Nickel selenide / cobalt molybdenum oxide composite material, preparation method and application thereof in hydrogen evolution, oxygen evolution and overall water splitting reaction
By preparing nickel selenide/cobalt-molybdenum oxide nanorods on nickel foam, the problems of high cost of noble metal catalysts and complex preparation of traditional selenides were solved, achieving highly efficient catalysis of water electrolysis, reducing preparation difficulty and cost, and improving catalytic performance.
Patent Information
- Application Number
- CN202311348632.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-17
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-10-17
AI Technical Summary
Existing precious metal-based catalysts are expensive and scarce, and traditional methods for preparing transition metal selenides are complex and cannot meet the practical application requirements of water electrolysis reactions.
Using nickel foam as a framework, nickel selenide/cobalt-molybdenum oxide composite materials were prepared by atmospheric pressure reaction and annealing, simplifying the selenization process and generating Ni₃Se₂/Co₂Mo₃O₈ nanorod structures, which can serve as highly efficient catalysts for hydrogen evolution, oxygen evolution, and total water splitting reactions.
This method achieves low-cost, high-efficiency catalytic water electrolysis, reduces the activation energy of water electrolysis, improves electrocatalytic performance, simplifies the preparation process, and enhances repeatability and catalytic activity.
Smart Images

Figure CN117448874B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the research field of inorganic nanomaterials and catalyst preparation, and particularly relates to a nickel selenide / cobalt molybdenum oxide composite material, its preparation method, and its application in hydrogen evolution, oxygen evolution, and total water splitting reactions. Background Technology
[0002] Hydrogen (H2) is considered a promising next-generation energy fuel for solving problems such as the energy crisis, environmental pollution, and climate change due to its high energy density, cleanliness, and renewability. Specifically, green H2 produced by electrochemical water splitting driven by electricity generated from tidal, wind, and solar power is a sustainable and realistic zero-carbon emission method. The water splitting reaction consists of two half-reactions: the oxygen evolution reaction (OER) at the anolyte and the hydrogen evolution reaction (HER) at the cathodicly.
[0003] However, the high energy barrier required to break down water molecules has prevented the widespread industrialization of water electrolysis. To address these issues, it is necessary to find an efficient catalyst to lower the energy barriers of HER and OER.
[0004] Currently, Ru, Ir, and Pt-based noble metal catalysts remain the most widely used catalysts for water electrolysis. However, their high cost and scarcity are unsatisfactory.
[0005] Among various emerging non-precious metal materials, transition metal compounds have been extensively explored and studied. These include transition metal oxides, carbides, nitrides, phosphides, sulfides, and selenides. Transition metal selenides, in particular, have attracted attention due to their suitable d-electron configuration and high conductivity. However, traditional selenization methods often involve high temperatures or pressures, placing excessive demands on the reaction process and resulting in cumbersome steps. The electrocatalytic performance of transition metal selenides has not yet met the requirements for practical applications.
[0006] In addition, patent CN 112216521 A, published on January 12, 2021, discloses a nickel molybdate-nickel selenide-molybdenum selenide composite material, its preparation method, and its application. The preparation method is as follows: Step a, Preparation of nickel molybdate: Weigh nickel nitrate hexahydrate and sodium molybdate dihydrate and dissolve them in a mixed solvent of anhydrous ethanol and deionized water. After stirring evenly, a mixed solution of nickel nitrate and sodium molybdate is obtained. The mixed solution is transferred to a high-pressure reactor for hydrothermal reaction. The solid material obtained after centrifugation is washed several times with deionized water and anhydrous ethanol and dried to obtain a hydrothermal product. The hydrothermal product is placed in… Nickel molybdate was obtained by calcination in a tube furnace under argon atmosphere. Step b: Preparation of nickel molybdate-nickel selenide-molybdenum selenide composite material: The nickel molybdate and selenium powder obtained in step a were placed in two quartz containers and subjected to selenization treatment in a tube furnace under argon atmosphere to obtain partially selenized nickel molybdate products, namely nickel molybdate-nickel selenide-molybdenum selenide composite material. The nickel molybdate-nickel selenide-molybdenum selenide composite material prepared by the disclosed method has high specific capacitance and good cycle stability, but its application as a catalyst is not disclosed.
[0007] Therefore, the development of transition metal selenide catalysts still warrants further exploration. Summary of the Invention
[0008] The purpose of this invention is to provide a nickel selenide / cobalt-molybdenum oxide composite material and its preparation method. The method involves a simple atmospheric pressure reaction and annealing process, using nickel foam as a framework to grow the nickel selenide / cobalt-molybdenum oxide composite material. This invention first selenizes the nickel foam, then grows a precursor on the selenized nickel framework, and finally anneals to generate the nickel selenide / cobalt-molybdenum oxide composite material Ni3Se2 / Co2Mo3O8. Furthermore, unlike the commonly used high-temperature selenization method using selenium powder, this invention provides an extremely simple and convenient selenization method.
[0009] Another objective of this invention is to provide an application of a nickel selenide / cobalt molybdenum oxide composite material in hydrogen evolution, oxygen evolution, and total water splitting reactions, serving as a highly efficient trifunctional catalyst for these reactions.
[0010] The specific technical solution of this invention is as follows:
[0011] A method for preparing a nickel selenide / cobalt-molybdenum oxide composite material includes the following steps:
[0012] 1) Add the selenium source to the solvent, then add nickel foam, and let it stand to react;
[0013] 2) Add cobalt and molybdenum sources, heat and allow to stand to react, and obtain the precursor;
[0014] 3) Anneal the precursor prepared in step 2) to obtain the nickel selenide / cobalt molybdenum oxide composite material Ni3Se2 / Co2Mo3O8.
[0015] In step 1), the selenium source is selenium dioxide;
[0016] In step 1), the concentration of the selenium source in the solvent is 0.005–0.025 M; more preferably 0.018 M.
[0017] In step 1), the solvent is selected from water, preferably deionized water;
[0018] In step 1), the standing time is a reaction time of 1 to 30 minutes at 5℃ to 40℃.
[0019] In step 2), the cobalt source is selected from soluble cobalt salts, preferably cobalt nitrate hexahydrate Co(NO3)2·6H2O;
[0020] In step 2), the molybdenum source is selected from soluble molybdenum salts, preferably ammonium molybdate tetrahydrate (NH4)6Mo7O. 24 ·4H2O;
[0021] The molar ratio of the selenium source, cobalt source and molybdenum source is (5-25):(75-130):(8-17); preferably 18:100:13.
[0022] In step 2), the heated and static reaction refers to the reaction at a temperature of 50℃ to 90℃ for 3h to 24h; preferably, the reaction is carried out at 60℃ for 8h.
[0023] In step 2), after the reaction is complete, the nickel foam is rinsed multiple times with deionized water and ethanol to remove unreacted substances on the surface, and then dried in a vacuum drying oven to obtain a purple precursor, which is then stored for later use.
[0024] In step 3), the annealing refers to annealing at 300-550°C for 1-4 hours, with the annealing atmosphere being hydrogen and argon.
[0025] In step 3), the precursor obtained in step 2) is placed in a tube furnace and heated, and a mixed gas composed of hydrogen and argon is introduced; the heating rate is between 1 and 10 °C / min, the temperature is raised to 300 to 550 °C and held for 1 to 4 hours; in the annealing atmosphere, the volume percentage of hydrogen should be between 5% and 20%.
[0026] Preferably, in step 3), the annealing conditions involve raising the temperature to 450°C at a rate of 5°C / min and holding it at this temperature for 2 hours; in the annealing atmosphere, hydrogen should account for 10% of the gas volume.
[0027] In step 3), after annealing, the material is naturally cooled to obtain a black nickel selenide / cobalt molybdenum oxide composite material.
[0028] The nickel selenide / cobalt-molybdenum oxide composite material prepared in this invention mainly involves: using water as a solvent, selenium dioxide dissolves and reacts with water to generate selenite, which has oxidizing properties; selenite reacts with nickel foam to generate nickel selenide, and then Co and Mo elements combine with O elements to form crystal nuclei on the surface of nickel selenide, subsequently growing cobalt-molybdenum oxide nanorods. The more complete the reaction, the greater the number of nanorods generated, achieved by increasing the reaction temperature and reaction time. The subsequent annealing step mainly enhances the interaction between the self-supporting carrier and the nanorods. Nickel selenide, due to its suitable d-electron configuration, can lower the activation energy of the water electrolysis reaction, promoting the production of hydrogen and oxygen; simultaneously, its high conductivity is also beneficial for electron transport in the electrocatalytic reaction. Furthermore, the various oxidation states of cobalt and molybdenum ions on the surface of the cobalt-molybdenum oxide can provide different reaction sites, promoting the water electrolysis reaction. Morphology can be controlled by adjusting the reaction temperature. The purpose of these steps is to optimize the structure and properties of the material.
[0029] The present invention provides a nickel selenide / cobalt molybdenum oxide composite material, which is prepared by the above method. The product is Ni3Se2 / Co2Mo3O8, which has a nanorod morphology. The length of the nanorods ranges from 15 to 40 μm, preferably from 20 to 30 μm, and the width of the nanorods is from 0.3 to 0.7 μm, preferably from 0.4 to 0.6 μm.
[0030] The present invention provides a nickel selenide / cobalt molybdenum oxide composite material for use in hydrogen evolution, oxygen evolution and electrocatalytic total water splitting reactions, exhibiting excellent catalytic performance.
[0031] The application of nickel selenide / cobalt-molybdenum oxide composites in hydrogen evolution through water electrolysis at a current density of 100 mA cm⁻¹ -2 When the catalyst prepared in Example 1 has an overpotential of less than 200 mV, preferably less than 140 mV; the application of the nickel selenide / cobalt-molybdenum oxide composite material in the oxygen evolution reaction, when the current density is 100 mA cm⁻¹ -2 At that time, the potential was less than 300mV; the application of nickel selenide / cobalt molybdenum oxide composite materials in water splitting was carried out at a current density of 100mA cm⁻¹. -2 At that time, the potential of the catalyst was only 1.60V.
[0032] In the nickel selenide / cobalt-molybdenum oxide composite material provided by this invention, selenium, as a member of the chalcogenide group, possesses abundant valence states, and valence state transitions are beneficial for electron transport. Furthermore, compared to sulfur, selenium has a larger atomic radius, lower ionization energy, and higher metallic properties. Therefore, it exhibits higher electrical conductivity, a suitable band gap, and a d-electron configuration, which facilitates electron transport and effectively disrupts HO-H bonds, thereby improving electrochemical performance.
[0033] Compared with existing technologies, the preparation method provided by this invention only needs to be carried out under normal pressure, without the need for high-temperature reactions in a reactor, and without the need for surfactants and precipitants, thus reducing costs. It has lower requirements for the precision of reaction temperature and time, is simple to operate, and has high repeatability. Furthermore, the product exhibits excellent catalytic performance in electrolytic water electrolysis for hydrogen evolution, electrolytic water electrolysis for oxygen evolution, and electrocatalytic total water splitting reactions. Attached Figure Description
[0034] Figure 1 Here is a scanning electron microscope image of the nickel selenide / cobalt molybdenum oxide composite material synthesized in Example 1 at 400°C.
[0035] Figure 2 Here is a scanning electron microscope image of the nickel selenide / cobalt molybdenum oxide composite material synthesized in Example 1 at 15 K;
[0036] Figure 3 The image shows the X-ray diffraction (XRD) pattern of the nickel selenide / cobalt molybdenum oxide composite material synthesized in Example 1.
[0037] Figure 4 Here is a scanning electron microscope image of the material synthesized in Example 4;
[0038] Figure 5 The HER polarization curves of the materials synthesized in Examples 1, 2, 3 and 4 in 1M KOH solution are shown.
[0039] Figure 6 The OER polarization curves of the materials synthesized in Examples 1, 2, 3 and 4 in 1M KOH solution are shown.
[0040] Figure 7 The image shows the total water decomposition polarization curve of the nickel selenide / cobalt molybdenum oxide composite material synthesized in Example 1 in 1M KOH solution;
[0041] Figure 8 Here is a scanning electron microscope image of the material synthesized in Comparative Example 1 at 300 K;
[0042] Figure 9 The image shows a scanning electron microscope (SEM) image of the material synthesized in Comparative Example 2.
[0043] Figure 10The HER polarization curves of the materials synthesized in Comparative Examples 1, 2, 3, and 4 and the material synthesized in Example 1 are shown in 1M KOH solution.
[0044] Figure 11 The OER polarization curves of the materials synthesized in Comparative Examples 1, 2, 3, and 4 and the material synthesized in Example 1 in 1M KOH solution are shown.
[0045] Figure 12 The image shows a scanning electron microscope (SEM) image of the material synthesized in Comparative Example 1 at 200 K. Detailed Implementation
[0046] The present invention will now be described in detail with reference to the embodiments and accompanying drawings.
[0047] Example 1
[0048] A method for preparing a nickel selenide / cobalt-molybdenum oxide composite material includes the following steps:
[0049] 1) Soak the nickel foam in 3M dilute hydrochloric acid and sonicate for 10 minutes to remove the surface oxidation. Then rinse off the hydrochloric acid with a large amount of ethanol, soak it in anhydrous ethanol again and sonicate for 10 minutes, and then vacuum dry it for later use.
[0050] 2) Dissolve 0.18 mmol of selenium dioxide in 10 mL of deionized water, place a piece of cleaned nickel foam measuring 1 cm × 3 cm in the solution, and soak at 25°C for 5 min.
[0051] 3) Add 1 mmol Co(NO3)2·6H2O and 0.13 mmol (NH4)6Mo7O to the container from step 2). 24 Add 4H₂O, sonicate until dissolved, and place in a 60°C oven for 8 hours. After the reaction is complete, wash three times alternately with deionized water and ethanol, and then dry at room temperature for later use.
[0052] 4) Place the nickel foam obtained in step 3) in a tube furnace, heat it to 450°C at a rate of 5°C / min, and hold it at that temperature for 2 hours. The entire calcination process is carried out in a hydrogen-argon mixture with a hydrogen content of 10%. After the reaction is completed, allow it to cool naturally to room temperature to obtain the final black product.
[0053] The nickel selenide / cobalt-molybdenum oxide composite material prepared by the method in Example 1 was analyzed by scanning electron microscopy. Figure 1 and Figure 2 Its morphology was observed, confirming it as an array structure composed of nanorods. X-ray diffraction was then performed. Figure 3 Further evidence confirms that the material is a nickel selenide / cobalt-molybdenum oxide composite material, with XRD results showing nickel selenide and cobalt-molybdenum oxide respectively. This demonstrates that the present invention successfully prepared the nickel selenide / cobalt-molybdenum oxide composite material.
[0054] Example 2
[0055] A method for preparing a nickel selenide / cobalt-molybdenum oxide composite material includes the following steps:
[0056] 1) Soak the nickel foam in 3M dilute hydrochloric acid and sonicate for 10 minutes to remove the surface oxidation. Then rinse off the hydrochloric acid with a large amount of ethanol, soak it in anhydrous ethanol again and sonicate for 10 minutes, and then vacuum dry it for later use.
[0057] 2) Dissolve 0.18 mmol of selenium dioxide in 10 mL of deionized water, place a piece of cleaned nickel foam measuring 1 cm × 3 cm in the solution, and soak at 10 °C for 5 min.
[0058] 3) Add 1 mmol Co(NO3)2·6H2O and 0.13 mmol (NH4)6Mo7O24·4H2O to the container from step 2), sonicate until dissolved, and place in a 60℃ oven for 8 hours. After the reaction is complete, wash three times alternately with deionized water and ethanol, and then dry at room temperature for later use.
[0059] 4) Place the nickel foam obtained in step 3) in a tube furnace, heat to 450°C at a rate of 5°C / min, and hold at that temperature for 2 hours. The entire calcination process is carried out in a hydrogen-argon mixture with a hydrogen content of 5%. After the reaction is complete, allow it to cool naturally to room temperature. A black final product is obtained.
[0060] Example 3
[0061] A method for preparing a nickel selenide / cobalt-molybdenum oxide composite material includes the following steps:
[0062] 1) Soak the nickel foam in 3M dilute hydrochloric acid and sonicate for 10 minutes to remove the surface oxidation. Then rinse off the hydrochloric acid with a large amount of ethanol, soak it in anhydrous ethanol again and sonicate for 10 minutes, and then vacuum dry it for later use.
[0063] 2) Dissolve 0.18 mmol of selenium dioxide in 10 mL of deionized water, place a piece of cleaned nickel foam measuring 1 cm × 3 cm in the solution, and soak at 30 °C for 5 min.
[0064] 3) Add 1 mmol Co(NO3)2·6H2O and 0.13 mmol (NH4)6Mo7O24·4H2O to the container from step 2), sonicate until dissolved, and place in a 60℃ oven for 8 hours. After the reaction is complete, wash three times alternately with deionized water and ethanol, and then dry at room temperature for later use.
[0065] 4) Place the nickel foam obtained in step 3) in a tube furnace, heat it to 400℃ at a rate of 5℃ / min, and hold it at that temperature for 2 hours. The entire calcination process is carried out in a hydrogen-argon mixture with a hydrogen content of 10%. After the reaction is complete, allow it to cool naturally to room temperature. A black final product is obtained.
[0066] Example 4
[0067] A method for preparing a nickel selenide / cobalt-molybdenum oxide composite material includes the following steps:
[0068] 1) Soak the nickel foam in 3M dilute hydrochloric acid and sonicate for 10 minutes to remove the surface oxidation. Then rinse off the hydrochloric acid with a large amount of ethanol, soak it in anhydrous ethanol again and sonicate for 10 minutes, and then vacuum dry it for later use.
[0069] 2) Dissolve 0.18 mmol of selenium dioxide in 10 mL of deionized water, place a piece of cleaned nickel foam measuring 1 cm × 3 cm in the solution, and soak at 40 °C for 5 min.
[0070] 3) Add 1.25 mmol Co(NO3)2·6H2O and 0.09 mmol (NH4)6Mo7O to the container from step 2). 24 Add 4H₂O, sonicate until dissolved, and place in a 60°C oven for 8 hours. After the reaction is complete, wash three times alternately with deionized water and ethanol, and then dry at room temperature for later use.
[0071] 4) Place the nickel foam obtained in step 3) in a tube furnace, heat to 450°C at a rate of 5°C / min, and hold at that temperature for 2 hours. The entire calcination process is carried out in a hydrogen-argon mixture with a hydrogen content of 10%. After the reaction is complete, allow it to cool naturally to room temperature. A black final product is obtained.
[0072] Comparative Example 1
[0073] The procedure was carried out as in Example 1, except that 1 mmol Co(NO3)2·6H2O and 0.13 mmol (NH4)6Mo7O were added. 24 After 4H2O, do not place it in a 60℃ oven. Instead, keep it at 25°C for 8 hours. The other steps are the same as in Example 1.
[0074] Scanning electron microscopy Figure 8 and 12 Observing the morphology of Comparative Example 1, it was observed that the material prepared according to the above method did not form nanorod structures on the nickel foam framework, but only a layer of small nanoflowers existed on the surface of the nickel foam. This indicates that after adding cobalt and molybdenum sources, due to the low temperature, cobalt and molybdenum ions could not successfully nucleate and crystallize, thus preventing the growth of cobalt and molybdenum oxide nanorods. This affects the material's properties.
[0075] pass Figure 1 , 2 and Figure 8 , 12 In comparison, it was found that at 25℃, Co and Mo formed small nanoflowers on the surface of nickel foam oxidized by selenite. However, at 60℃, larger nanorods were formed.
[0076] Comparative Example 2
[0077] The procedure was carried out according to Example 1, except that 0.005 g (0.045 mmol) of selenium dioxide was dissolved in 10 mL of deionized water, and the other steps were the same as in Example 1.
[0078] Scanning electron microscopy Figure 9 Observing the morphology of Comparative Example 2, it was found that the material obtained according to the above preparation method presents as particulate matter without a specific morphology. This indicates that the amount of selenite solution generated by the reaction of selenium dioxide and water is insufficient to completely oxidize the nickel foam, and the untreated nickel foam surface is not conducive to the growth of cobalt-molybdenum oxides. This affects the material's performance.
[0079] Comparative Example 3
[0080] The process was carried out according to Example 1, except that the annealing temperature was [temperature missing]. 650℃ Everything else is the same as in Example 1.
[0081] Comparative Example 4
[0082] The procedure is the same as in Example 1, except that: The amount of Co(NO3)2·6H2O added was 0.44g (1.5mmol). (NH4)6Mo7O 24 The amount of 4H2O is 0.4g (0.32mmol). The other steps are the same as in Example 1.
[0083] Application Example 1
[0084] The application of nickel selenide / cobalt-molybdenum oxide composite materials in the hydrogen evolution reaction is as follows:
[0085] The HER electrochemical performance of the material was evaluated using a three-electrode system connected to a CHI760 electrochemical workstation. The prepared material (1 cm × 2 cm), a graphite rod, and Ag / AgCl were used as the working electrode, counter electrode, and reference electrode, respectively. The sample was first activated by cyclic voltammetry (CV) at a scan rate of 50 mV / s. -1 The reaction was cycled 50 times to minimize polarization effects and stabilize the reaction system as much as possible. The LSV of HER was measured at 5 mV s⁻¹ in a 1 M potassium hydroxide solution at room temperature. -1 The scan rate was measured. All LSV reactions were corrected by iR compensation (90%). The measured potential of HER was converted to that of the reversible hydrogen electrode (RHE) according to the following equation: E (vs.RHE) =E(vs.Ag / AgCl) +0.197 +0.0591 × pH. When the current density is 100 mA / cm². -2 At that time, the overpotential of the catalyst prepared in Example 1 was only 90mV.
[0086] Figure 5 The HER polarization curves of the products of Examples 1, 2, 3, and 4 in 1M KOH solution are shown. Figure 10 The HER polarization curves of the materials synthesized in Comparative Examples 1, 2, 3, and 4 and the material synthesized in Example 1 are shown in 1M KOH solution. Specifically, the polarization curves are shown at a current density of 100 mA cm⁻¹. -2 At that time, the overpotential of the catalyst prepared in Example 1 was only 90mV, the overpotential of the catalyst prepared in Example 2 was 137mV, the overpotential of the catalyst prepared in Example 3 was 120mV, and the overpotential of the catalyst prepared in Example 4 was 117mV. The overpotentials of the above examples were all much less than 200mV, and they had excellent catalytic performance. Figure 10 Specifically, at a current density of 100 mA cm⁻¹ -2 At that time, the overpotential of the catalyst prepared in Comparative Example 1 was 364 mV, the overpotential of the catalyst prepared in Comparative Example 2 was 391 mV, the overpotential of the catalyst prepared in Comparative Example 3 was 247 mV, and the overpotential of the catalyst prepared in Comparative Example 4 was 262 mV. The overpotentials of the above examples were all greater than 200 mV, indicating that the catalytic activity was low.
[0087] Application Example 2
[0088] The application of nickel selenide / cobalt-molybdenum oxide composites in the oxygen evolution reaction is as follows:
[0089] The HER electrochemical performance of the material was evaluated using a three-electrode system connected to a CHI760 electrochemical workstation. The prepared material (1 cm × 2 cm), a platinum sheet, and Ag / AgCl were used as the working electrode, counter electrode, and reference electrode, respectively. The sample was first activated by cyclic voltammetry (CV) at a scan rate of 50 mV / s. -1 The reaction was cycled 50 times to minimize polarization effects and stabilize the reaction system as much as possible. The LSV of HER was measured at 1 mV s⁻¹ in a 1 M potassium hydroxide solution at room temperature. -1 The scan rate was measured. All LSV reactions were corrected by iR compensation (90%). The measured potential of HER was converted to that of the reversible hydrogen electrode (RHE) according to the following equation: E (vs.RHE) =E (vs.Ag / AgCl) +0.197 +0.0591 × pH. When the current density is 100 mA / cm². -2 At that time, the overpotential of the catalyst prepared in Example 1 was only 266mV.
[0090] Figure 6 The OER polarization curves of the products of Examples 1, 2, 3, and 4 in 1M KOH solution are shown. Figure 11 The OER polarization curves of the materials synthesized in Comparative Examples 1, 2, 3, and 4, and the material synthesized in Example 1, are shown in 1M KOH solution. Specifically, the polarization curves are shown at a current density of 100 mA cm⁻¹. -2 At that time, the overpotential of the catalyst prepared in Example 1 was only 266mV, the overpotential of the catalyst prepared in Example 2 was 273mV, the overpotential of the catalyst prepared in Example 3 was 279mV, and the overpotential of the catalyst prepared in Example 4 was 283mV. The overpotentials of the above examples were all less than 300mV, indicating that they have excellent catalytic performance. Figure 11 In the case of a current density of 100 mA cm⁻¹ -2 At that time, the overpotential of the catalyst prepared in Comparative Example 1 was 414 mV, the overpotential of the catalyst prepared in Comparative Example 2 was 513 mV, the overpotential of the catalyst prepared in Comparative Example 3 was 406 mV, and the overpotential of the catalyst prepared in Comparative Example 4 was 363 mV. The overpotentials of the above examples are all much greater than 300 mV, indicating that the catalytic activity is low.
[0091] Application Example 3
[0092] The application of nickel selenide / cobalt-molybdenum oxide composite materials in water splitting is as follows:
[0093] The polarization curves of the nickel selenide / cobalt molybdenum oxide composite material under alkaline conditions were obtained by electrochemical linear scanning voltammetry. Specifically, in a 1M potassium hydroxide solution, two 1cm × 2cm samples from Example 1 were used as the cathode and anode, respectively. Connected to a CHI760 electrochemical workstation, the sample was first activated by cyclic voltammetry (CV) within a potential range of 1.7–1.2 V (vs. RHE) at a scan rate of 50 mV / s. -1 Repeat 50 times. Use 1mV s -1 The scanning rate was set, and 90% iR compensation was applied to obtain the polarization curves for the complete water splitting. At a current density of 100 mA cm⁻¹ -2 At that time, the potential of the catalyst prepared in Example 1 was only 1.60V.
[0094] Figure 7 The image shows the total hydrolysis polarization curve of the product from Example 1 in a 1M KOH solution.
[0095] The method employed in this invention is simple to operate, requires minimal reaction equipment, and has good repeatability. It can significantly reduce production costs.
[0096] The above detailed description of the nickel selenide / cobalt molybdenum oxide composite material for promoting the three-functional applications of HER, OER and total water splitting, with reference to the embodiments, is illustrative rather than limiting. Several embodiments may be listed within the defined scope. Therefore, variations and modifications without departing from the overall concept of the present invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a nickel selenide / cobalt-molybdenum oxide composite material, characterized in that, The preparation method includes the following steps: 1) Add the selenium source to the solvent, then add nickel foam, and let it stand to react; 2) Add cobalt and molybdenum sources, heat and allow to stand to react, and obtain the precursor; 3) Anneal the precursor prepared in step 2) to obtain nickel selenide / cobalt molybdenum oxide composite material; In step 1), the selenium source is selenium dioxide; The molar ratio of the selenium source, cobalt source, and molybdenum source is (5~25):(75~130):(8~17); the concentration of the selenium source in the solvent is 0.005~0.025 M; In step 3), the annealing refers to annealing at 300~550℃ for 1~4 hours, with the annealing atmosphere being hydrogen and argon.
2. The preparation method according to claim 1, characterized in that, In step 1), the solvent is selected from water.
3. The preparation method according to claim 1, characterized in that, In step 1), the standing time is a reaction that is allowed to stand at 5℃~40℃ for 1~30 min.
4. The preparation method according to claim 1, characterized in that, In step 2), the heating and static reaction refers to the reaction at a temperature of 50℃~90℃ for 3 h~24 h.
5. The preparation method according to claim 1, characterized in that, In step 3), the annealing, The volume percentage of hydrogen in the annealing atmosphere should be between 5% and 20%.
6. A nickel selenide / cobalt molybdenum oxide composite material prepared by the preparation method according to any one of claims 1-5.
7. The application of a nickel selenide / cobalt molybdenum oxide composite material prepared by the preparation method according to any one of claims 1-5 in hydrogen evolution, oxygen evolution and total water splitting reactions.
Citation Information
Patent Citations
Nickel molybdate-nickel selenide-molybdenum selenide composite material and preparation method and application thereof
CN112216521A