A composite catalyst, a preparation method and application thereof, and a preparation method of allyl alcohol block polyoxyethylene polyoxypropylene ether

By using a composite catalyst containing magnesium, palladium, and platinum, allyl alcohol block polyoxyethylene polyoxypropylene ether was prepared, which solved the problems of low double bond retention and wide molecular distribution in the prior art and improved the hydrophilicity of the fabric finishing agent.

CN117447692BActive Publication Date: 2026-11-24ZHEJIANG HUANGMA TECH CO LTD +3
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311604784.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-28
Publication Date
2026-11-24
Estimated Expiration
2043-11-28

AI Technical Summary

Technical Problem

In the existing preparation process of allyl alcohol polyether, the double bond retention rate is not high and the molecular distribution is wide, which leads to poor solubility of the finishing agent in aqueous solution and affects the hydrophilicity.

Method used

Using a composite catalyst containing magnesium, palladium, and platinum, magnesium, palladium, and platinum are supported on activated carbon and combined with two addition reactions to prepare allyl alcohol block polyoxyethylene polyoxypropylene ether, thereby improving the double bond retention rate and the narrow molecular distribution.

Benefits of technology

The preparation of allyl alcohol block polyoxyethylene polyoxypropylene ether with high double bond retention rate and narrow molecular distribution was achieved, which improved the hydrophilicity and solubility of the fabric finishing agent in aqueous solution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of polyether preparation technology, and more particularly to a composite catalyst, its preparation method and application, and a method for preparing allyl alcohol block polyoxyethylene polyoxypropylene ether. This invention provides a composite catalyst containing magnesium, palladium, and platinum, comprising activated carbon and magnesium, palladium, and platinum supported on the activated carbon; the total mass ratio of the magnesium, palladium, and platinum to the activated carbon is 1:(3-6). The composite catalyst enables the prepared allyl alcohol block polyoxyethylene polyoxypropylene ether to possess excellent properties such as high double bond retention and narrow distribution. 。
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyether preparation technology, and in particular to a composite catalyst, its preparation method and application, and a method for preparing allyl alcohol block polyoxyethylene polyoxypropylene ether. Background Technology

[0002] Allyl alcohol is an important chemical intermediate and fine chemical product. It possesses both double bonds and hydroxyl groups, enabling it to participate in various reactions such as oxidation, reduction, esterification, etherification, and addition. Addition reactions are the most common, particularly with ethylene oxide and propylene oxide. Allyl alcohol polyoxyethylene polyoxypropylene ether, formed from the reaction of allyl alcohol with ethylene oxide and propylene oxide, is a major raw material for producing organic textile finishing agents. It can modify the hydrophilicity and antistatic properties of organosilicon. Garments treated with this agent have a soft, smooth feel and excellent antistatic and hydrophilic properties, making it a widely used textile finishing agent in my country. However, current allyl alcohol polyether preparation processes have certain drawbacks. Specifically, the resulting polyether has a low double bond retention rate and a wide molecular distribution, which limits its application in organosilicon modification and grafting, thus affecting the hydrophilicity of the textile finishing agent and resulting in poor solubility in aqueous solutions, failing to achieve optimal effects. Therefore, developing an allyl alcohol polyether with high double bond retention and narrow molecular distribution is particularly important. Summary of the Invention

[0003] The purpose of this invention is to provide a composite catalyst, its preparation method and application, and a method for preparing allyl alcohol block polyoxyethylene polyoxypropylene ether. The composite catalyst enables the prepared allyl alcohol block polyoxyethylene polyoxypropylene ether to possess excellent properties such as high double bond retention rate and narrow distribution.

[0004] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0005] The present invention provides a composite catalyst containing magnesium, palladium and platinum, comprising activated carbon and magnesium, palladium and platinum supported on the activated carbon;

[0006] The total mass ratio of magnesium, palladium, and platinum to activated carbon is 1:(3-6).

[0007] Preferably, the mass ratio of magnesium, palladium and platinum is (10-70):(10-70):(10-70).

[0008] This invention also provides a method for preparing the magnesium-, palladium-, and platinum-containing composite catalyst described in the above technical solution, comprising the following steps:

[0009] A mixture is prepared by mixing soluble magnesium salt, soluble palladium salt, soluble platinum salt and water.

[0010] Under alkaline conditions, sodium carbonate solution and the mixture are mixed, a precipitation reaction is carried out, and then heat treatment is performed to obtain a metal mixture of magnesium, palladium and platinum.

[0011] The magnesium, palladium and platinum metal mixture is mixed with activated carbon and calcined to obtain the magnesium, palladium and platinum composite catalyst.

[0012] Preferably, the calcination process is as follows: the temperature is increased to 550°C at a heating rate of 30°C / 10min, and then held for 12 hours.

[0013] The present invention also provides the application of the composite catalyst containing magnesium, palladium and platinum as described in the above technical solution or the composite catalyst containing magnesium, palladium and platinum prepared by the preparation method described in the above technical solution in the preparation of allyl alcohol block polyoxyethylene polyoxypropylene ether.

[0014] This invention also provides a method for preparing allyl alcohol block polyoxyethylene polyoxypropylene ether, comprising the following steps:

[0015] Allyl alcohol, potassium hydroxide and ethylene oxide are mixed and subjected to the first addition reaction to obtain allyl alcohol polyoxyethylene ether.

[0016] The allyl alcohol polyoxyethylene ether, a composite catalyst containing magnesium, palladium and platinum, and propylene oxide are mixed and subjected to a second addition reaction to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether.

[0017] The magnesium-, palladium-, and platinum-containing composite catalyst is the magnesium-, palladium-, and platinum-containing composite catalyst described in the above technical solution or the magnesium-, palladium-, and platinum-containing composite catalyst prepared by the preparation method described in the above technical solution.

[0018] Preferably, the molar ratio of allyl alcohol to ethylene oxide is 1:(20-30);

[0019] The potassium hydroxide accounts for 1‰ of the mass percentage of the allyl alcohol polyoxyethylene ether.

[0020] Preferably, the temperature of the first addition reaction is 100–105°C.

[0021] Preferably, the molar ratio of allyl alcohol to propylene oxide is 1:(30-35);

[0022] The composite catalyst containing magnesium, palladium, and platinum accounts for 1.5 to 2‰ of the mass of the allyl alcohol block polyoxyethylene polyoxypropylene ether.

[0023] Preferably, the temperature of the second addition reaction is 100–105°C.

[0024] This invention provides a composite catalyst containing magnesium, palladium, and platinum, comprising activated carbon and magnesium, palladium, and platinum supported on the activated carbon; the total mass ratio of magnesium, palladium, and platinum to activated carbon is 1:(3-6). The composite catalyst of this invention contains a certain metal mixture. Magnesium and platinum have a certain degree of ductility, allowing for better loading onto the activated carbon. In particular, palladium metal exhibits excellent catalytic activity, effectively enabling the ring-opening of propylene oxide while simultaneously undergoing surface addition isomerization due to its high selectivity. Furthermore, the activated carbon has a porous structure and a large specific surface area, which can significantly increase the contact area and reactivity of the supported material, thereby accelerating the reaction. Activated carbon also has excellent adsorption properties, allowing for effective removal of activated carbon from the final product, thus improving the application performance and prospects of polyethers.

[0025] This invention also provides a method for preparing allyl alcohol block polyoxyethylene polyoxypropylene ether, comprising the following steps: mixing allyl alcohol, potassium hydroxide, and ethylene oxide, and performing a first addition reaction to obtain allyl alcohol polyoxyethylene ether; mixing the allyl alcohol polyoxyethylene ether, a composite catalyst containing magnesium, palladium, and platinum, and propylene oxide, and performing a second addition reaction to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether; wherein the composite catalyst containing magnesium, palladium, and platinum is the composite catalyst containing magnesium, palladium, and platinum described in the above technical solution or the composite catalyst containing magnesium, palladium, and platinum prepared by the preparation method described in the above technical solution. The composite catalyst of this invention has excellent selectivity, preferentially undergoing the ring-opening reaction of epoxide, thereby protecting the double bonds from reaction and increasing the double bond retention rate, while the excellent activity of the catalyst ensures a narrow molecular distribution. Detailed Implementation

[0026] The present invention provides a composite catalyst containing magnesium, palladium and platinum, comprising activated carbon and magnesium, palladium and platinum supported on the activated carbon;

[0027] The total mass ratio of magnesium, palladium, and platinum to activated carbon is 1:(3-6).

[0028] In this invention, the particle size of the activated carbon is preferably 1 mm. This invention does not impose any special limitations on the type of activated carbon; any type well-known to those skilled in the art can be used. In an embodiment of this invention, the activated carbon is specifically coconut shell activated carbon.

[0029] In this invention, the mass ratio of magnesium, palladium and platinum is preferably (10-70):(10-70):(10-70), more preferably (15-40):(15-40):(20-70), and most preferably (30-40):(30-40):(30-40).

[0030] In this invention, the mass ratio of the total mass of magnesium, palladium and platinum to the mass of activated carbon is preferably 1:(3-6), more preferably 1:(4-5), and most preferably 1:4.

[0031] This invention also provides a method for preparing the magnesium, palladium and platinum-containing composite catalyst described in the above technical solution, comprising the following steps:

[0032] A mixture is prepared by mixing soluble magnesium salt, soluble palladium salt, soluble platinum salt and water.

[0033] Under alkaline conditions, sodium carbonate solution and the mixture are mixed, a precipitation reaction is carried out, and then heat treatment is performed to obtain a metal mixture of magnesium, palladium and platinum.

[0034] The magnesium, palladium and platinum metal mixture is mixed with activated carbon and calcined to obtain the magnesium, palladium and platinum composite catalyst.

[0035] In this invention, unless otherwise specified, all raw materials used in the preparation are commercially available products well known to those skilled in the art.

[0036] This invention involves mixing soluble magnesium salt, soluble palladium salt, soluble platinum salt, and water to obtain a mixed solution.

[0037] In this invention, the soluble magnesium salt is preferably magnesium nitrate; the soluble palladium salt is preferably palladium nitrate; the soluble platinum salt is preferably platinum nitrate; and the water is preferably distilled water.

[0038] In this invention, the preferred mass ratio of magnesium in the soluble magnesium salt, palladium in the soluble palladium salt, and platinum in the soluble platinum salt is (10-70):(10-70):(10-70), more preferably (15-40):(15-40):(20-70), and most preferably (30-40):(30-40):(30-40). This invention does not impose any special limitation on the amount of water used; any amount of water known to those skilled in the art can be used to ensure complete dissolution of the soluble magnesium salt, soluble palladium salt, and soluble platinum salt in the water.

[0039] In this invention, the mixing is preferably carried out under stirring conditions. This invention does not impose any special limitations on the stirring process, and any process well known to those skilled in the art can be used.

[0040] After obtaining the mixture, the present invention mixes the sodium carbonate solution and the mixture under alkaline conditions, performs a precipitation reaction, and then heat-treats to obtain a metal mixture of magnesium, palladium and platinum.

[0041] In this invention, the preferred mass concentration of the sodium carbonate solution is 2%. This invention does not impose any special limitations on the amount of sodium carbonate solution used; any amount well-known to those skilled in the art that ensures the resulting mixture is alkaline is acceptable.

[0042] In this invention, the mixing is preferably performed by adding the mixture to the sodium carbonate solution; the addition is preferably done dropwise. In this invention, the addition temperature is preferably 50°C, more preferably 55°C; the addition is preferably performed under stirring conditions. This invention does not impose any special limitations on the stirring process; any process well-known to those skilled in the art can be used. After the dropwise addition is completed, this invention further preferably includes continuing stirring for 1 hour.

[0043] In this invention, the alkaline conditions are preferably adjusted using a sodium hydroxide solution with a concentration of 2 mol / L; the pH of the alkaline conditions is preferably 9 to 10.

[0044] In this invention, the precipitation reaction is preferably carried out in a water bath under static conditions, the temperature of the precipitation reaction is preferably 50°C, and the time is preferably 24 hours.

[0045] After the precipitation reaction is completed, the present invention preferably includes sequential filtration, washing, drying and grinding; the detergent used for washing is preferably deionized water; the drying temperature is preferably 100°C and the drying time is preferably 10 hours; the present invention does not impose any special limitations on the filtration, washing and grinding process, and any process known to those skilled in the art can be used.

[0046] After obtaining a metal mixture of magnesium, palladium and platinum, the present invention mixes the metal mixture of magnesium, palladium and platinum with activated carbon and calcines it to obtain the composite catalyst containing magnesium, palladium and platinum.

[0047] Before mixing, the present invention preferably includes pretreatment of the activated carbon; the pretreatment process preferably involves grinding, filtering, washing and drying the activated carbon sequentially; the present invention does not have any special limitations on the grinding process, and any process known to those skilled in the art can be used; the pore size of the filter screen used for filtering is preferably 1 mm; the detergent used for washing is preferably distilled water; the drying temperature is preferably 100-105°C; and the drying time is preferably 10-12 h.

[0048] The present invention does not impose any special limitations on the mixing process; any process known to those skilled in the art can be used.

[0049] In this invention, the preferred calcination process is to heat the temperature to 550°C at a heating rate of 30-35°C / 10 min and hold it at that temperature for 12 h; the most preferred process is to heat the temperature to 550°C at a heating rate of 30°C / 10 min and hold it at that temperature for 12 h.

[0050] The present invention also provides the application of the composite catalyst containing magnesium, palladium and platinum as described in the above technical solution or the composite catalyst containing magnesium, palladium and platinum prepared by the preparation method described in the above technical solution in the preparation of allyl alcohol block polyoxyethylene polyoxypropylene ether.

[0051] This invention also provides a method for preparing allyl alcohol block polyoxyethylene polyoxypropylene ether, comprising the following steps:

[0052] Allyl alcohol, potassium hydroxide and ethylene oxide are mixed and subjected to the first addition reaction to obtain allyl alcohol polyoxyethylene ether.

[0053] The allyl alcohol polyoxyethylene ether, a composite catalyst containing magnesium, palladium and platinum, and propylene oxide are mixed and subjected to a second addition reaction to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether.

[0054] The magnesium-, palladium-, and platinum-containing composite catalyst is the magnesium-, palladium-, and platinum-containing composite catalyst described in the above technical solution or the magnesium-, palladium-, and platinum-containing composite catalyst prepared by the preparation method described in the above technical solution.

[0055] In this invention, allyl alcohol, potassium hydroxide and ethylene oxide are mixed and subjected to a first addition reaction to obtain allyl alcohol polyoxyethylene ether.

[0056] In this invention, the molar ratio of allyl alcohol to ethylene oxide is preferably 1:(20-30), more preferably 1:(22-28), and most preferably 1:(24-26). In this invention, the mass percentage of potassium hydroxide in the allyl alcohol polyoxyethylene ether is preferably 1‰.

[0057] In this invention, the mixing process preferably involves placing allyl alcohol and potassium hydroxide in a reaction vessel, purging the vessel of nitrogen three times, heating to 100°C, and then adding ethylene oxide dropwise. In this invention, the dropping rate of the ethylene oxide is preferably 50–70 g / 10 min, more preferably 50 g / 10 min.

[0058] In this invention, the potassium hydroxide serves to accelerate the reaction, and the ethylene oxide is a reactant in the ring-opening reaction.

[0059] In this invention, the temperature of the first addition reaction is preferably 100-105°C, more preferably 101-104°C, and most preferably 102-103°C; the time of the first addition reaction is preferably based on the pressure inside the reactor remaining essentially constant; the criterion for determining that the pressure inside the reactor remains essentially constant is preferably a pressure decrease of no more than 0.02 MPa within 10 minutes.

[0060] After the first addition reaction is completed, the present invention preferably includes cooling and degassing. The present invention does not have any special limitations on the cooling and degassing process, and any process known to those skilled in the art can be used.

[0061] After obtaining allyl alcohol polyoxyethylene ether, the present invention mixes the allyl alcohol polyoxyethylene ether, a composite catalyst containing magnesium, palladium and platinum and propylene oxide, and carries out a second addition reaction to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether.

[0062] In this invention, the molar ratio of allyl alcohol to propylene oxide is preferably 1:(30-35), more preferably 1:(31-34), and most preferably 1:(32-33).

[0063] In this invention, the composite catalyst containing magnesium, palladium and platinum accounts for 1.5 to 2‰ of the mass percentage of the allyl alcohol block polyoxyethylene polyoxypropylene ether, more preferably 1.6 to 1.9‰, and most preferably 1.7 to 1.8‰.

[0064] In this invention, the mixing is preferably carried out by: adding allyl alcohol polyoxyethylene ether and a composite catalyst containing magnesium, palladium and platinum into a reaction vessel, replacing the nitrogen gas in the vessel three times, dehydrating for 40 min under a vacuum of ≥0.097 MPa and a temperature of 115-120°C, cooling, and then adding propylene oxide dropwise; in this invention, the dropwise rate of the propylene oxide is preferably 30-40 g / 10 min, more preferably 30-35 g / 10 min, and most preferably 35 g / 10 min.

[0065] In this invention, the temperature of the second addition reaction is preferably 100-105°C, more preferably 101-104°C, and most preferably 102-103°C; the time of the second addition reaction is preferably based on the pressure inside the reactor remaining essentially constant; the criterion for determining that the pressure inside the reactor remains essentially constant is preferably that the pressure decrease is no more than 0.02 MPa within 10 minutes.

[0066] After the second addition reaction is completed, the present invention preferably includes cooling and degassing. The present invention does not have any special limitations on the cooling and degassing process, and any process known to those skilled in the art can be used.

[0067] The following examples illustrate in detail the composite catalyst, its preparation method, and its application, as well as the preparation method of allyl alcohol block polyoxyethylene polyoxypropylene ether provided by the present invention. However, these examples should not be construed as limiting the scope of protection of the present invention.

[0068] Example 1

[0069] After placing 4.27g magnesium nitrate, 0.32g palladium nitrate and 0.16g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0070] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was filtered, and the filter cake was washed three times with deionized water. The resulting filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 70:20:10.

[0071] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0072] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 70:20:10, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 70:20:10.

[0073] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0074] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 70:20:10 were added to a 2.5L reactor. The reactor was purged with N2 three times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 96.8%, and the molecular distribution was 1.13.

[0075] Example 2

[0076] After placing 4.27g magnesium nitrate, 0.24g palladium nitrate and 0.245g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0077] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was then filtered, and the filter cake was washed three times with deionized water. The resulting filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 70:15:15.

[0078] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0079] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 70:15:15 evenly, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 70:15:15.

[0080] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0081] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 70:15:15 were added to a 2.5L reactor. The reactor was purged with N2 3 times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 96.4%, and the molecular distribution was 1.13.

[0082] Example 3

[0083] After placing 4.27g magnesium nitrate, 0.16g palladium nitrate and 0.33g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0084] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was filtered, and the filter cake was washed three times with deionized water. The resulting filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 70:10:20.

[0085] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0086] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 70:10:20, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 70:10:20.

[0087] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0088] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 70:10:20 were added to a 2.5L reactor. The reactor was purged with N2 three times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reactor was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 96.1%, and the molecular distribution was 1.15.

[0089] Example 4

[0090] After placing 1.22g magnesium nitrate, 1.11g palladium nitrate and 0.16g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0091] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was filtered, and the filter cake was washed three times with deionized water. The resulting filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 20:70:10.

[0092] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0093] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 20:70:10, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 20:70:10.

[0094] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0095] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 20:70:10 were added to a 2.5L reactor. The reactor was purged with N2 3 times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reactor was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 99.4%, and the molecular distribution was 1.08.

[0096] Example 5

[0097] After placing 0.61g magnesium nitrate, 1.11g palladium nitrate and 0.33g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0098] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was filtered, and the filter cake was washed three times with deionized water. The obtained filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 10:70:20.

[0099] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0100] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 10:70:20 evenly, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 10:70:20.

[0101] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0102] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 10:70:20 were added to a 2.5L reactor. The nitrogen in the reactor was replaced 3 times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain the allyl alcohol block polyoxyethylene polyoxypropylene ether product. The measured double bond retention rate was 99.5%, and the molecular distribution was 1.08.

[0103] Example 6

[0104] After placing 0.92g magnesium nitrate, 1.11g palladium nitrate and 0.245g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0105] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was filtered, and the filter cake was washed three times with deionized water. The resulting filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 15:70:15.

[0106] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0107] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 15:70:15 evenly, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 15:70:15.

[0108] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0109] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 15:70:15 were added to a 2.5L reactor. The reactor was purged with N2 3 times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 99.1%, and the molecular distribution was 1.11.

[0110] Example 7

[0111] After placing 1.22g magnesium nitrate, 0.16g palladium nitrate and 1.145g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0112] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was then filtered, and the filter cake was washed three times with deionized water. The resulting filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 20:10:70.

[0113] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0114] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 20:10:70, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 20:10:70.

[0115] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0116] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 20:10:70 were added to a 2.5L reactor. The reactor was purged with N2 3 times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 98.3%, and the molecular distribution was 1.11.

[0117] Example 8

[0118] After placing 0.92g magnesium nitrate, 0.24g palladium nitrate and 1.145g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0119] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was then filtered, and the filter cake was washed three times with deionized water. The resulting filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 15:15:70.

[0120] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0121] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 15:15:70, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 15:15:70.

[0122] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0123] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 15:15:70 were added to a 2.5L reactor. The nitrogen in the reactor was replaced 3 times. After dehydration at 115℃ under a vacuum of ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain the allyl alcohol block polyoxyethylene polyoxypropylene ether product. The measured double bond retention rate was 98.5%, and the molecular distribution was 1.11.

[0124] Example 9

[0125] After placing 0.61g magnesium nitrate, 0.32g palladium nitrate and 1.145g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0126] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was filtered, and the filter cake was washed three times with deionized water. The obtained filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 10:20:70.

[0127] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 2mm pore size filter screen, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0128] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 10:20:70, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 10:20:70.

[0129] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0130] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 10:20:70 were added to a 2.5L reactor. The reactor was purged with N2 3 times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reactor was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 98.9%, and the molecular distribution was 1.10.

[0131] Example 10

[0132] After placing 1.83g magnesium nitrate, 0.64g palladium nitrate and 0.49g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0133] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was filtered, and the filter cake was washed three times with deionized water. The resulting filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 30:40:30.

[0134] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0135] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 30:40:30 evenly, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 30:40:30.

[0136] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0137] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 30:40:30 were added to a 2.5L reactor. The reactor was purged with N2 3 times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain the allyl alcohol block polyoxyethylene polyoxypropylene ether product. The measured double bond retention rate was 98.1%, and the molecular distribution was 1.13.

[0138] Example 11

[0139] After placing 1.83g magnesium nitrate, 0.48g palladium nitrate and 0.65g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0140] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the dropwise addition. After the dropwise addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was filtered, and the filter cake was washed three times with deionized water. The obtained filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 30:30:40.

[0141] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0142] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 30:30:40, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to heat the mixture to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 30:30:40.

[0143] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0144] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 30:30:40 were added to a 2.5L reactor. The reactor was purged with N2 3 times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 98.1%, and the molecular distribution was 1.12.

[0145] Example 12

[0146] After placing 2.44g magnesium nitrate, 0.48g palladium nitrate and 0.49g platinum nitrate in a beaker, add 50mL distilled water and stir until completely dissolved to obtain a mixture;

[0147] The above mixture was added dropwise to 60 mL of 2% sodium carbonate solution in a water bath with magnetic stirring at 55℃. The pH was controlled at 9-10 in an alkaline environment using 2 mol / L sodium hydroxide solution during the addition. After the addition was completed, the mixture was stirred and mixed evenly for 1 hour, and then allowed to stand in a constant temperature water bath at 50℃ for 24 hours. The mixture was filtered, and the filter cake was washed three times with deionized water. The resulting filter cake was then dried in an oven at 100℃ for 10 hours to obtain a metal mixture of magnesium, palladium and platinum with a mass ratio of 40:30:30.

[0148] After thoroughly grinding the coconut shell activated carbon, filter out large particles using a 1mm sieve, wash the activated carbon powder twice with distilled water to remove impurities, and then dry it in a 100℃ oven for 12 hours to obtain activated carbon powder.

[0149] After mixing 4g of the activated carbon powder and 1g of a metal mixture of magnesium, palladium and platinum in a mass ratio of 40:30:30, the mixture was subjected to programmed temperature calcination. The programmed temperature calcination process was to raise the temperature to 550℃ at a heating rate of 30℃ / min and then hold it at that temperature for 12h to obtain a composite catalyst with a mass ratio of magnesium, palladium and platinum of 40:30:30.

[0150] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0151] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of a composite catalyst with a mass ratio of magnesium, palladium, and platinum of 40:30:30 were added to a 2.5L reactor. The reactor was purged with N2 3 times. After dehydration at 115℃ under a vacuum ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 97.9%, and the molecular distribution was 1.14.

[0152] Comparative Example 1

[0153] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0154] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of DMC bimetallic catalyst were added to a 2.5L reactor. The nitrogen in the reactor was replaced 3 times. After dehydration at 115℃ under a vacuum of ≥0.097MPa for 40min, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 96.5%, and the molecular distribution was 1.18.

[0155] Comparative Example 2

[0156] 116g of allyl alcohol and 1.88g of KOH catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. The temperature was raised to 100℃. 1760g of ethylene oxide was slowly added dropwise to the reactor (dropping rate 70g / 10min). After the ethylene oxide was added, the reaction was matured at 105℃ for 3 hours until the pressure basically stopped changing. The mixture was then cooled and degassed to obtain allyl alcohol polyoxyethylene ether.

[0157] 600g of the allyl alcohol polyoxyethylene ether and 2.56g of boron trifluoride diethyl ether catalyst were added to a 2.5L reactor. The N2 in the reactor was replaced 3 times. After dehydration at 115℃ under a vacuum of ≥0.097MPa, the reactor was cooled, and 1113g of propylene oxide was slowly added dropwise (dropping rate 40g / 10min). After the propylene oxide addition was complete, the reaction was matured at 105℃ for 3 hours until the pressure essentially stabilized. The reactor was then cooled and degassed to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The measured double bond retention rate was 97.1%, and the molecular distribution was 1.17.

[0158] Based on the double bond retention rate and molecular distribution data of the allyl alcohol block polyoxyethylene polyoxypropylene ethers prepared in Examples 1-12 and Comparative Examples 1-2, it can be seen that the composite catalyst used in this invention has a very good effect, and the effect is significantly improved compared with the catalyst used in the comparative examples. The allyl alcohol block polyoxyethylene polyoxypropylene ethers synthesized under this ratio have a high double bond retention rate and a narrow molecular distribution. In particular, the 70% palladium metal mixture has the highest double bond retention rate and the narrowest molecular distribution among similar products. At the same time, it is also the best in terms of its application performance.

[0159] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing allyl alcohol block polyoxyethylene polyoxypropylene ether, characterized in that, Includes the following steps: Allyl alcohol, potassium hydroxide and ethylene oxide are mixed and subjected to the first addition reaction to obtain allyl alcohol polyoxyethylene ether. The allyl alcohol polyoxyethylene ether, a composite catalyst containing magnesium, palladium and platinum, and propylene oxide are mixed and subjected to a second addition reaction to obtain allyl alcohol block polyoxyethylene polyoxypropylene ether. The composite catalyst containing magnesium, palladium and platinum is activated carbon and magnesium, palladium and platinum supported on the activated carbon; The total mass ratio of magnesium, palladium and platinum to activated carbon is 1:

4. The mass ratio of magnesium, palladium and platinum is (10~70):70:(10~70); Furthermore, the palladium accounts for 70% of the total mass of the magnesium, palladium, and platinum.

2. The preparation method according to claim 1, characterized in that, The preparation method of the composite catalyst containing magnesium, palladium and platinum includes the following steps: A mixture is prepared by mixing soluble magnesium salt, soluble palladium salt, soluble platinum salt and water. Under alkaline conditions, sodium carbonate solution and the mixture are mixed, a precipitation reaction is carried out, and then heat treatment is performed to obtain a metal mixture of magnesium, palladium and platinum. The magnesium, palladium and platinum metal mixture is mixed with activated carbon and calcined to obtain the magnesium, palladium and platinum composite catalyst.

3. The preparation method according to claim 2, characterized in that, The calcination process is as follows: the temperature is increased to 550℃ at a rate of 30℃ / 10min, and then held for 12 hours.

4. The preparation method according to claim 1, characterized in that, The molar ratio of allyl alcohol to ethylene oxide is 1:(20~30). The potassium hydroxide accounts for 1‰ of the mass percentage of the allyl alcohol polyoxyethylene ether.

5. The preparation method according to claim 1 or 4, characterized in that, The temperature of the first addition reaction is 100~105℃.

6. The preparation method according to claim 1, characterized in that, The molar ratio of allyl alcohol to propylene oxide is 1:(30~35). The composite catalyst containing magnesium, palladium, and platinum accounts for 1.5 to 2‰ of the mass of the allyl alcohol block polyoxyethylene polyoxypropylene ether.

7. The preparation method according to claim 1 or 6, characterized in that, The temperature for the second addition reaction is 100~105℃.

Citation Information

Patent Citations

  • A mixed-metal catalysts for alkylene oxide addition and process for preparing the same