Perfluorosulfonic acid resin slurry and method of making, proton exchange membrane

The perfluorosulfonic acid resin slurry was prepared by high-temperature and high-pressure treatment and homogenization technology, which solved the problems of uneven molecular weight and uneven dispersion of perfluorosulfonic acid resin, and improved the mechanical strength and durability of proton exchange membranes.

CN117447725BActive Publication Date: 2026-11-20STATE POWER INVESTMENT CORP HYDROGEN ENERGY CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311393277.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-25
Publication Date
2026-11-20
Estimated Expiration
2043-10-25

AI Technical Summary

Technical Problem

In existing technologies, the molecular weight of perfluorosulfonic acid resin is not uniform and the dispersion is uneven, resulting in poor mechanical strength of the proton exchange membrane.

Method used

Perfluorosulfonate resin is dispersed in a solvent by high temperature and high pressure treatment, which de-entangles and stretches the chain segments. Then, it is acidified and freeze-dried, and then dissolved and homogenized at room temperature and pressure to prepare a perfluorosulfonate resin slurry with uniform molecular weight and uniform dispersion.

Benefits of technology

It improves the mechanical strength, swelling resistance, and crystallinity of the proton exchange membrane, thereby enhancing the membrane's durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004513142310000121
    Figure BDA0004513142310000121
  • Figure BDA0004513142310000131
    Figure BDA0004513142310000131
Patent Text Reader

Abstract

The application provides a perfluorosulfonic acid resin slurry, a preparation method and a proton exchange membrane. The preparation method comprises the following steps: mixing a first part of water, a first organic solvent and a perfluorosulfonate resin to obtain a first resin dispersion liquid, drying the first resin dispersion liquid to obtain a first resin powder, mixing the first resin powder and an acid aqueous solution, and sequentially performing water washing and freeze drying to obtain a perfluorosulfonic acid resin; mixing a second part of water, a second organic solvent and the perfluorosulfonic acid resin to obtain a second resin dispersion liquid, and performing homogenization treatment on the second resin dispersion liquid to obtain the perfluorosulfonic acid resin slurry, wherein the temperature of the first mixing is 90-200 DEG C, the pressure is 3-30 MPa, the temperature of the third mixing is 20-40 DEG C, and the pressure is 0.1-0.11 MPa. The perfluorosulfonic acid resin slurry prepared by the application has uniform resin molecular weight and uniform dispersion, and can improve the mechanical strength, crystallinity, anti-swelling property and durability of the proton exchange membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fuel cell technology, and more specifically, to a perfluorosulfonic acid resin slurry and its preparation method, and a proton exchange membrane. Background Technology

[0002] A proton exchange membrane fuel cell (PEMFC) is a power generation device that directly converts the chemical energy stored in hydrogen and oxygen into electrical energy through electrode chemical reactions. As the core component of a polymer electrolyte fuel cell, the proton exchange membrane determines the fuel cell's performance and lifespan. An ideal PEMFC should possess characteristics such as high proton conductivity, low gas permeability, high mechanical strength, good chemical stability, and low cost.

[0003] For the preparation of selectively permeable resins for proton exchange membranes, perfluorosulfonic acid resins are currently the most commercially successful due to their good stability and long lifespan. Perfluorosulfonic acid resins are typically prepared by copolymerizing perfluorovinyl ethers and tetrafluoroethylene, then formulated into a slurry, and finally cast to obtain the proton exchange membrane.

[0004] To improve the strength of proton exchange membranes, one method is to dope the perfluorosulfonic acid resin solution with additives. For example, in patent CN112803051A, lignin sulfonic acid and polyvinyl alcohol are added to the perfluorosulfonic acid resin solution; in patent CN101071873A, polymer ultrashort fibers are mixed into the resin dispersion. However, the addition of dopants affects the exchange equivalent and crystallinity of the resin, thus affecting the conductivity and uniformity of the proton exchange membrane. In addition, patent CN116231018A first prepares a fiber mat by electrospinning, and then coats the perfluorosulfonic acid resin solution onto the electrospun fiber mat to prepare a composite proton exchange membrane; in patent CN114094154A, a polystyrene fiber membrane is first prepared by electrospinning, and then the fiber membrane is cold-pressed and sulfonated to obtain a sulfonated polystyrene membrane, which serves as a reinforcing layer for the composite proton exchange membrane to enhance its strength. However, under the above production process conditions, the molecular weight distribution of perfluorosulfonic acid resin is still uneven, the solute in the perfluorosulfonic acid resin dispersion is still unevenly dispersed, and the mechanical strength of the proton exchange membrane is still poor. Summary of the Invention

[0005] The main objective of this invention is to provide a perfluorosulfonic acid resin slurry and its preparation method, as well as a proton exchange membrane, to solve the problems of uneven molecular weight, uneven dispersion, and poor mechanical strength of the proton exchange membrane in the prior art.

[0006] To achieve the above objectives, according to one aspect of the present invention, a method for preparing a perfluorosulfonic acid resin slurry is provided, comprising the following steps: Step S1, mixing a first portion of water, a first organic solvent, and a perfluorosulfonate resin to obtain a first resin dispersion; Step S2, drying the first resin dispersion to obtain a first resin powder, then mixing it with an acidic aqueous solution, and sequentially washing with water and freeze-drying to obtain a perfluorosulfonic acid resin; Step S3, mixing a second portion of water, a second organic solvent, and a perfluorosulfonic acid resin to obtain a second resin dispersion; Step S4, homogenizing the second resin dispersion to obtain a perfluorosulfonic acid resin slurry; wherein the temperature of the first mixing is 90–200°C and the pressure is 3–30 MPa; the temperature of the third mixing is 20–40°C and the pressure is 0.1–0.11 MPa.

[0007] Furthermore, the temperature of the first mixture is greater than the temperature of the drying process, the temperature of the drying process is greater than the temperature of the second mixture, and the temperature of the second mixture is greater than the temperature of the third mixture.

[0008] Further, in step S1, the perfluorosulfonate resin is potassium perfluorosulfonate resin and / or sodium perfluorosulfonate resin; and / or, the weight average molecular weight of the perfluorosulfonate resin is 500,000 to 9,000,000; and / or, the weight percentage of the perfluorosulfonate resin in the first resin dispersion is 5% to 30%; and / or, the first organic solvent is an alcohol solvent; preferably, the first organic solvent is two or more of methanol, ethanol, n-propanol and isopropanol; and / or, the mass ratio of the first portion of water to the first organic solvent is (1 to 5):1, and the first mixing time is 6 to 18 hours; and / or, the first mixing is carried out in an inert gas atmosphere, the inert gas being nitrogen and / or argon.

[0009] Further, in step S2, the acid aqueous solution is an aqueous solution of sulfuric acid and / or an aqueous solution of nitric acid; preferably, the mass concentration of the acid aqueous solution is 20-55%; more preferably, the mass ratio of the acid aqueous solution to the first resin powder is (5-10):1.

[0010] Further, in step S2, the drying temperature is 50–150°C and the time is 10–48 h; and / or, the second mixing temperature is 50–120°C and the time is 12–30 h; and / or, the freeze-drying temperature is -70–-90°C and the time is 24–120 h.

[0011] Further, in step S3, the mass ratio of perfluorosulfonic acid resin to the second portion of water is 1:(5-35); and / or, the second organic solvent is an alcohol solvent; preferably, the second organic solvent is two or more of methanol, ethanol, n-propanol, and isopropanol; and / or, the mass ratio of the second portion of water to the second organic solvent is (2-5):1, preferably (2.5-4):1.

[0012] Further, in step S3, the third mixing time is 17–32 h; and / or, the third mixing is carried out in an inert gas atmosphere, wherein the inert gas is nitrogen and / or argon.

[0013] Further, in step S4, the homogenization treatment is one or more of ultrasonication, shearing, stirring, grinding and high-pressure impact; preferably, the homogenization treatment is high-pressure impact; and / or, the temperature of the homogenization treatment is 25 to 40°C; and / or, when the homogenization treatment is high-pressure impact, the pressure of the homogenization treatment is 500 to 1725 bar.

[0014] According to another aspect of the present invention, a perfluorosulfonic acid resin slurry is provided, which is obtained by the above preparation method.

[0015] According to another aspect of the present invention, a proton exchange membrane is provided, which is prepared from the above-mentioned perfluorosulfonic acid resin slurry.

[0016] The technical solution of this invention involves first subjecting the perfluorosulfonate resin to high-temperature and high-pressure treatment to disperse it in a solvent. During this process, the entangled molecular chains in the resin absorb sufficient energy to disentangle, transforming into a more thermodynamically stable state, and the chain segments extend. The extended perfluorosulfonate resin is then acidified through ion exchange to obtain perfluorosulfonic acid resin. Next, the perfluorosulfonic acid resin is dissolved at room temperature and pressure to obtain a dispersion. This dissolution process has low equipment requirements and does not introduce impurities. Finally, the dispersion is homogenized to prepare a perfluorosulfonic acid resin slurry with uniform molecular weight and good dispersion effect.

[0017] The perfluorosulfonic acid resin slurry prepared by this invention has a uniform molecular weight of resin and uniform solute dispersion. When this perfluorosulfonic acid resin slurry is used in proton exchange membranes, it can significantly improve the mechanical strength and crystallinity of the proton exchange membrane, while also enhancing its anti-swelling properties and durability. Detailed Implementation

[0018] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0019] It should be noted that the terms "first," "second," etc., in the specification and claims of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate to describe embodiments of the invention. It should also be noted that the first portion of water and the second portion of water do not differ in composition or properties.

[0020] As described in the background section of this invention, existing technologies suffer from problems such as non-uniform molecular weight, uneven dispersion, and poor mechanical strength of proton exchange membranes in perfluorosulfonic acid resins. To address these issues, in a typical embodiment of this invention, a method for preparing perfluorosulfonic acid resin slurry is provided, comprising the following steps: Step S1, a first mixing of perfluorosulfonate resin, organic solvent, and water to obtain a first resin dispersion; drying the first resin dispersion to obtain a first resin powder, then mixing it with an acidic aqueous solution, followed by sequential washing with water and freeze-drying to obtain perfluorosulfonic acid resin; a third mixing of perfluorosulfonic acid resin, organic solvent, and water to obtain a perfluorosulfonic acid resin dispersion; homogenizing the perfluorosulfonic acid resin dispersion to obtain a perfluorosulfonic acid resin slurry, wherein the temperature of the first mixing is 90–200°C and the pressure is 3–30 MPa; the temperature of the third mixing is 20–40°C and the pressure is 0.1–0.11 MPa.

[0021] During their research, the inventors unexpectedly discovered that perfluorosulfonic acid resins, as polymers, do not have a fixed molecular weight but are mixtures of homologues with different molecular weights. Due to the limitations of the polymerization reaction itself, commercially available perfluorosulfonic acid resins generally have a wide molecular weight distribution. Even after removing unreacted monomers and low-molecular-weight products during the product purification stage, the overall molecular weight distribution of perfluorosulfonic acid resins is still not ideal. This disordered molecular weight distribution of perfluorosulfonic acid resins not only makes resin testing and characterization difficult but also results in poor physical and mechanical properties and processing difficulties, further leading to poor mechanical properties and swelling resistance of the proton exchange membranes prepared from the resin. The inventors unexpectedly discovered that by specifically selecting and treating the resin raw materials and resin solutions, the molecular weight, molecular weight distribution, and crystallinity of perfluorosulfonic acid resins can be improved, further enhancing the mechanical properties and swelling resistance of the proton exchange membranes.

[0022] This invention first subjects perfluorosulfonate resin to high-temperature and high-pressure treatment to disperse it in a solvent. During this process, the entangled molecular chains in the resin absorb sufficient energy to disentangle, becoming more thermodynamically stable, with extended chain segments. Furthermore, perfluorosulfonate resin is neutral, and the solution has low corrosiveness to equipment during the high-temperature dissolution process, thus requiring less sophisticated equipment. Next, acidification treatment is performed, followed by water washing and freeze-drying to thoroughly remove impurities from the resin surface and generate perfluorosulfonate resin through ion exchange. The perfluorosulfonate resin is then dissolved at low temperature and normal pressure to prepare a homogeneous and stable resin dispersion. Following this, homogenization treatment is performed. Under the influence of cavitation, shearing, and impact, the long molecular chains of the resin further disentangle or break, resulting in a decrease in molecular weight, closer chain lengths, and a narrower molecular weight distribution, while maintaining the resin's ion exchange equivalent (EW value). Large resin particles are broken down and dispersed into uniform microparticles, improving the dispersibility of the resin in solution, resulting in a homogenized perfluorosulfonate resin slurry. The homogenization treatment can be performed using conventional methods. Meanwhile, conventional perfluorosulfonic acid resins require high temperature and high pressure to dissolve, and their inherent acidity can cause significant corrosion to equipment. However, the perfluorosulfonic acid resin obtained by this invention has a more uniform molecular weight and can be dissolved at low temperature and normal pressure, reducing the requirements for equipment and improving the safety of the perfluorosulfonic acid resin dissolution process.

[0023] The perfluorosulfonic acid resin slurry prepared by the method of this invention has resin chain lengths that are close together, a narrow molecular weight distribution, and uniform solute dispersion. When this perfluorosulfonic acid resin slurry is applied, especially to proton exchange membranes, it can improve the mechanical strength, swelling resistance, crystallinity, and durability of the proton exchange membrane. Furthermore, this invention innovatively introduces the concept of homogenization. Through a series of cavitation, shearing, and impact effects, the long resin chains are broken down, reducing the resin molecular weight and narrowing the molecular weight distribution. This breaks down large resin particles into microparticles, improving the resin's dispersion effect in solution.

[0024] In order to enable the resin to maintain a more stable thermodynamic unfolded and stretched state after obtaining sufficient energy, so as to facilitate subsequent processing, in a preferred embodiment, the temperature of the first mixing is higher than the drying temperature, the drying temperature is higher than the second mixing temperature, and the second mixing temperature is higher than the third mixing temperature, thereby further reducing pre-film crystallization and further reducing processing difficulty.

[0025] In a preferred embodiment, in step S1, the perfluorosulfonate resin is potassium perfluorosulfonate resin and / or sodium perfluorosulfonate resin. The production process requirements for the above-mentioned perfluorosulfonate resin are lower, the production cost is lower, and the safety is higher. To further improve the solution and resin dissolution conditions, and to ensure more complete contact and dissolution of the resin and solvent during the dissolution process, the weight-average molecular weight of the perfluorosulfonate resin is 500,000 to 9,000,000; and / or, the perfluorosulfonate resin accounts for 5% to 30% of the weight of the first resin dispersion; and / or, the first organic solvent is an alcohol solvent; preferably, the first organic solvent is two or more of methanol, ethanol, n-propanol, and isopropanol; and / or, the mass ratio of the first portion of water to the first organic solvent is (1 to 5):1.

[0026] To further ensure complete dissolution of the perfluorosulfonate resin, in a preferred embodiment, the first mixing time in step S1 is 6 to 18 hours; and / or, the first mixing is carried out in an inert gas atmosphere, wherein the inert gas is nitrogen and / or argon.

[0027] For the purpose of further making the ion exchange reaction more complete, in a preferred embodiment, in step S2, the acid aqueous solution is an aqueous solution of sulfuric acid and / or an aqueous solution of nitric acid; preferably, the mass concentration of the acid aqueous solution is 20-55%; more preferably, the mass ratio of the acid aqueous solution to the first resin powder is (5-10):1.

[0028] To ensure the perfluorosulfonate resin molecular chains remain extended while facilitating thorough removal of solvent from the perfluorosulfonate resin dispersion, in a preferred embodiment, step S2 involves drying at a temperature of 50–150°C for 10–48 hours. Preferably, the drying process includes a first drying and a second drying. The first drying is carried out at 70–80°C for 12–15 hours, and the second drying is carried out at 80–95°C for 15–24 hours. This invention preferably divides the drying process into two stages, with the first stage conducted at a relatively lower temperature and the second stage at a relatively higher temperature. Under these conditions, solvent and water in the potassium perfluorosulfonate resin can be removed more thoroughly, further reducing resin loss during subsequent acidification processes and thus improving the recovery rate.

[0029] In order to make the ion exchange reaction more complete, in a preferred embodiment, in step S2, the temperature of the second mixing is 50-120°C and the time is 12-30h.

[0030] For the purpose of more thoroughly removing solvent and water, in a preferred embodiment, in step S2, the freeze-drying temperature is -70 to -90°C and the time is 24 to 120 hours.

[0031] To further improve solution conditions and enable the perfluorosulfonic acid resin to come into more complete contact with the solvent and dissolve more fully during the dissolution process, in a preferred embodiment, in step S3, the mass ratio of the perfluorosulfonic acid resin to the second portion of water is 1:(5-35); the second organic solvent is an alcohol solvent; and / or, preferably, the second organic solvent is two or more of methanol, ethanol, n-propanol, and isopropanol; and / or, the mass ratio of the second portion of water to the second organic solvent is (2-5):1, preferably (2.5-4):1.

[0032] In order to further improve the dissolution conditions of perfluorosulfonic acid resin and further reduce equipment requirements and production costs during the production process, in a preferred embodiment, the third mixing time in step S3 is 17-32 hours; and / or, the third mixing is carried out in an inert gas atmosphere, wherein the inert gas is nitrogen and / or argon.

[0033] To break down large solute particles into more uniform microparticles and further improve the dispersion effect of the resin dispersion, in a preferred embodiment, in step S4, the homogenization treatment is one or more of ultrasonication, shearing, stirring, grinding, and high-pressure impaction; preferably, the homogenization treatment is high-pressure impaction; and / or, the homogenization treatment temperature is 25–40°C; and / or, when the homogenization treatment is high-pressure impaction, the homogenization treatment pressure is 500–1725 bar. Under the above conditions, the resin molecular weight can be further reduced and the uniformity of resin molecular weight can be improved, thereby further improving the dispersion effect of the resin in the solution, and at the same time further improving the physical and mechanical strength and anti-swelling properties of the resin. Preferably, a microfluidic homogenizer, ultrasonicator, high-speed mixer, grinding pump, and shear emulsifier are used for homogenization treatment.

[0034] In another typical embodiment of the present invention, a perfluorosulfonic acid resin slurry is also provided, obtained by the above preparation method. The perfluorosulfonic acid resin slurry obtained by the preparation method of the present invention is free of impurities, has good solute dispersibility, and the resin has a uniform molecular weight, narrow molecular weight distribution, and its exchange capacity is not adversely affected.

[0035] In another typical embodiment of the present invention, a proton exchange membrane is also provided, prepared from the above-mentioned perfluorosulfonic acid resin slurry, for example, prepared by a casting method using the above-mentioned perfluorosulfonic acid resin slurry. The proton exchange membrane prepared from the perfluorosulfonic acid resin slurry of the present invention exhibits easier crystallization, higher mechanical strength, better anti-swelling properties, and stronger durability after heat treatment, and its conductivity is not adversely affected. The casting method described above is understandable to those skilled in the art and will not be elaborated upon here.

[0036] Typically, but not limitingly, in step S1, the temperature of the first mixture is 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, or any two of these values; the pressure of the first mixture is 3 MPa, 4 MPa, 6 MPa, 8 MPa, 10 MPa, 12 MPa, 14 MPa, 16 MPa, 18 MPa, 20 MPa, 22 MPa, 24 MPa, 26 MPa, 28 MPa, 30 MPa, or any two of these values; and the time of the first mixture is 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, or any two of these values.

[0037] Typically, but not limitingly, in step S1, the weight-average molecular weight of the perfluorosulfonate resin is a range of 500,000, 1,000,000, 2,000,000, 3,000,000, 4,000,000, 5,000,000, 6,000,000, 7,000,000, 8,000,000, or any two of these values; and the weight percentage of the perfluorosulfonate resin in the first resin dispersion is 5%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, or any two of these values.

[0038] Typically, but not limitingly, in step S2, the drying temperature is 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, or any two of these values; the drying time is 10h, 12h, 14h, 15h, 16h, 17h, 18h, 20h, 22h, 24h, 26h, 28h, 30h, 32h, 34h, 36h, 38h, 40h, 42h, 46h, 48h, or any two of these values.

[0039] Typically, but not limitingly, in step S2, the temperature of the second mixing is 50°C, 60°C, 70°C, 80°C, 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C, 99°C, 100°C, 110°C, 120°C, or any two of these values; the time of the second mixing is 12h, 14h, 16h, 18h, 20h, 22h, 24h, 26h, 28h, 30h, or any two of these values.

[0040] Typically, but not limitingly, in step S2, the mass concentration of the acid aqueous solution is 20%, 25%, 30%, 35%, 38%, 40%, 45%, 50%, 55%, or any two of these values; the mass ratio of the acid aqueous solution to the first resin powder is 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, or any two of these values.

[0041] Typically, but not limitingly, in step S2, the freeze-drying temperature is -70℃, -72℃, -74℃, -76℃, -78℃, -80℃, -82℃, -84℃, -86℃, -88℃, -90℃, or any two of these values; the freeze-drying time is 24h, 26h, 28h, 30h, 40h, 50h, 60h, 70h, 80h, 90h, 100h, 110h, 120h, or any two of these values.

[0042] Typically, but not limitingly, in step S3, the temperature of the third mixture is 20°C, 22°C, 24°C, 25°C, 26°C, 28°C, 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, or any two of these values; the pressure of the third mixture is 0.1 MPa, 0.101 MPa, 0.102 MPa, 0.104 MPa, 0.105 MPa, 0.106 MPa, 0.108 MPa, 0.11 MPa, or any two of these values; and the time of the third mixture is 17 h, 18 h, 20 h, 22 h, 24 h, 25 h, 26 h, 28 h, 30 h, 32 h, or any two of these values.

[0043] Typically, but not limitingly, in step S4, the homogenization temperature is 25°C, 26°C, 28°C, 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, or any two of these values; when the homogenization is performed by high-pressure impact, the homogenization pressure is 500 bar, 600 bar, 700 bar, 800 bar, 900 bar, 1000 bar, 1100 bar, 1200 bar, 1300 bar, 1325 bar, 1400 bar, 1500 bar, 1600 bar, 1700 bar, 1725 bar, or any two of these values.

[0044] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in this application.

[0045] Example 1

[0046] S1. Weigh out the following components according to the following formula: potassium perfluorosulfonate resin (weight average molecular weight approximately 1 million), deionized water, ethanol, isopropanol, and n-propanol in the first organic solvent at a weight percentage of 20% in the first resin dispersion, a water-to-first organic solvent mass ratio of 5:1, and an ethanol:isopropanol:n-propanol mass percentage of 62.5:25:12.5. Add these components sequentially to a 2L reactor and seal the reactor tightly. Then, pressurize the reactor with nitrogen gas to ensure there is no leakage. After that, release the gas. Repeat the gas filling and releasing operation 5 times to displace the air in the reactor. Start stirring and heating the reactor. After the temperature inside the reactor reaches 190°C, control the pressure inside the reactor to 3MPa. Maintain the temperature and stir for 12 hours. Then, stop heating and wait for the temperature inside the reactor to cool to 20°C before opening the pressure relief valve to release the pressure.

[0047] S2, open the reactor, transfer the product to a vacuum oven and vacuum dry for 34 hours. Control the temperature at 75℃ for the first 14 hours and at 90℃ for the next 20 hours. Then collect the dried powder. Weigh a 50% sulfuric acid aqueous solution according to a sulfuric acid aqueous solution to powder mass ratio of 5:1. Add the dried powder to the sulfuric acid aqueous solution and stir for 24 hours, controlling the temperature of the mixed solution at 95℃ during stirring. Take out the acidified resin and wash it with ultrapure water until the washing solution is neutral. Then, freeze-dry the resin at -80℃ for 120 hours to obtain perfluorosulfonic acid resin.

[0048] S3. Weigh the second part of water according to the mass ratio of perfluorosulfonic acid resin to the second part of water of 1:5. Weigh the second part of organic solvent according to the mass ratio of the second part of water to the second organic solvent of 3:1. Weigh the ethanol, isopropanol and n-propanol according to the mass ratio of ethanol, isopropanol and n-propanol of 3:2:1. Stir the mixed solution of perfluorosulfonic acid resin, water, ethanol, isopropanol and n-propanol at 0.101MPa, nitrogen atmosphere protection and 25°C for 25h to obtain perfluorosulfonic acid resin dispersion.

[0049] S4. The perfluorosulfonic acid resin dispersion was treated using a microfluidic homogenizer at a temperature of 30°C and a pressure of 1325 bar. After three cycles, a perfluorosulfonic acid resin slurry was obtained.

[0050] S5. First, lay a base film. Pour the perfluorosulfonic acid resin slurry into the front of the scraper through the hopper of the container. After controlling the gap between the scraper and the base film, move the scraper forward to scrape out a wet film. After covering the reinforcing layer, scrape out a wet film again to make it cast and form. Dry it to obtain a proton exchange membrane.

[0051] Example 2

[0052] S1. Weigh out the following components according to the following ratios: potassium perfluorosulfonate resin (weight average molecular weight of 5 million), deionized water, ethanol, isopropanol, and n-propanol. These components are added sequentially to a 2L reactor. The reactor is then sealed and secured. Nitrogen gas is introduced to maintain pressure, and after ensuring no leakage, the gas is released. This process is repeated to completely replace the air inside the reactor. The reactor is then stirred and heated. Once the temperature inside the reactor reaches 150°C, the pressure inside the reactor is controlled at 16MPa. The temperature is maintained and the reactor is stirred for 12 hours. Heating is then stopped. After the temperature inside the reactor cools to 20°C, the pressure relief valve is opened to release the pressure.

[0053] S2, open the reactor, transfer the product to a vacuum oven and vacuum dry for 34 hours. Control the temperature at 75℃ for the first 14 hours and at 90℃ for the next 20 hours. Then collect the dried powder. Weigh a 38% sulfuric acid aqueous solution according to a sulfuric acid aqueous solution to powder mass ratio of 8:1. Add the dried powder to the sulfuric acid aqueous solution and stir for 18 hours, controlling the temperature of the mixed solution at 98℃ during stirring. Take out the acidified resin and wash it with ultrapure water until the washing solution is neutral. Then, freeze-dry the resin at -85℃ for 100 hours to obtain perfluorosulfonic acid resin.

[0054] S3, weigh the second part of water according to the mass ratio of perfluorosulfonic acid resin to the second part of water of 1:20, weigh the second part of organic solvent according to the mass ratio of the second part of water to the second organic solvent of 3.3:1, weigh the ethanol, isopropanol and n-propanol according to the mass ratio of 1:1:1, and stir the mixed solution of perfluorosulfonic acid resin, water, ethanol, isopropanol and n-propanol at 0.105MPa, nitrogen atmosphere and 25℃ for 25h to obtain perfluorosulfonic acid resin dispersion;

[0055] S4. The perfluorosulfonic acid resin dispersion was treated using a microfluidic homogenizer at a temperature of 30°C and a pressure of 1325 bar. After three cycles, a perfluorosulfonic acid resin slurry was obtained.

[0056] S5. First, lay a base film. Pour the perfluorosulfonic acid resin slurry into the front of the scraper through the hopper of the container. After controlling the gap between the scraper and the base film, move the scraper forward to scrape out a wet film. After covering the reinforcing layer, scrape out a wet film again to make it cast and form. Dry it to obtain a proton exchange membrane.

[0057] Example 3

[0058] The difference from Example 2 is as follows:

[0059] The perfluorosulfonate potassium resin has a weight percentage of 30% in the first resin dispersion, the mass ratio of water to the first organic solvent is 5:1, the first organic solvent is ethanol and isopropanol with a mass percentage of ethanol:isopropanol of 80:20, and the weight average molecular weight of the perfluorosulfonate potassium resin is 9 million.

[0060] Example 4

[0061] The difference from Example 2 is as follows:

[0062] Sodium perfluorosulfonate resin comprises 5% by weight in the first resin dispersion, the mass ratio of water to the first organic solvent is 1:1, the first organic solvent is methanol, ethanol, n-propanol and isopropanol and the mass percentage of methanol:ethanol:n-propanol:isopropanol is 5:55:25:15, and the weight average molecular weight of sodium perfluorosulfonate resin is approximately 500,000.

[0063] Example 5

[0064] The only difference from Example 2 is:

[0065] In step S1, potassium perfluorosulfonate resin, deionized water, ethanol, isopropanol, and n-propanol are added sequentially to a 2L reactor. The reactor is then sealed and secured, and argon gas is introduced to maintain pressure. After ensuring there is no leakage, the gas is released. The process of introducing and releasing gas is repeated to completely replace the air inside the reactor. The reactor is then stirred and heated. Once the temperature inside the reactor reaches 200°C, the pressure inside the reactor is controlled at 3MPa. The temperature is maintained and the reactor is stirred for 18 hours. Heating is then stopped, and the pressure is released after the temperature inside the reactor cools down to 25°C by opening the pressure relief valve.

[0066] Example 6

[0067] The only difference from Example 2 is:

[0068] In S1, potassium perfluorosulfonate resin (weight average molecular weight of 5 million), deionized water, ethanol, isopropanol, and n-propanol are added sequentially to a 2L reactor. The reactor is then sealed and secured, and argon gas is introduced to maintain pressure. After ensuring there is no leakage, the gas is released. The gas introduction and release process is repeated to completely replace the air in the reactor. The reactor is then stirred and heated. Once the temperature inside the reactor reaches 90°C, the pressure inside the reactor is controlled at 30MPa. The temperature is maintained and the reactor is stirred for 6 hours. Heating is then stopped, and the temperature inside the reactor is allowed to cool to 28°C before the pressure relief valve is opened to release the pressure.

[0069] Example 7

[0070] The difference from Example 2 is as follows:

[0071] In S2, a 55% sulfuric acid aqueous solution is weighed according to a mass ratio of acid aqueous solution to powder of 5:1. The dried powder is added to the sulfuric acid aqueous solution and stirred for 12 hours. The temperature of the mixed solution is controlled at 50℃ during stirring.

[0072] Example 8

[0073] The only difference from Example 2 is that:

[0074] In S2, a 20% nitric acid aqueous solution is weighed according to a sulfuric acid aqueous solution to powder mass ratio of 10:1. The dried powder is added to the nitric acid aqueous solution and stirred for 30 hours. During stirring, the temperature of the mixed solution is controlled at 120℃.

[0075] Example 9

[0076] The only difference from Example 2 is:

[0077] In S2, the reactor was opened, and the product was transferred to a vacuum oven for vacuum drying for 27 hours. The temperature was controlled at 80°C for the first 12 hours and at 95°C for the next 15 hours. The dried powder was then collected. A 38% sulfuric acid aqueous solution was weighed according to a sulfuric acid aqueous solution to powder mass ratio of 8:1. The dried powder was added to the sulfuric acid aqueous solution and stirred for 18 hours, while the temperature of the mixed solution was controlled at 98°C during stirring. The acidified resin was then removed and washed with ultrapure water until the washing solution was neutral. Next, the resin was freeze-dried at -90°C for 120 hours to obtain perfluorosulfonic acid resin.

[0078] Example 10

[0079] The only difference from Example 2 is:

[0080] In step S2, the reactor was opened, and the product was transferred to a vacuum oven for vacuum drying for 39 hours. The temperature was controlled at 70°C for the first 15 hours and at 80°C for the next 24 hours. The dried powder was then collected. A 38% sulfuric acid aqueous solution was weighed according to a sulfuric acid aqueous solution to powder mass ratio of 8:1. The dried powder was added to the sulfuric acid aqueous solution and stirred for 18 hours, while the temperature of the mixed solution was controlled at 98°C. The acidified resin was then removed and washed with ultrapure water until the washing solution was neutral. Next, the resin was freeze-dried at -70°C for 24 hours to obtain perfluorosulfonic acid resin.

[0081] Example 11

[0082] The only difference from Example 2 is:

[0083] S3. Weigh the second part of water according to a mass ratio of perfluorosulfonic acid resin to water of the second part of water of 1:5. Weigh the second organic solvent according to a mass ratio of water of the second part of water to the second organic solvent of 4:1. Weigh ethanol and n-propanol according to a mass ratio of ethanol and n-propanol of 1:1. Stir the mixed solution of perfluorosulfonic acid resin, water, ethanol and n-propanol at 0.1 MPa, nitrogen atmosphere and 40°C for 17 h to obtain perfluorosulfonic acid resin dispersion.

[0084] Example 12

[0085] The only difference from Example 2 is:

[0086] S3. Weigh the second part of water according to a mass ratio of perfluorosulfonic acid resin to water of the second part of water of 1:5. Weigh the second organic solvent according to a mass ratio of water of the second part of water to the second organic solvent of 2.5:1. Weigh methanol, ethanol, isopropanol and n-propanol according to a mass ratio of 1:1:1:1. Stir the mixed solution of perfluorosulfonic acid resin, water, methanol, ethanol, isopropanol and n-propanol at 0.11 MPa, nitrogen atmosphere and 20°C for 32 h to obtain perfluorosulfonic acid resin dispersion.

[0087] Example 13

[0088] The only difference from Example 2 is:

[0089] S3. Weigh the second part of water according to a mass ratio of perfluorosulfonic acid resin to water of the second part of water of 1:5. Weigh the second organic solvent according to a mass ratio of water of the second part of water to the second organic solvent of 5:1. Weigh ethanol, isopropanol and n-propanol according to a mass ratio of 3:1:1. Stir the mixed solution of perfluorosulfonic acid resin, water, ethanol, isopropanol and n-propanol at 0.102 MPa, argon atmosphere and 40°C for 25 h to obtain perfluorosulfonic acid resin dispersion.

[0090] Example 14

[0091] The only difference from Example 2 is:

[0092] In S3, the second part of water is weighed according to a mass ratio of perfluorosulfonic acid resin to water of the second part of water of 1:35, the second organic solvent is weighed according to a mass ratio of water of the second part of water to the second organic solvent of 2:1, and ethanol, isopropanol and n-propanol are weighed according to a mass ratio of 1:3:1. The mixed solution of perfluorosulfonic acid resin, water, ethanol, isopropanol and n-propanol is stirred for 25 h in an argon atmosphere at 0.108 MPa to obtain a perfluorosulfonic acid resin dispersion.

[0093] Example 15

[0094] The only difference from Example 2 is that:

[0095] S4. The perfluorosulfonic acid resin dispersion was treated with an ultrasonic instrument at a temperature of 40°C for 30 minutes to obtain a perfluorosulfonic acid resin slurry.

[0096] Example 16

[0097] The only difference from Example 2 is:

[0098] S4. The perfluorosulfonic acid resin dispersion was treated using a high-speed mixer at a temperature of 25°C and a speed of 1000 rpm for 30 minutes to obtain a perfluorosulfonic acid resin slurry.

[0099] Example 17

[0100] The only difference from Example 2 is:

[0101] S4. The perfluorosulfonic acid resin dispersion was treated using a grinding pump at a temperature of 25°C for 30 minutes to obtain a perfluorosulfonic acid resin slurry.

[0102] Example 18

[0103] The only difference from Example 2 is that:

[0104] S4. The perfluorosulfonic acid resin dispersion was treated using a shear emulsifier at a temperature of 25°C for 30 minutes to obtain a perfluorosulfonic acid resin slurry.

[0105] Comparative Example 1

[0106] The only difference from Example 1 is that the homogenization step is not included; specifically:

[0107] S1. Weigh out the following components according to the following ratios: potassium perfluorosulfonate resin (weight average molecular weight of 5 million), deionized water, ethanol, isopropanol, and n-propanol. These components are added sequentially to a 2L reactor. The reactor is then sealed and secured. Nitrogen gas is introduced to maintain pressure, and after ensuring no leakage, the gas is released. This process is repeated to completely replace the air inside the reactor. The reactor is then stirred and heated. Once the temperature inside the reactor reaches 150°C, the pressure inside the reactor is controlled at 16MPa. The temperature is maintained and the reactor is stirred for 12 hours. Heating is then stopped. After the temperature inside the reactor cools to 20°C, the pressure relief valve is opened to release the pressure.

[0108] S2, open the reactor, transfer the product to a vacuum oven and vacuum dry for 34 hours. Control the temperature at 75℃ for the first 14 hours and at 90℃ for the next 20 hours. Then collect the dried powder. Weigh a 38% sulfuric acid aqueous solution according to a sulfuric acid aqueous solution to powder mass ratio of 8:1. Add the dried powder to the sulfuric acid aqueous solution and stir for 18 hours, controlling the temperature of the mixed solution at 98℃ during stirring. Take out the acidified resin and wash it with ultrapure water until the washing solution is neutral. Then, freeze-dry the resin at -85℃ for 100 hours to obtain perfluorosulfonic acid resin.

[0109] S3, weigh the second part of water according to the mass ratio of perfluorosulfonic acid resin to the second part of water of 1:20, weigh the second part of organic solvent according to the mass ratio of the second part of water to the second organic solvent of 3.3:1, weigh the ethanol, isopropanol and n-propanol according to the mass ratio of 1:1:1, and stir the mixed solution of perfluorosulfonic acid resin, water, ethanol, isopropanol and n-propanol at 0.105MPa, nitrogen atmosphere and 25℃ for 25h to obtain perfluorosulfonic acid resin dispersion;

[0110] S4. First, lay a base film. Pour the perfluorosulfonic acid resin dispersion into the front of the scraper through the hopper of the container. After controlling the gap between the scraper and the base film, move the scraper forward to scrape out a wet film. After covering the reinforcing layer, scrape out a wet film again to make it cast and form. Dry it to obtain a proton exchange membrane.

[0111] Verification has shown that perfluorosulfonic acid resin has a relatively high molecular weight and uneven distribution, resulting in relatively low tensile strength and elongation at break of the proton exchange membrane, but relatively high linear swelling rate.

[0112] Comparative Example 2

[0113] Commercially available perfluorosulfonic acid resin was used. Water was weighed at a mass ratio of 1:20, organic solvent was weighed at a mass ratio of 3.3:1, and ethanol, isopropanol, and n-propanol were weighed at a mass ratio of 1:1:1. The mixture of perfluorosulfonic acid resin, water, ethanol, isopropanol, and n-propanol was stirred for 25 hours under a nitrogen atmosphere at 0.105 MPa and 25°C.

[0114] It was verified that commercially available perfluorosulfonic acid resin was difficult to dissolve after stirring at room temperature and pressure, and perfluorosulfonic acid resin slurry could not be obtained.

[0115] The EW value, molecular weight, tensile strength, swelling properties, and conductivity of the perfluorosulfonic acid resins in the above examples and comparative examples were tested. The results are shown in Table 1.

[0116] Test method:

[0117] EW value: The resin is immersed in a saturated NaCl solution at room temperature for 24 hours, and the solution is then subjected to acid-base titration and calculated.

[0118] Molecular weight: Measured by gel permeation chromatography (GPC);

[0119] Tensile strength: The tensile strength of the proton exchange membrane was tested using a universal tensile testing machine at 25℃ and 50% RH; where MD is the tensile strength in the membrane coating direction and TD is the tensile strength perpendicular to the membrane coating direction.

[0120] Swelling performance: The proton exchange membrane was cut into 3×4cm pieces, with a width of 3cm in the MD direction and a width of 4cm in the TD direction. After immersing it in water at 80℃ for 17h, the dimensional changes of the membrane in different directions were measured and calculated.

[0121] Conductivity: The conductivity of the proton exchange membrane was tested using the four-electrode probe method.

[0122] Table 1

[0123]

[0124]

[0125] As can be seen from the above, compared with the comparative example, the weight-average molecular weight of the resins in each embodiment of the present invention decreased to varying degrees. Furthermore, the homogenization treatment resulted in a smaller molecular weight distribution index, indicating a narrower molecular weight distribution and more uniform molecular chain segment lengths. This makes it easier for the molecular chain segments to align into a regular structure during subsequent film-forming heat treatment, which is more conducive to improving the crystallinity of the membrane. This further enhances the membrane's mechanical strength, anti-swelling properties, and extends its service life. Simultaneously, the slurry prepared after homogenization treatment exhibits better dispersion, allowing for better filling of the reinforcing layer during coating, which is more beneficial for improving the conductivity of the proton exchange membrane and thus more effectively improving the fuel cell's performance. Moreover, the EW value was not significantly affected by the homogenization process. In summary, the method provided by the present invention results in a uniform weight-average molecular weight distribution of the perfluorosulfonic acid resin, uniform solute dispersion in the perfluorosulfonic acid resin slurry, and a proton exchange membrane with high mechanical strength, strong anti-swelling properties, and minimal impact of the treatment process on the proton exchange membrane's conductivity.

[0126] Furthermore, it can be seen that when all process parameters are within the preferred range of this invention, the molecular weight distribution of perfluorosulfonic acid resin is narrower, the molecular chain segment length is more uniform, the solute distribution in the perfluorosulfonic acid resin slurry is more uniform, and the overall performance of the proton exchange membrane prepared is better.

[0127] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a perfluorosulfonic acid resin slurry, characterized in that, Includes the following steps: Step S1: The first portion of water, the first organic solvent, and the perfluorosulfonate resin are mixed to obtain a first resin dispersion; the temperature of the first mixing is 90~200℃, the pressure is 3~30 MPa, and the time is 6~18h. Step S2: The first resin dispersion is dried to obtain a first resin powder, which is then mixed with an acidic aqueous solution, and subsequently washed with water and freeze-dried to obtain a perfluorosulfonic acid resin. The drying temperature is 50~150℃ and the time is 10~48 h; the second mixing temperature is 50~120℃ and the time is 12~30 h; the freeze-drying temperature is -70~-90℃ and the time is 24~120 h. Step S3: The second portion of water, the second organic solvent, and the perfluorosulfonic acid resin are mixed in a third mixture to obtain a second resin dispersion; the temperature of the third mixing is 20~40℃, the pressure is 0.1~0.11 MPa, and the time is 17~32h. Step S4: The second resin dispersion is homogenized to obtain the perfluorosulfonic acid resin slurry; the homogenization treatment is one or more of ultrasonication, shearing, stirring, grinding and high-pressure impact; the temperature of the homogenization treatment is 25~40℃.

2. The preparation method according to claim 1, characterized in that, In step S1 The perfluorosulfonate resin is potassium perfluorosulfonate resin and / or sodium perfluorosulfonate resin; and / or The perfluorosulfonate resin has a weight-average molecular weight of 500,000 to 9,000,000; and / or The perfluorosulfonate resin accounts for 5-30% of the weight of the first resin dispersion.

3. The preparation method according to claim 1 or 2, characterized in that, In step S1 The first organic solvent is two or more of methanol, ethanol, n-propanol, and isopropanol; and / or The mass ratio of the first portion of water to the first organic solvent is (1~5):1; and / or The first mixing is carried out in an inert gas atmosphere, wherein the inert gas is nitrogen and / or argon.

4. The preparation method according to claim 1 or 2, characterized in that, In step S2, the acidic aqueous solution is an aqueous solution of sulfuric acid and / or an aqueous solution of nitric acid, and the mass concentration of the acidic aqueous solution is 20-55%.

5. The preparation method according to claim 4, characterized in that, In step S2, the mass ratio of the acidic aqueous solution to the first resin powder is (5~10):

1.

6. The preparation method according to claim 1 or 2, characterized in that, In step S3 The mass ratio of the perfluorosulfonic acid resin to the second portion of water is 1:(5~35); and / or The second organic solvent is two or more of methanol, ethanol, n-propanol, and isopropanol; and / or The mass ratio of the second portion of water to the second organic solvent is (2~5):

1.

7. The preparation method according to claim 1 or 2, characterized in that, In step S3, the third mixing is carried out in an inert gas atmosphere, wherein the inert gas is nitrogen and / or argon.

8. The preparation method according to claim 1 or 2, characterized in that, In step S4, the homogenization process is a high-pressure impact, and the pressure of the homogenization process is 500~1725 bar.

9. A perfluorosulfonic acid resin slurry, characterized in that, It is obtained by the preparation method according to any one of claims 1 to 8.

10. A proton exchange membrane, characterized in that, It is prepared from the perfluorosulfonic acid resin slurry described in claim 9.

Citation Information

Patent Citations

  • Polymer supershort fiber reinforced fuel cell proton exchange membrane and its preparing method

    CN101071873A

  • Preparation method of novel lignosulfonic acid / Nafion composite proton exchange membrane

    CN112803051A

  • Self-humidifying proton exchange membrane and preparation method and application thereof

    CN111146482A

  • Sodium perfluorosulfonate ion battery electrolyte membrane as well as preparation method and application thereof

    CN111341980A