" refers to the temperature at which the hydrophilic polymerizable monomer undergoes a condensation or polymerization reaction, which varies depending on the monomer. Since the polymerizable monomer of this invention is a polar monomer, and the alumina support has the characteristic of adsorbing polar monomers, the polymerizable monomer of this invention will be adsorbed into the pores of the alumina support, and the resulting polymer will also be formed within the pores.
[0056] The polymerization temperature in step 1 is 80-200℃, and the polymerization time is not particularly limited in this invention.
[0057] In step 2, tris(4-formylphenyl)amine and tetraphenyldiamine compounds are mixed with semi-finished catalyst A, wherein the tris(4-formylphenyl)amine and tetraphenyldiamine compounds react to form an organic cage which is supported on the outer pores of the support. In one embodiment, the reaction between tris(4-formylphenyl)amine and tetraphenyldiamine compounds is carried out under the catalysis of haloacetic acid, and the molar ratio of tetraphenyldiamine compounds to tris(4-formylphenyl)amine is 1.2 to 2.5:1. The tetraphenyldiamine compounds are preferably p-tetraphenyldiamines.
[0058] In this invention, the formyl group on the benzene ring can undergo a condensation reaction with the amino group of an aromatic hydrocarbon to form an imine group. Since the monomer is tris(4-formylphenyl)amine, the three formyl groups on the benzene ring can react with three aromatic diamine molecules. The other end of the aromatic diamine molecule can then react with tris(4-formylphenyl)amine. Since tris(4-formylphenyl)amine has three active groups, it can form a cross-linked structure. The imine group is a non-linear molecule, which ultimately forms a large organic molecule with a network (cross-linked) and a cage-like spatial structure.
[0059] In steps (3) and (5), the organic palladium compound is palladium acetate or palladium acetylacetonate.
[0060] The reducing agent is a reducing compound, such as methanol, formaldehyde, formic acid, ethanol, acetaldehyde, hydrazine hydrate, etc. The alcohol is either ethanol or methanol, preferably ethanol.
[0061] In step (4), the silver-containing compound is a soluble silver salt, that is, a silver salt that can be dissolved in water or an organic solvent, such as silver nitrate that can be dissolved in water, silver acetylacetonate that can be dissolved in an organic solvent, etc., preferably silver nitrate that can be dissolved in water. The solvent that does not dissolve the silver-containing compound is, for example, ethanol, and the reducing agent is a reducing compound, such as methanol, formaldehyde, formic acid, ethanol, acetaldehyde, hydrazine hydrate, etc.
[0062] The mass ratio of palladium in the pre-loaded organopalladium compound to the remaining organopalladium compound is 0–1:0.36–2.12. The pre-loaded and remaining organopalladium compounds represent the total palladium supported on the catalyst carrier. In the catalyst preparation process of this invention, the mass ratio of the total organopalladium compound (based on palladium) to tris(4-formylphenyl)amine is 2–14:1. The reducing agent is a reducing compound, such as methanol, formaldehyde, formic acid, ethanol, acetaldehyde, hydrazine hydrate, etc. The alcohol is ethanol or methanol, preferably ethanol.
[0063] In the catalyst obtained by the present invention, after palladium is loaded twice and silver is loaded once, the mass content of Pd is 0.045-0.075% and the mass content of Ag is 0.06-0.12% based on the mass of the support (100%).
[0064] Therefore, this invention provides a selective hydrogenation method for alkynes, using a catalyst with high selectivity and catalytic activity for acetylene hydrogenation, and the catalyst is not prone to coking and has a long service life. When the hydrogen source is crude hydrogen, the catalyst of this invention, due to the presence of silver and the specific loading sites of silver, results in a lower C4 yield in the acetylene hydrogenation process, especially a lower yield of oxygen-containing byproducts, i.e., a lower amount of byproducts generated.
[0065] Furthermore, since the byproducts are significantly reduced when the catalyst of this invention is used for the selective hydrogenation of acetylene, the catalyst of this invention may not even require regeneration. Even when the catalyst of this invention requires regeneration, it can be regenerated at a temperature below 450°C without damaging the organic cage structure, thus ensuring the catalytic performance of the catalyst and significantly extending its lifespan.
[0066] The technical solution of the present invention will be further described in detail below through specific embodiments.
[0067] The catalyst of this invention was prepared using the following characterization method: a BET analyzer (McClone Systems, Inc., USA) was used to measure the specific surface area and pore size distribution.
[0068] The A240FS atomic absorption spectrometer was used to determine the contents of Pd and Ag in the catalyst.
[0069] The Agilent 7890A gas chromatograph measures the hydrogen, acetylene, and butene content at the reactor outlet and inlet.
[0070] The catalyst weight was measured using a 0.1 mg electronic balance.
[0071] Raw materials: Tris(4-formylphenyl)amine, dichloroacetic acid, dichloroethane, benzidine, hydrazine hydrate, ethanol, methanol, acetic acid, formic acid, formaldehyde, lactic acid, glacial acetic acid, acrylic acid, palladium acetate, palladium acetylacetone, silver nitrate, analytical grade, Shanghai Sinopharm Group Co., Ltd.
[0072] Alumina, Shandong Aluminum Group Corporation.
[0073] Example 1
[0074] Catalyst support: Commercially available spherical alumina-titanium oxide support with a titanium oxide content of 15 wt% and a diameter of 3 mm was used. After calcination at 1100℃ for 4 hours, the pore volume was 0.55 μm. 3 / g, with a specific surface area of 25.71m². 2 / g. Weigh 100g of the carrier.
[0075] Catalyst preparation:
[0076] (1) Weigh 58.44g of lactic acid and mix it with 100g of calcined support. Keep the temperature at 180℃ for 8 hours to obtain semi-finished catalyst A.
[0077] (2) Weigh 18.33 mg of tris(4-formylphenyl)amine and 0.0031 mg of dichloroacetic acid, mix them, dissolve them in 50 ml of dichloroethane, and then mix them with semi-finished catalyst A. Stir and add a mixed solution of 46.75 mg of p-tetraphenyldiamine and 10 ml of dichloroethane. Let the mixture stand at room temperature for 200 hours, pour off the residue, wash it with ethanol and deionized water respectively, and dry it to obtain semi-finished catalyst B.
[0078] (3) Dissolve 76 mg of palladium acetate in 60 mL of glacial acetic acid. After the palladium acetate is completely dissolved, a palladium acetate solution is obtained. Immerse the semi-finished catalyst B in 50 mL of ethanol solution. Add the prepared palladium acetate solution dropwise to the mixture of semi-finished catalyst B and ethanol, while stirring for 5 hours. Then add 20 mL of formaldehyde solution dropwise to the above solution, stir at 70 °C for 1 hour, decant the solution, wash with deionized water, dry at 120 °C, and calcine at 240 °C for 8 hours to obtain semi-finished catalyst C.
[0079] (4) Weigh 94.5 mg of silver nitrate and dissolve it in 55 g of deionized water. Immerse the semi-finished catalyst C in the prepared solution. After the solution is completely absorbed, let it stand for 4 hours. Then add 5 ml of 5 wt% hydrazine hydrate solution to the above solution. Stir at 40 °C for 1 hour. Pour off the solution, wash with deionized water, and dry at 120 °C to obtain the semi-finished catalyst D.
[0080] (5) Dissolve 40 mg of palladium acetate in 50 mL of glacial acetic acid until the palladium acetate is completely dissolved to obtain a palladium acetate solution. Immerse the semi-finished catalyst D in 50 mL of ethanol solution. Add the prepared palladium acetate solution dropwise to the mixture of semi-finished catalyst D and ethanol, while stirring for 30 hours. Then add 20 mL of formaldehyde solution dropwise to the above solution, stir at 70 °C for 1 hour, decant the solution, wash with deionized water, dry at 120 °C, and calcine at 550 °C to obtain the desired catalyst.
[0081] The first load was 65.5% Pd, and the second load was 34.5% Pd.
[0082] The prepared catalyst was determined by atomic absorption spectrometry, and the Pd content in the catalyst of Example 1 was found to be 0.055% and the Ag content was 0.06%.
[0083] Comparative Example 1
[0084] Catalyst support: The support prepared in Example 1 was used.
[0085] Catalyst preparation:
[0086] Compared with Example 1, the obtained catalyst has the same content of active component. The catalyst was prepared using a conventional method, the specific method of which is as follows:
[0087] (1) Weigh 91.67 mg of palladium chloride, dissolve it in hydrochloric acid, dilute the solution to 55 g, adjust the pH to 2.3, mix it with 100 g of calcined support, stir until the solution is completely absorbed, dry at 120 °C, and calcine at 500 °C to obtain semi-finished catalyst A1.
[0088] (2) Dissolve 94.5 mg of silver nitrate in 55 g of deionized water, immerse the semi-finished catalyst A1 in the prepared silver nitrate solution, and after the solution is completely absorbed, let it stand for 4 hours, dry at 120°C, and calcine at 550°C to obtain the desired catalyst.
[0089] The prepared catalyst was determined by atomic absorption spectrometry, and the catalyst in Comparative Example 1 had a Pd content of 0.055% and an Ag content of 0.06%.
[0090] Implementation effect
[0091] Operating Condition 1
[0092] Process conditions: material space velocity 1000 / h, operating pressure 2.0MPa, reactor inlet temperature 120℃, hydrogen / acetylene molar ratio 1.3, catalyst loading 100mL.
[0093] Catalyst reduction: 150℃, hydrogen reduction for 4 hours.
[0094] Composition of hydrogenated feedstock:
[0095] Acetylene 0.1% (v / v), Ethylene 90% (v / v), C3 0.5% (v / v)
[0096] The crude hydrogen contains 20% hydrogen (v / v) and 1% CO (v / v), while the hydrogenated feedstock contains 65 ppm CO.
[0097] Table 1. Evaluation results of the catalysts of Example 1 and Comparative Example 1 under operating condition 1.
[0098]
[0099] As shown in Table 1, from the start of the reaction to 1500 hours, the acetylene content at the reactor outlet in Example 1 was within acceptable limits; however, the acetylene content at the reactor outlet in Comparative Example 1 was not within acceptable limits. From the start of the reaction to 1500 hours, the amounts of C4 and oxygen-containing byproducts generated in Comparative Example 1 and Example 1 were very similar, with Example 1 even showing slightly higher amounts. However, the acetylene content at the reactor outlet in Comparative Example 1 was unacceptable because Ag in Comparative Example 1 was located on the outer surface of the active center, preventing the adsorption of acetylene and CO on the catalyst surface. While this objectively reduced the amount of C4 and oxygen-containing byproducts generated, it also significantly reduced the acetylene hydrogenation activity of the catalyst, resulting in an excessive acetylene content at the reactor outlet.
[0100] Operating Condition 2
[0101] Process conditions: material space velocity 1000 / h, operating pressure 2.0MPa, reactor inlet temperature 120℃, catalyst loading 100mL. Hydrogen / acetylene molar ratio 1.8.
[0102] Catalyst reduction: 150℃, hydrogen reduction for 4 hours.
[0103] Composition of hydrogenated feedstock:
[0104] Acetylene 0.1% (v / v), ethylene 90% (v / v), C3 0.5% (v / v), crude hydrogen 95% (v / v), CO 1%, CO content in the material 18.9 ppm.
[0105] Table 2 Evaluation results of the catalysts in Example 1 and Comparative Example 1 under operating condition 2
[0106]
[0107] As can be seen from the comparison between Table 2 and Table 1, for the catalyst of Comparative Example 1, increasing the hydrogen content alone, while keeping other conditions unchanged, can significantly reduce the acetylene content at the reactor outlet and reduce the generation of C4 and oxygen-containing byproducts. However, in Comparative Example 1, Ag is located on the outer surface of the active center, which leads to a decrease in catalyst activity, and this problem cannot be solved by significantly increasing the hydrogen content.
[0108] Example 2
[0109] Carrier: Commercially available spherical alumina carrier with a diameter of 3 mm was used. After calcination at 1080℃ for 4 hours, the water absorption rate and pore volume were 0.60 m³ / s. 3 / g, with a specific surface area of 29.95m². 2 / g. Weigh 100g of the carrier.
[0110] Catalyst preparation:
[0111] (1) Weigh 61.44g of lactic acid and mix it with 100g of calcined support. Keep the temperature at 180℃ for 1 hour to obtain semi-finished catalyst E.
[0112] (2) Take 22.5 mg of tris(4-formylphenyl)amine and 0.0056 mg of trifluoroacetic acid, dissolve them in 50 ml of dichloroethane, then mix them with catalyst E, stir and add a mixed solution of 34.43 mg of p-tetraphenyldiamine and 50 ml of dichloroethane dropwise. Let the mixture stand at room temperature for 100 hours, pour off the residue, wash with ethanol and deionized water respectively, and dry to obtain semi-finished catalyst F;
[0113] (3) Dissolve 94.47 mg of palladium acetylacetonate in 50 ml of chloroform. After the palladium acetylacetonate is completely dissolved, a palladium acetylacetonate solution is obtained. Immerse the semi-finished catalyst F in 50 ml of ethanol solution. Add the prepared palladium acetylacetonate solution dropwise to the mixture of semi-finished catalyst F and ethanol, while stirring for 20 hours. Then add 10 ml of formaldehyde solution dropwise to the above solution, stir at 60°C for 1 hour, decant the solution, wash with deionized water, dry at 120°C, and calcine at 300°C for 2 hours to obtain semi-finished catalyst G.
[0114] (4) Weigh 142 mg of silver nitrate and dissolve it in 60 g of deionized water. Immerse the semi-finished catalyst G in the prepared solution. After the solution is completely absorbed, let it stand for 4 hours. Then add 10 ml of formaldehyde solution to the above solution. Stir at 60 °C for 1 hour. Pour off the solution, wash with deionized water, and dry at 120 °C to obtain the semi-finished catalyst H.
[0115] (5) Dissolve 34.39 mg of palladium acetylacetonate in 50 ml of chloroform. After the palladium acetylacetonate is completely dissolved, a palladium acetylacetonate solution is obtained. Immerse the semi-finished catalyst H in 50 ml of ethanol solution. Add the prepared palladium acetylacetonate solution dropwise to the mixture of semi-finished catalyst H and ethanol, while stirring for 30 hours. Then add 10 ml of formaldehyde solution dropwise to the above solution, stir at 60°C for 1 hour, decant the solution, wash with deionized water, dry at 120°C, and calcine at 300°C for 2 hours to obtain the desired catalyst.
[0116] The prepared catalyst was determined by atomic absorption spectrometry, and the catalyst in Example 2 was found to have a Pd content of 0.045% and an Ag content of 0.09%.
[0117] Catalyst reduction: 150℃, hydrogen reduction for 4 hours.
[0118] Comparative Example 2
[0119] Carrier: The same carrier as in Example 2 was used, and the preparation conditions were the same, except that step (1) in Example 2 was omitted.
[0120] Catalyst preparation:
[0121] (1) Take 22.5 mg of tris(4-formylphenyl)amine and 0.0056 mg of trifluoroacetic acid, dissolve them in 50 ml of dichloroethane, and then mix them with 100 g of calcined support. Stir and add a mixed solution of 34.43 mg of p-tetraphenyldiamine and 50 ml of dichloroethane. Let the mixture stand at room temperature for 100 hours, pour off the residue, wash with ethanol and deionized water respectively, and dry to obtain the semi-finished catalyst F1.
[0122] (2) Dissolve 94.47 mg of palladium acetylacetonate in 50 ml of chloroform. After the palladium acetylacetonate is completely dissolved, a palladium acetylacetonate solution is obtained. Immerse the semi-finished catalyst F1 in 50 ml of ethanol solution. Add the prepared palladium acetylacetonate solution dropwise to the mixture of semi-finished catalyst F1 and ethanol, and stir for 20 hours. Then add 10 ml of formaldehyde solution dropwise to the above solution, stir at 60°C for 1 hour, decant the solution, wash with deionized water, dry at 120°C, and calcine at 300°C for 2 hours to obtain semi-finished catalyst G1.
[0123] (3) Weigh 142 mg of silver nitrate and dissolve it in 60 g of deionized water. Immerse the semi-finished catalyst G1 in the prepared solution. After the solution is completely absorbed, let it stand for 4 hours. Then add 10 ml of formaldehyde solution to the above solution. Stir at 60 °C for 1 hour. Pour off the solution, wash with deionized water, and dry at 120 °C to obtain the semi-finished catalyst H1.
[0124] (4) Dissolve 34.39 mg of palladium acetylacetonate in 50 ml of chloroform. After the palladium acetylacetonate is completely dissolved, a palladium acetylacetonate solution is obtained. Immerse the semi-finished catalyst H1 in 50 ml of ethanol solution. Add the prepared palladium acetylacetonate solution dropwise to the mixture of semi-finished catalyst H1 and ethanol, and stir for 30 hours. Then add 10 ml of formaldehyde solution dropwise to the above solution, stir at 60°C for 1 hour, decant the solution, wash with deionized water, dry at 120°C, and calcine at 300°C for 2 hours to obtain the desired catalyst.
[0125] The prepared catalyst was determined by atomic absorption spectrometry, and the catalyst in Comparative Example 2 had a Pd content of 0.045% and an Ag content of 0.09%.
[0126] Implementation effect
[0127] Process conditions: material space velocity 3000 / h, operating pressure 2.0MPa, reactor inlet temperature 95℃, hydrogen / acetylene ratio 2.0 (v / v).
[0128] Catalyst loading amount: 100 mL.
[0129] Catalyst reduction: 120℃, hydrogen reduction for 6 hours.
[0130] Composition of hydrogenated feedstock:
[0131] Acetylene 1.5% (v / v), Ethylene 70% (v / v), C3 0.7% (v / v)
[0132] The crude hydrogen contains 40% (v / v) hydrogen and 0.5% (v / v) CO, while the hydrogenated material contains 75 ppm CO.
[0133] Table 3 Evaluation results of the catalysts in Example 2 and Comparative Example 2
[0134]
[0135] As shown in Table 3, since the polymerization step of the monomer is not included in the preparation process of the catalyst in Comparative Example 2, the synthesis of the organic cage can be carried out at all positions inside the support, and the palladium loading also depends on the position of the organic cage. Due to the internal diffusion restriction effect of the gas phase reaction, only some active centers can participate normally in the hydrogenation reaction of acetylene, while some active centers cannot participate effectively, resulting in a significant excess of acetylene content at the reactor outlet of Comparative Example 2.
[0136] Even with an acetylene content of 1.5% (v / v) at the reactor inlet, a single-stage reactor can completely remove acetylene. In contrast, conventional methods require three reactor stages to completely remove acetylene when the content exceeds 1.4%, indicating that this hydrogenation method reduces the number of reactor stages and significantly lowers investment costs. Furthermore, in conventional methods, C4 formation can reach 500 ppm after 1500 hours, with significant catalyst coking, rendering a single-stage reactor insufficient for complete acetylene removal. This is why conventional hydrogenation methods cannot employ single-stage or even two-stage reactors.
[0137] Example 3
[0138] Commercially available spherical alumina-titanium oxide carriers with a titanium oxide content of 15 wt% and a diameter of 3 mm were used. After calcination at 1130℃ for 4 hours, the pore volume was 0.55 μm. 3 / g, with a specific surface area of 15.03m². 2 / g. Weigh 100g of the carrier.
[0139] Catalyst preparation:
[0140] (1) Weigh 18.38g acrylic acid, 30g water, 0.015g potassium hypophosphite monohydrate, 0.03g copper acetate monohydrate, and 0.20ml 30wt% hydrogen peroxide as initiator. After mixing evenly, add 100g of calcined carrier. After the solution is completely absorbed, transfer to a reflux flask and heat to 80℃ with stirring. Keep the temperature constant for 1 hour to obtain semi-finished catalyst I.
[0141] (2) Take 8.13 mg of tris(4-formylphenyl)amine and 0.0041 mg of trichloroacetic acid, dissolve them in 50 ml of dichloroethane, then mix them with catalyst I, stir and add a mixed solution of 17.17 mg of 2-methyltetraphenyldiamine and 10 ml of trichloroethane dropwise. Let the mixture stand at room temperature for 150 hours, pour off the residue, wash with ethanol and deionized water respectively, and dry to obtain semi-finished catalyst J;
[0142] (3) Dissolve 93 mg of palladium acetylacetonate in 50 ml of chloroform. After the palladium acetylacetonate is completely dissolved, a palladium acetylacetonate solution is obtained. Immerse catalyst J in 50 ml of methanol solution. Add the prepared palladium acetylacetonate solution dropwise to a mixture of semi-finished catalyst J and ethanol, and stir for 60 hours. Then add 10 ml of formic acid solution dropwise to the above solution, heat and stir at 70°C for 2 hours, decant the solution, wash with deionized water, dry at 120°C, and calcine at 400°C for 2 hours to obtain semi-finished catalyst K.
[0143] (4) Dissolve 157.48 mg of silver nitrate in 50 g of deionized water, immerse catalyst K in the prepared solution, and let it stand for 4 hours after the solution is completely absorbed. Add 5 ml of 10 wt% hydrazine hydrate solution to the above solution, stir at 40 °C for 1 hour, descalcify the solution, wash with deionized water, and dry at 120 °C to obtain semi-finished catalyst M.
[0144] (5) Dissolve 93.14 mg of palladium acetylacetonate in 50 ml of chloroform. After the palladium acetylacetonate is completely dissolved, a palladium acetylacetonate solution is obtained. Immerse catalyst M in 50 ml of methanol solution. Add the prepared palladium acetylacetonate solution dropwise to a mixture of the semi-finished catalyst and ethanol, while stirring for 30 hours. Then add 10 ml of formic acid solution dropwise to the above solution, heat and stir at 70°C for 2 hours, decant the solution, wash with deionized water, and dry at 120°C to obtain the desired catalyst.
[0145] The prepared catalyst was determined by atomic absorption spectrometry, and the catalyst in Example 3 had a Pd content of 0.065% and an Ag content of 0.10%.
[0146] Comparative Example 3
[0147] The same carrier as in Example 3 was used, except that the amount of tris(4-formylphenyl)amine was three times that in Example 3.
[0148] Catalyst preparation:
[0149] (1) Weigh 18.38g acrylic acid, 30g water, 0.015g potassium hypophosphite monohydrate, 0.03g copper acetate monohydrate, and 0.20ml 30% hydrogen peroxide as initiator. After mixing evenly, add 100g of calcined carrier. After the solution is completely absorbed, transfer to a reflux flask and heat to 80℃ with stirring. Keep the temperature constant for 1 hour to obtain semi-finished catalyst I1.
[0150] (2) Take 24.39 mg of tris(4-formylphenyl)amine and 0.0041 mg of trichloroacetic acid, dissolve them in 50 ml of dichloroethane, then mix them with catalyst I1, stir and add a mixed solution of 17.17 mg of 2-methyltetraphenyldiamine and 10 ml of trichloroethane, let the mixture stand at room temperature for 150 hours, pour off the residue, wash with ethanol and deionized water respectively, and dry to obtain semi-finished catalyst J1;
[0151] (3) Dissolve 93 mg of palladium acetylacetonate in 50 ml of chloroform. After the palladium acetylacetonate is completely dissolved, a palladium acetylacetonate solution is obtained. Immerse catalyst J1 in 50 ml of methanol solution. Add the prepared palladium acetylacetonate solution dropwise to a mixture of semi-finished catalyst J and ethanol, and stir for 60 hours. Then add 10 ml of formic acid solution dropwise to the above solution, heat and stir at 70°C for 2 hours, decant the solution, wash with deionized water, dry at 120°C, and calcine at 400°C for 2 hours to obtain semi-finished catalyst K1.
[0152] (4) Dissolve 157.48 mg of silver nitrate in 50 g of deionized water, immerse catalyst K1 in the prepared solution, and let it stand for 4 hours after the solution is completely absorbed. Add 5 ml of 10% hydrazine hydrate solution dropwise to the above solution, stir at 40 °C for 1 hour, decant the solution, wash with deionized water, and dry at 120 °C to obtain semi-finished catalyst M1.
[0153] (5) Dissolve 93.14 mg of palladium acetylacetonate in 50 ml of chloroform. After the palladium acetylacetonate is completely dissolved, a palladium acetylacetonate solution is obtained. Immerse catalyst M1 in 50 ml of methanol solution. Add the prepared palladium acetylacetonate solution dropwise to a mixture of the semi-finished catalyst and ethanol, while stirring for 30 hours. Then add 10 ml of formic acid solution dropwise to the above solution, heat and stir at 70°C for 2 hours, decant the solution, wash with deionized water, and dry at 120°C to obtain the desired catalyst.
[0154] The prepared catalyst was determined by atomic absorption spectrometry, and the catalyst in Comparative Example 3 had a Pd content of 0.065% and an Ag content of 0.10%.
[0155] Implementation results:
[0156] Process conditions: Two-stage hydrogenation process, material space velocity 6000 / h, operating pressure 2.5MPa, inlet temperature of the first-stage reactor 45℃, inlet temperature of the second-stage reactor 95℃, hydrogen / acetylene volume ratio of the first stage 1.1, hydrogen / acetylene volume ratio of the second stage 2.0, catalyst loading of each reactor 100mL.
[0157] Composition of hydrogenated feedstock:
[0158] Acetylene 0.8% (v / v), ethylene 80% (v / v), C3 0.3% (v / v);
[0159] The crude hydrogen contains 50% hydrogen (v / v) and 0.1% CO, while the CO content in the first-stage inlet material is 17.6 ppm.
[0160] The evaluation results are shown in Table 4.
[0161] Table 4 Evaluation results of the catalysts in Example 3 and Comparative Example 3
[0162]
[0163] As shown in Table 4, when the catalysts of Example 3 and Comparative Example 3 were used for selective hydrogenation of acetylene, the acetylene conversion rate of the reactor in Example 3 was significantly higher than that in Comparative Example 3. This may be because there were too many tris(4-formylphenyl)amine molecules in Comparative Example 3, resulting in an excessive number of organic cages generated in the early stage of organic cage synthesis. After loading the active component palladium, the average palladium loaded on each organic cage was too small, and its activity was low, especially after CO participated in the reaction, its activity was even more insufficient.
[0164] Example 4
[0165] Carrier: Commercially available toothed spherical alumina-magnesium oxide carrier with a magnesium oxide content of 3% and a diameter of 2 mm was used. After calcination at 1110℃ for 4 hours, the pore volume was 0.50 m³ / s. 3 / g, with a specific surface area of 20.83m².2 / g. Weigh 100g of the carrier.
[0166] Catalyst preparation:
[0167] (1) Weigh 56.71g of lactic acid and mix it with 100g of calcined support. Add the mixture and keep it at 160℃ for 6 hours to obtain the semi-finished catalyst N.
[0168] (2) Take 5.35 mg of tris(4-formylphenyl)amine and 0.0018 mg of trifluoroacetic acid, dissolve them in 50 ml of dichloroethane, and then mix them with the semi-finished catalyst N. Stir and add a mixed solution of 10.93 mg of tetraphenyldiamine and 10 ml of dichloroethane. Let the mixture stand at room temperature for 180 hours, pour off the residue, wash with ethanol and deionized water respectively, and dry to obtain the semi-finished catalyst O.
[0169] (3) Dissolve 63.42 mg of palladium acetate in 50 ml of chloroform. After the palladium acetate is completely dissolved, a palladium acetate solution is obtained. Immerse the semi-finished catalyst O in 50 ml of ethanol solution. Add the prepared palladium acetate solution dropwise to the mixture of semi-finished catalyst O and ethanol, and stir for 20 hours. Then add 20 ml of methanol solution dropwise to the above solution, stir at 80°C for 1 hour, decant the solution, wash with deionized water, dry at 120°C, and calcine at 400°C for 1 hour to obtain the semi-finished catalyst P.
[0170] (4) Dissolve 230.23 mg of silver acetylacetonate in 39.45 g of ethanol. Immerse the semi-finished catalyst P in the prepared solution. After the solution is completely absorbed, let it stand for 4 hours. Then add 20 ml of formic acid solution to the above solution. Stir at 80 °C for 1 hour. Pour off the solution, wash with deionized water, and dry at 120 °C to obtain the semi-finished catalyst Q.
[0171] (5) Dissolve 94.84 mg of palladium acetate in 50 ml of chloroform until the palladium acetate is completely dissolved to obtain a palladium acetate solution. Immerse the semi-finished catalyst Q in 50 ml of ethanol solution. Add the prepared palladium acetate solution dropwise to the mixture of support and ethanol while stirring for 20 hours. Then add 20 ml of methanol solution dropwise to the above solution and stir at 80°C for 1 hour. Pour off the solution, wash with deionized water, dry at 120°C, and calcine at 400°C for 1 hour to obtain the desired catalyst.
[0172] The prepared catalyst was determined by atomic absorption spectrometry, and the catalyst in Example 4 had a Pd content of 0.075% and an Ag content of 0.12%.
[0173] Comparative Example 4
[0174] The catalyst support used is the same as in Example 4, except that the calcination temperature in step (3) is 550°C.
[0175] Catalyst preparation:
[0176] (1) Weigh 56.71g of lactic acid and mix it with 100g of calcined support. Add the mixture and keep it at 160℃ for 6 hours to obtain the semi-finished catalyst N1.
[0177] (2) Take 5.35 mg of tris(4-formylphenyl)amine and 0.0018 mg of trifluoroacetic acid, dissolve them in 50 ml of dichloroethane, and then mix them with the semi-finished catalyst N1. Stir and add a mixed solution of 10.93 mg of tetraphenyldiamine and 10 ml of dichloroethane. Let the mixture stand at room temperature for 180 hours, pour off the residual liquid, wash it with ethanol and deionized water respectively, and dry it to obtain the semi-finished catalyst O1.
[0178] (3) Dissolve 63.42 mg of palladium acetate in 50 ml of chloroform. After the palladium acetate is completely dissolved, a palladium acetate solution is obtained. Immerse the semi-finished catalyst O1 in 50 ml of ethanol solution. Add the prepared palladium acetate solution dropwise to the mixture of semi-finished catalyst O1 and ethanol, and stir for 20 hours. Then add 20 ml of methanol solution dropwise to the above solution, stir at 80°C for 1 hour, decant the solution, wash with deionized water, dry at 120°C, and calcine at 550°C for 1 hour to obtain the semi-finished catalyst P1.
[0179] (4) Dissolve 230.23 mg of silver acetylacetonate in 39.45 g of ethanol. Immerse the semi-finished catalyst P1 in the prepared solution. After the solution is completely absorbed, let it stand for 4 hours. Then add 20 ml of formic acid solution to the above solution. Stir at 80 °C for 1 hour. Pour off the solution, wash with deionized water, and dry at 120 °C to obtain the semi-finished catalyst Q1.
[0180] (5) Dissolve 94.84 mg of palladium acetate in 50 ml of chloroform until the palladium acetate is completely dissolved to obtain a palladium acetate solution. Immerse the semi-finished catalyst Q1 in 50 ml of ethanol solution. Add the prepared palladium acetate solution dropwise to the mixture of support and ethanol while stirring for 20 hours. Then add 20 ml of methanol solution dropwise to the above solution and stir at 80°C for 1 hour. Pour off the solution, wash with deionized water, dry at 120°C, and calcine at 550°C for 1 hour to obtain the desired catalyst.
[0181] The prepared catalyst was determined by atomic absorption spectrometry, and the catalyst in Comparative Example 4 had a Pd content of 0.075% and an Ag content of 0.12%.
[0182] Implementation effect
[0183] Process conditions: Two-stage hydrogenation process, material space velocity 5000 / h, operating pressure 2.6MPa, inlet temperature of the first-stage reactor 50℃, inlet temperature of the second-stage reactor 70℃, hydrogen / acetylene ratio of 1.3 (v / v) in the first stage, and hydrogen / acetylene ratio of 1.8 (v / v) in the second stage.
[0184] Catalyst loading amount for each reactor: 100 mL.
[0185] Catalyst reduction: 150℃, hydrogen reduction for 4 hours.
[0186] Composition of hydrogenated feedstock:
[0187] Acetylene 1.0% (v / v), Ethylene 60% (v / v), C3 0.4% (v / v)
[0188] The crude hydrogen contains 70% hydrogen (v / v) and 0.2% CO. The CO content in the first inlet material is 37.1 ppm.
[0189] Table 5 Evaluation results of the catalysts in Example 4 and Comparative Example 4
[0190]
[0191]
[0192] As shown in Table 5, the evaluation results of the catalysts in Example 4 and Comparative Example 4 differ significantly, especially in the two-stage reactor of Comparative Example 4, which could not completely convert acetylene. The reason may be that the calcination temperature in step (3) of the catalyst preparation in Comparative Example 4 was 550°C, which destroyed the structure of the organic cage, resulting in the palladium loading in step (5) not being effectively positioned within the organic cage, and its dispersion being too high, so some palladium could not form active aggregates.
[0193] Example 5
[0194] The carrier is a spherical alumina-magnesia carrier with a magnesium oxide content of 10% and a diameter of 2 mm. After calcination at 1090℃ for 4 hours, the pore volume is 0.53 m³. 3 / g, with a specific surface area of 28.45m². 2 / g. Weigh 100g of the carrier.
[0195] Catalyst preparation:
[0196] (1) Weigh 58.30g of lactic acid and mix it with 100g of calcined support. Add the mixture and keep it at 190℃ for 2 hours to obtain the semi-finished catalyst R.
[0197] (2) Take 7 mg of tris(4-formylphenyl)amine and 0.0028 mg of dichloroacetic acid, dissolve them in 50 ml of dichloroethane, then mix them with catalyst R, stir and add a mixed solution of 17.32 mg of 2-chlorotetraphenyldiamine and 10 ml of dichloroethane, let the mixture stand at room temperature for 190 hours, pour off the residue, wash with ethanol and deionized water respectively, and dry to obtain semi-finished catalyst S;
[0198] (3) Dissolve 157 mg of silver nitrate in 50 g of deionized water, immerse the semi-finished catalyst S in the prepared solution, and after the solution is completely absorbed, let it stand for 4 hours. Then add 20 ml of formic acid solution to the above solution, stir at 50 °C for 1 hour, pour off the solution, wash with deionized water, and dry at 120 °C to obtain the semi-finished catalyst U.
[0199] (4) Dissolve 203.32 mg of palladium acetylacetonate in 50 ml of benzene. After the palladium acetylacetonate is completely dissolved, a palladium acetylacetonate solution is obtained. Immerse the semi-finished catalyst U in 50 ml of methanol solution. Add the prepared palladium acetylacetonate solution dropwise to the mixture of semi-finished catalyst U and methanol, and stir for 50 hours. Then add 10 ml of formic acid solution dropwise to the above solution, stir at 50°C for 1 hour, decant the solution, wash with deionized water, dry at 120°C, and calcine at 380°C for 1 hour to obtain the desired catalyst.
[0200] The prepared catalyst was determined by atomic absorption spectrometry, and the catalyst in Example 5 was found to have a Pd content of 0.070% and an Ag content of 0.1%.
[0201] Comparative Example 5
[0202] The catalyst support and preparation conditions were the same as in Example 5, except that in step (2), the amount of tris(4-formylphenyl)amine used was 1 / 2 times that in Example 5.
[0203] (1) Weigh 58.30g of lactic acid and mix it with 100g of calcined support. Add the mixture and keep it at 190℃ for 2 hours to obtain the semi-finished catalyst R1.
[0204] (2) Take 3.5 mg of tris(4-formylphenyl)amine and 0.0028 mg of dichloroacetic acid, dissolve them in 50 ml of dichloroethane, and then mix them with catalyst R1. Stir and add dropwise a mixed solution of 17.32 mg of 2-chlorotetraphenyldiamine and 10 ml of dichloroethane. Let the mixture stand at room temperature for 190 hours, pour off the residue, wash with ethanol and deionized water respectively, and dry to obtain semi-finished catalyst S1;
[0205] (4) Dissolve 157 mg of silver nitrate in 50 g of deionized water, immerse the semi-finished catalyst S1 in the prepared solution, and after the solution is completely absorbed, let it stand for 4 hours. Then add 20 ml of formic acid solution to the above solution, stir at 50 °C for 1 hour, pour off the solution, wash with deionized water, and dry at 120 °C to obtain the semi-finished catalyst U1.
[0206] (5) Dissolve 200.32 mg of palladium acetylacetonate in 50 ml of benzene. After the palladium acetylacetonate is completely dissolved, a palladium acetylacetonate solution is obtained. Immerse the semi-finished catalyst U1 in 50 ml of methanol solution. Add the prepared palladium acetylacetonate solution dropwise to the mixture of semi-finished catalyst U1 and methanol, and stir for 50 hours. Then add 10 ml of formic acid solution dropwise to the above solution, stir at 50°C for 1 hour, decant the solution, wash with deionized water, dry at 120°C, and calcine at 380°C for 1 hour to obtain the desired catalyst.
[0207] The prepared catalyst was determined by atomic absorption spectrometry, and the catalyst in Comparative Example 5 had a Pd content of 0.070% and an Ag content of 0.1%.
[0208] Implementation effect
[0209] Process conditions: Two-stage hydrogenation process, material space velocity 6000 / h, operating pressure 3.0MPa, inlet temperature of the first stage reactor 70℃, inlet temperature of the second stage reactor 80℃, hydrogen / acetylene ratio of 1.2 in the first stage, and hydrogen / acetylene ratio of 1.4 in the second stage.
[0210] Catalyst loading amount for each reactor: 100 mL.
[0211] Catalyst reduction: 110℃, hydrogen reduction for 6 hours.
[0212] Composition of hydrogenated feedstock:
[0213] Acetylene 0.6% (v / v), Ethylene 70% (v / v), C3 0.4% (v / v)
[0214] The crude hydrogen contains 20% hydrogen (v / v) and 1% CO, while the inlet material contains 360 ppm CO.
[0215] Table 6 Evaluation results of the catalysts in Example 5 and Comparative Example 5
[0216]
[0217] As shown in Table 6, when the catalyst of Example 5 was used for selective hydrogenation of acetylene, the acetylene content at the outlet of the first-stage reactor was already very low. With a hydrogen / acetylene ratio of only 1.4 in the second stage, it was possible to ensure that there was no acetylene residue at the outlet of the second-stage reactor. However, when the catalyst of Comparative Example 5 was used for selective hydrogenation of acetylene, the acetylene content at the outlet of the second-stage reactor exceeded the standard. The reason may be that the content of tris(4-formylphenyl)amine was low during the preparation of the catalyst of Comparative Example 5, and the number of synthesized organic cages was correspondingly small. After loading silver, when palladium was loaded for secondary loading, the volume of the palladium precursor in the primary loading was large, and the organic cage could not accommodate so much palladium precursor. As a result, some palladium was loaded at other positions on the catalyst during the secondary loading, and could not form an active aggregate structure, resulting in unsatisfactory acetylene conversion efficiency.
[0218] Of course, the present invention may have other various embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications according to the present invention, but these corresponding changes and modifications should all fall within the protection scope of the claims of the present invention.
Claims
1. A method for selective hydrogenation of alkynes, characterized in that, The hydrogenation feedstock is a C2 fraction, which enters a reactor for gas-phase hydrogenation to remove acetylene. The process conditions for this gas-phase hydrogenation are: reactor inlet temperature 45–120°C, pressure 1.5–3.0 MPa, and gas hourly space velocity 1000–6000 h⁻¹. -1 The hydrogen required for this gas-phase hydrogenation comes from crude hydrogen, which contains 0.1-1% CO by volume and 20-95% hydrogen by volume. The catalyst used for this gas-phase hydrogenation has an alumina support and Pd and Ag as active components. Based on 100% of the support mass, the mass content of Pd is 0.045-0.075%, and the mass content of Ag is 0.06-0.12%. Palladium is located in an organic cage on the outer surface of the catalyst, and the size of the organic cage is 2.7-3.6 nm. Silver is located in the middle or bottom of the palladium active center. The method for preparing the catalyst includes: (1) The hydrophilic polymerizable monomer is mixed with the calcined support and polymerized at a certain temperature to obtain the semi-finished catalyst A; (2) Take tris(4-formylphenyl)amine and haloacetic acid, dissolve them in haloalkanes, and then mix them with semi-finished catalyst A. Stir and add a mixed solution of tetraphenyldiamine and haloalkanes dropwise. Let the mixture stand until the reaction is complete, pour off the residual liquid, wash it with alcohol and deionized water respectively, and dry it to obtain semi-finished catalyst B. (3) Dissolve the organic palladium compound in an organic solvent to obtain the first solution of the palladium precursor; The semi-finished catalyst B is immersed in an alcohol solution. The first solution of palladium precursor is added dropwise to the mixture of semi-finished catalyst B and alcohol while stirring. Then, a reducing agent is added dropwise, and the mixture is heated and stirred. When the surface of semi-finished catalyst B no longer changes color, the solution is poured off, washed with deionized water, dried, and calcined at a temperature below 450°C where the polymer formed in step (1) can be decomposed, to obtain semi-finished catalyst C. (4) Dissolve the silver-containing compound in deionized water or organic solvent to obtain a silver impregnation solution. The total amount of the silver impregnation solution is equivalent to the pore volume of the carrier. Immerse the semi-finished catalyst C in the silver impregnation solution. After complete absorption, let it stand, add a reducing agent to reduce the silver, pour off the solution, wash with deionized water, and dry to obtain the semi-finished catalyst D. (5) Dissolve the organic palladium compound in an organic solvent. After the organic palladium is completely dissolved, a second palladium precursor solution is obtained. The semi-finished catalyst D is immersed in an alcohol solution. The second palladium precursor solution is added dropwise to the mixture of semi-finished catalyst D and alcohol while stirring. Add the reducing agent dropwise to the above solution, heat and stir. When the surface of the semi-finished catalyst D no longer changes color, pour off the solution, wash and dry to obtain the catalyst. Alternatively, without reduction, pour off the solution, wash with deionized water, dry, and calcine to obtain the catalyst. The tetraphenyldiamine compound is tetraphenyldiamine or tetraphenyldiamine with substituents on the benzene ring, wherein the substituents are alkyl or halogens.
2. The selective hydrogenation method for alkynes according to claim 1, characterized in that, The reactor is an adiabatic reactor or an isothermal reactor; the reactor is a single-stage reactor or a two-stage reactor.
3. The selective hydrogenation method for alkynes according to claim 2, characterized in that, The reactor is a fixed-bed single-stage reactor with a hydrogen / acetylene molar ratio of 1.3 to 2.0 at the reactor inlet; or, the reactor is a fixed-bed two-stage reactor with a hydrogen / acetylene molar ratio of 1.1 to 1.3 at the inlet of the first-stage reactor and a hydrogen / acetylene molar ratio of 1.4 to 2.0 at the inlet of the second-stage reactor.
4. The selective hydrogenation method for alkynes according to claim 1, characterized in that, The C2 fraction contains 60-90% ethylene by volume and 0.1-1.5% acetylene by volume.
5. The selective hydrogenation method for alkynes according to claim 1, characterized in that, The catalyst has a specific surface area of 15–30 m². 2 / g.
6. The selective hydrogenation method for alkynes according to claim 1, characterized in that, The volume of the polymer synthesized from the hydrophilic polymerizable monomer is 80-95% of the carrier pore volume; The molar ratio of tetraphenyldiamine compounds to tris(4-formylphenyl)amine is 1.2-2.5:1, and the mass ratio of tris(4-formylphenyl)amine to haloacetic acid is 2000-6000:
1.
7. The selective hydrogenation method for alkynes according to claim 1, characterized in that, The hydrophilic polymerizable monomer contains a carbonyl group, a carboxyl group, or a carbon-carbon double bond; the hydrophilic polymerizable monomer can undergo polymerization or condensation reactions at temperatures below 420°C; after polymerization, the hydrophilic polymerizable monomer can decompose at temperatures above 420°C and below 450°C.
8. The selective hydrogenation method for alkynes according to claim 1, characterized in that, The organic palladium compound is palladium acetate or palladium acetylacetonate; the silver-containing compound is a soluble silver salt; and the reducing agent is methanol, formaldehyde, formic acid, ethanol, acetaldehyde, or hydrazine hydrate.
9. The selective hydrogenation method for alkynes according to claim 8, characterized in that, The mass ratio of palladium in a portion of the organopalladium compound in step (3) to the remaining organopalladium compound in step (5) is 0~1:0.36~2.
12.
10. The selective hydrogenation method for alkynes according to claim 6, characterized in that, The total mass ratio of palladium to tris(4-formylphenyl)amine in steps (3) and (5) is 2-14:
1.
11. The selective hydrogenation method for alkynes according to claim 6, characterized in that, The volume of the polymer synthesized from the hydrophilic polymerizable monomer is 85-95% of the carrier pore volume.
12. The selective hydrogenation method for alkynes according to claim 6, characterized in that, The tetraphenyldiamine compound is p-tetraphenyldiamine or p-tetraphenyldiamine with a substituent on the benzene ring, wherein the substituent is an alkyl group or a halogen.
Citation Information
Patent Citations
Hydrogenation catalyst and preparation method thereof
CN101433842A
Selectively hydrogenating catalyst and preparation method thereof
CN101433845A
Non-noble metal supported selective hydrogenation catalyst and preparation method and application thereof
CN101664682A
A selective hydrogenation method for C2 fraction alkynes
CN112679301B
Two peak hole distribution calalyst for hydrocarbon conversion and preparation thereof
CN1129606A