A method for producing a glass passivation protective layer
By combining printing coating and photolithography development processes with a specific ratio of photoresist and glass powder, the automation challenges and cutting damage issues in existing glass passivation processes have been solved, achieving automated production and cost reduction.
Patent Information
- Application Number
- CN202311490423.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-10
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-11-10
AI Technical Summary
Existing glass passivation processes have problems such as difficulty in implementation in automated production, damage to glass during cutting, and high costs. In particular, electrophoresis and spin coating photolithography are not suitable for automation, while scraping is not conducive to automation and has a high product failure rate.
A specific ratio of photoresist and glass powder is mixed and coated onto the PN junction surface of the chip using a printing coating method. Combined with photolithography development and sintering processes, a glass passivation protective layer is formed. Uniform coating is achieved through automated printing coating and parameter optimization, avoiding cutting damage and reducing the amount of glass adhesive used.
It has achieved full automation of the chip production line, reduced the waste and cost of glass glue, and improved product reliability and glass protection during cutting.
Smart Images

Figure CN117457574B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of chip passivation layer coating technology, specifically relating to a method for preparing a glass passivation protective layer. Background Technology
[0002] Covering the surface of a chip's PN junction with a glass passivation protective layer is increasingly becoming a method for protecting the PN junction. A glass passivation film is applied to the surface of the chip's PN junction to form a barrier layer against contaminants such as sodium ions, further preventing external contaminants from entering the PN junction surface. Current glass passivation processes mainly consist of two major steps: glass powder coating and glass powder sintering. Glass powder coating methods include electrophoresis, spin coating, and blade coating; glass powder sintering generally uses furnace tube sintering. Therefore, the main difference in coating methods lies in the glass powder coating scheme. The main process of electrophoresis includes: primary photolithography, etching trenching, resist removal, RCA cleaning, SIPOS deposition, secondary photolithography, electrophoretic glass deposition, glass passivation, LTO deposition, tertiary photolithography, mesa etching, surface metallization, testing, cutting, and packaging. The advantages of electrophoresis are its uniform glass protective layer, no glass residue on the die cutting path, and no damage to the glass when cutting on the silicon substrate. However, its disadvantages are that electrophoresis requires manual loading and unloading, making automation difficult, and it is not suitable for chip cascading processes. The main process of spin-coating lithography is as follows: first-stage photolithography – etching trenching, resist removal, RCA cleaning, SIPOS deposition, spin-coating glass resist, second-stage photolithography, glass passivation, LTO deposition, third-stage photolithography, mesa etching, surface metallization, testing, cutting, and packaging. The advantages of spin-coating lithography are its high degree of automation and its design that cuts on the silicon substrate without damaging the glass. The disadvantages are the difference in glass thickness between the diagonal and tangential edges of the die, resulting in thinner glass on the diagonal. Furthermore, the use of photoresist spraying and developing makes it difficult to ensure no glass residue on the cutting path while maintaining the integrity of the glass protection on both sides of the trench. This process is also unsuitable for chip cascading processes, and the high cost due to the large amount of PG photoresist consumed results in higher costs. The main process of the blade coating method includes: first photolithography, etching and trenching, resist removal, RCA cleaning, SIPOS deposition, blade coating of glass slurry, glass passivation, LTO deposition, third photolithography, mesa etching, surface metallization, testing, cutting, and packaging. The advantages of the blade coating method are its simple process, large solderable area, strong forward surge capability, and suitability for chip stacking processes. The disadvantages are that it requires manual application of glass slurry, which is not conducive to automated production, and the cleavage after cutting is on the glass, resulting in a high product failure rate.
[0003] Existing technologies also include technical solutions that combine the above-mentioned processes to leverage their strengths and compensate for their weaknesses, but due to unreasonable setup methods, there is still much room for improvement in technical effectiveness.
[0004] Chinese invention patent publication CN114334793A discloses a glass passivation process using printed glass paste. By improving the coating method, it adopts a printing method, increasing work efficiency. However, glass remains at the bottom of the groove, posing a risk of glass damage during cutting. Chinese invention patent publication CN104465330B discloses a rectifier diode, chip, and its manufacturing method; however, it primarily uses a coating method, which is not conducive to automated production, and the coated glass is a gel-like material, resulting in significant waste. Summary of the Invention
[0005] This invention proposes a method for preparing a glass passivation protective layer. The method involves mixing photoresist and glass powder in a specific ratio using a printing coating method, coating the mixture onto the PN junction surface of a chip, and then removing the glass adhesive from the dicing channels using a photolithography development method and sintering the glass. This method can effectively solve the shortcomings of existing processes.
[0006] Specifically, this is achieved through the following technical means:
[0007] A method for preparing a glass passivation protective layer includes the following steps:
[0008] (1) Prepare materials: Prepare a mixture of photoresist and glass powder in a weight ratio of (21-41):(38-58). The photoresist and glass powder are mixed by grinding to obtain a glass mixture. Prepare a silicon wafer substrate with a PN junction, wherein the silicon wafer substrate with a PN junction is a silicon wafer substrate with trenches and exposed PN junctions.
[0009] (2) Coating: The glass mixture adhesive obtained in step (1) is coated onto the silicon wafer substrate with PN junction described in step (1) by printing.
[0010] (3) Soft baking: Place the wafer obtained after coating in step (2) into a soft oven at a temperature of 80-120°C and keep it at 80-120°C for 15-35 minutes to obtain the soft-baked wafer.
[0011] (4) Photolithography and development: The wafer obtained in step (3) is placed on an exposure machine for continuous exposure, then developed and fixed using a spray developer, and finally placed in an oven for baking to obtain the developed wafer.
[0012] (5) Photoresist removal, glass sintering and LTO deposition: The wafer obtained in step (4) is placed in a photoresist removal furnace. The temperature of the photoresist removal furnace is maintained at 485-520°C and in an oxygen atmosphere for 45-60 minutes to remove the photoresist on the wafer and retain the glass powder. Then the wafer obtained after photoresist removal is directly transferred to a glass sintering furnace and glass sintering is performed at 800-840°C for 5-30 minutes in a mixed atmosphere of oxygen and nitrogen. After removal, the glass-sintered wafer is obtained. Then, an LTO oxide film is deposited on the surface of the glass-sintered wafer.
[0013] (6) Surface metallization: The mesa and back side of the wafer obtained in step (5) are subjected to photolithography and etching to remove the oxygen-doped polysilicon thin film (SIPOS film) and / or oxide layer on the surface. During the removal of the oxygen-doped polysilicon thin film and / or oxide layer on the surface, an oxide layer is left around the edge of each mesa to expose the silicon on the mesa and the silicon on the back side. Then, surface metallization is performed on the exposed silicon to obtain a solderable wafer with a glass passivation protective layer.
[0014] As part of the parameter refinement and optimization, the following steps are included:
[0015] (1) Material preparation: Prepare a mixture of photoresist and glass powder according to a weight ratio of (21-41):(38-58), wherein the photoresist preferably has a density of 0.86-0.89 g / cm³. 3 Negative photoresist; glass powder with a thermal expansion coefficient of (41-46)×10⁻⁶ at 30-300℃. -7 The lead borosilicate glass powder has a softening point of 660–698℃, a particle size ≤44μm, and a density of 3.68–3.88 g / cm³. 3 Photoresist and glass powder are mixed by grinding to obtain glass mixed adhesive; a silicon wafer substrate with PN junction is prepared, wherein the silicon wafer substrate with PN junction is a silicon wafer substrate with trenches and exposed PN junctions, and the trench depth is 70-200μm and the trench width is 200-500μm.
[0016] (2) Coating: The glass mixed adhesive obtained in step (1) is coated onto the silicon wafer substrate with PN junction described in step (1) by printing. The coating thickness of the glass mixed adhesive on the mesa of the silicon wafer substrate is 20-60 μm, and the coating thickness of the glass mixed adhesive in the trench is 40-120 μm.
[0017] (3) Soft baking: Place the wafer obtained after coating in step (2) into a soft oven at a temperature of 80-120°C and keep it at 80-120°C for 15-35 minutes to obtain the soft-baked wafer.
[0018] (4) Photolithography and development: The wafer obtained in step (3) is placed on an exposure machine and exposed for 1 to 10 seconds. Then, it is developed and fixed using a spray developer. Finally, it is placed in an oven at a temperature of 130 to 150°C for 25 to 50 minutes to obtain the developed wafer.
[0019] (5) Photoresist removal, glass sintering and LTO deposition: The wafer obtained in step (4) is placed in a photoresist removal furnace. The temperature of the photoresist removal furnace is maintained at 500-510℃ and in an oxygen atmosphere for 50-60 minutes to remove the photoresist on the wafer and retain the glass powder. Then, the wafer obtained after photoresist removal is directly transferred to a glass sintering furnace and heated to 800-840℃. The temperature is maintained at 800-840℃ for 5-30 minutes in a mixed atmosphere of oxygen and nitrogen to perform glass sintering. After removal, the glass-sintered wafer is obtained. Then, an LTO oxide film (abbreviation for Low Temperature Oxide, i.e., low temperature oxide film. The main component is SiO2) is deposited on the surface of the glass-sintered wafer.
[0020] (6) Surface metallization: The mesa and back side of the wafer obtained in step (5) are subjected to photolithography and etching to remove the oxygen-doped polysilicon thin film (SIPOS film) or oxide layer on the surface. During the removal of the oxygen-doped polysilicon thin film or oxide layer on the surface, an oxide layer is left around the edge of each mesa to expose the silicon on the mesa and the silicon on the back side. Then, surface metallization is performed on the exposed silicon to obtain a solderable wafer with a glass passivation protective layer.
[0021] Preferably, in step (2), the glass composite adhesive obtained in step (1) is applied to the silicon wafer substrate with a PN junction described in step (1) by printing, specifically including the following steps:
[0022] I. The silicon wafer substrate with PN junction is placed on a printing press, and a printing screen is placed on top, with the center position of the mesh of the printing screen corresponding to the center position of the silicon wafer substrate.
[0023] II. Place the glass mixture obtained in step (1) on one side of the printing screen mesh, and use a screen brush to reciprocate once in the same direction. The printing amount is such that the coating thickness of the glass mixture on the mesa of the silicon wafer substrate is 20-60 μm and the coating thickness in the trench is 40-120 μm.
[0024] III. Raise the printing screen and remove the coated wafer.
[0025] As a preferred method, in step (1), the specific method for obtaining the glass mixed adhesive by grinding and mixing photoresist and glass powder is as follows: First, the photoresist and glass powder in a weight ratio of (21-41):(38-58) are placed together in a grinding jar and sealed. Then, the whole assembly is placed on a grinding mill. The rotation speed of the grinding jar body is set to 36-45 rpm and the grinding time is 24-59 hours. Then, the glass mixed adhesive obtained by grinding and mixing is poured out to obtain the glass mixed adhesive.
[0026] Preferably, in step (1), the upper plane between two adjacent trenches in the silicon wafer substrate with PN junction is the mesa of the silicon wafer substrate, and all trench surfaces and mesa surfaces in the silicon wafer substrate with PN junction are covered with an oxygen-doped polycrystalline silicon thin film (SIPOS film) or are not covered with an oxygen-doped polycrystalline silicon thin film.
[0027] Preferably, the lead borosilicate glass powder mentioned in step (1) has a particle size of 10–44 μm and a density of 3.78 g / cm³. 3 The coefficient of thermal expansion is 44×10. -7 / K and the softening point temperature is 680℃.
[0028] Preferably, after step (2), the amount of photoresist and glass powder mixture retained in the wafer coated with glass adhesive is 92-98 wt.% of the amount of glass adhesive used.
[0029] Preferably, the surface metallization process in step (6) is as follows: a metal layer is deposited on silicon by chemical plating, with a thickness of 0.1-2.0 μm. The plated wafer is then placed in an oven for baking. The baked wafer is then placed in a metal sintering furnace for sintering to form an alloy layer. After cleaning, chemical plating is repeated once, with a thickness of 0.1-2.0 μm. The plated wafer is then placed in an oven for baking and removed to complete the surface metallization process.
[0030] A solderable wafer with a glass passivation protective layer is prepared by the above-described preparation method.
[0031] Preferably, the wafer includes a silicon wafer substrate with a PN junction, a surface metal layer, an oxide layer, and a glass passivation protective layer. The silicon wafer substrate with the PN junction includes a trench and a mesa. The glass passivation protective layer extends from the outer end of the center of the bottom of the trench to the edge of the mesa. The surface metal layer is attached to the mesa. The oxide layer is disposed between the glass passivation protective layer and the surface metal layer on the mesa. The distance from the edge of the glass passivation protective layer at the bottom of the trench to the center of the bottom of the trench is 20-160 μm. The width of the glass passivation protective layer extending from the same side of the glass at the bottom of the trench to the mesa is 70-150 μm.
[0032] A chip comprising the aforementioned solderable wafer with a glass passivation protective layer.
[0033] The advantages of this invention are:
[0034] 1. This invention, through the rational setting of raw materials, coating thickness, and printing coating methods, enables automatic wafer loading and unloading, automatic adjustment of the spacing between the stencil and the silicon wafer, and automatic addition of glass-mixed adhesive, thereby achieving full automation of the production line. Because this invention combines specific photoresist with specific glass powder, uniform coating of the glass protective layer can be achieved simply by automatically adjusting the printing pressure. By specifically setting the exposure, development, fixing, and baking parameters of the printed glass adhesive, this invention ensures that there is no glass at the cutting edge (bottom center) at the bottom of the trench, preventing damage to the protective glass on the PN junction surface during cutting, thus improving product reliability. Although electrophoresis sometimes results in the absence of glass at the cutting edge, electrophoresis requires manual wafer loading and unloading, making automation difficult. Therefore, this invention reliably achieves the effect of no glass at the cutting edge at the bottom of the trench while maintaining automation, further improving product reliability.
[0035] 2. This invention, through specific settings of raw material ratios and types, combined with subsequent coating parameters and soft baking, photolithography, and development, significantly reduces the amount of glass adhesive used. Due to the specific density of the photoresist and the specific density and particle size of the glass powder, as well as the specific grinding and mixing method, the resulting glass mixture adhesive can be printed and coated using the specific method of this invention (i.e., the raw material composition and printing and coating have a close coordination relationship). It remains unchanged after one use and can be reused. That is, if the added glass adhesive is not used up at once, it can be reused. Therefore, in mass production, the loss is negligible, thereby greatly reducing costs. Attached Figure Description
[0036] Figure 1 This is a cross-sectional structural schematic diagram of the glass passivation protective layer of the present invention.
[0037] Figure 2 This is a schematic diagram of the protective layer in cross-section, as shown in Comparative Example 2.
[0038] Wherein: 101-cut line, 102-surface metal layer, 103-oxide layer, 104-glass passivation protective layer, 105-silicon wafer substrate with PN junction. Detailed Implementation
[0039] Example 1
[0040] A method for preparing a glass passivation protective layer includes the following steps:
[0041] (1) Material preparation: Prepare a mixture of photoresist and glass powder at a weight ratio of 31:48, wherein the photoresist is Fuji SC-450 (a negative photoresist with a density of 0.86~0.89g / cm³). 3 (Requirements), the glass powder is NEG GP200S (a lead borosilicate glass powder with a thermal expansion coefficient of 44×10⁻⁶ at 30–300℃). -7 For powders with a softening point of 680℃ and a particle size ≤44μm and a density of 3.78g / cm³, the following conditions must be met: 3 The photoresist and glass powder are mixed by rolling grinding. First, the two materials and alumina balls are placed in a grinding jar and sealed. Then, they are placed on a rolling mill for grinding. The speed is set to 40 rpm (the speed of the grinding jar itself). The grinding time is ≥24 hours but not more than 60 hours. Within this time range, the glass adhesive is poured out for use. Prepare a silicon wafer substrate with a PN junction. The silicon wafer substrate with a PN junction is a single 4-inch wafer substrate with trenches exposed to expose the PN junction. The trench depth is 120-140 μm and the trench width is 320-400 μm.
[0042] (2) Printing and Coating: The mixture of photoresist and glass powder obtained in step (1) is printed onto the silicon wafer substrate with PN junction described in step (1). In this embodiment, the amount of photoresist used per wafer is 1.0g (in other embodiments, for a 4-inch wafer substrate, the amount used can be 0.88~1.10g). First, the silicon wafer is placed on the printing machine, and a printing screen is placed on top, with the center of the screen corresponding to the center of the silicon wafer. Then, the photoresist is placed on one side of the screen, and the screen is printed once in one direction with a brush. Finally, the printing screen is raised and the silicon wafer is removed. The coating thickness is 20~40μm on the mesa and 50~80μm on the trench bottom.
[0043] (3) Soft baking: Place the wafer obtained after coating in step (2) into an oven at 100±5℃ and bake at this temperature for 25±5 minutes to obtain the soft-baked wafer.
[0044] (4) Photolithography and development: The wafer obtained in step (3) after soft baking is placed in a photolithography machine and exposed for 3 to 4 seconds. Then, it is fixed by spray developing machine and baked in an oven at 140±5℃ for 35±5 minutes.
[0045] (5) Photoresist removal, glass sintering, and LTO: The wafer obtained in step (4) is placed in a photoresist removal furnace and kept at 500±5℃ in an oxygen atmosphere for 50-60 minutes to remove the photoresist, leaving glass powder; then it is transferred to a glass sintering furnace, heated to 820±10℃, and kept at this temperature for 15±5 minutes in a mixed atmosphere of oxygen and nitrogen to obtain a glass-sintered wafer. An LTO oxide film is deposited on the surface of the glass-sintered wafer.
[0046] (6) Surface metallization: The mesa and back side of the wafer obtained in step (5) are processed by photolithography and etching to remove the SIPOS film and oxide layer on the surface, exposing the silicon on the mesa and back side (leaving an oxide layer around the edge of each mesa). Surface metallization is performed on the silicon to obtain a solderable wafer with a glass passivation protective layer.
[0047] The test showed that the weight of the glass adhesive on the surface of the single wafer in step (2) was 0.96g.
[0048] Comparative Example 1
[0049] This comparative example uses a blade-scraping method with a single photolithography step – etching and trenching – resist removal – RCA cleaning – SIPOS deposition – blade-scraping glass – glass passivation – LTO deposition – three-stage photolithography – mesa etching – surface metallization – testing – dicing – packaging steps to prepare a single 4-inch wafer. The resulting product is as follows: Figure 2 As shown. By Figure 2 It can be seen that, in Comparative Example 1, the presence of a glass layer at the bottom of the groove during cutting will damage the glass layer on the PN junction surface, thus compromising the reliability of the product.
[0050] Comparative Example 2
[0051] This comparative example uses spin-coating lithography to prepare a single 4-inch wafer. The total amount of spin-coated wafer used in this comparative example is 2.97g, with 0.94g remaining, which is a loss of 2.03g.
[0052] The following is a comparison of the amount of silicone sealant used (per sheet) and the amount wasted (per sheet) in the two methods of Example 1 and Comparative Example 2:
[0053] Example 1: Total usage: 0.96g, loss is negligible.
[0054] Comparative Example 2 spin coating lithography: total amount used 2.97g, loss amount 2.03g, loss rate 68.4wt.%.
[0055] Therefore, it can be seen that the glass adhesive used in this invention has almost no loss, and the amount used is only about 32% of that used in spin coating photolithography, which has a very significant effect on saving materials and reducing costs.
[0056] Comparative Example 3
[0057] In step (1) of this comparative example, ordinary lead-free glass silicate powder with an average particle size of 65 μm and a grinding time of 60 hours were used. Other settings were the same as in Example 1. After comparative testing and experiments, it was found that the adhesion decreased during the coating process after two uses, making it impossible to achieve more than three reuses. This was not the case in Example 1. Although the glass powder in Example 1 was lead-containing lead borosilicate glass powder, the amount used in Example 1 of this invention was small, and the reuse was almost lossless (no emissions), thus having virtually no significant adverse impact on the environment.
[0058] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a glass passivation protective layer, characterized in that, Includes the following steps: (1) Prepare materials. Prepare a mixture of photoresist and glass powder according to the weight ratio of photoresist to glass powder as (21~41): (38~58). The photoresist and glass powder are mixed by grinding to obtain a glass mixture. Prepare a silicon wafer substrate with a PN junction, wherein the silicon wafer substrate with a PN junction is a silicon wafer substrate with trenches and exposed PN junctions; (2) Coating: The glass mixture adhesive obtained in step (1) is coated onto the silicon wafer substrate with PN junction described in step (1) by printing. (3) Soft baking: Place the wafer obtained after coating in step (2) into a soft oven at a temperature of 80-120°C and keep it at 80-120°C for 15-35 minutes to obtain the soft-baked wafer. (4) Photolithography and development: The wafer obtained in step (3) is placed on an exposure machine for continuous exposure, then developed and fixed using a spray developer, and finally placed in an oven for baking to obtain the developed wafer. (5) Photoresist removal, glass sintering and LTO deposition: The wafer obtained in step (4) is placed in a photoresist removal furnace and kept at a temperature of 485~520℃ for 45~60min in an oxygen atmosphere to remove the photoresist on the wafer and retain the glass powder; then the wafer obtained after photoresist removal is directly transferred to a glass sintering furnace and kept at a temperature of 800~840℃ for 5~30min in a mixed atmosphere of oxygen and nitrogen to perform glass sintering, and the glass-sintered wafer is obtained after removal. Then, an LTO oxide film is deposited on the surface of the wafer after glass sintering. (6) Surface metallization: The mesa and back side of the wafer obtained in step (5) are photolithographically and etched to remove the oxygen-doped polysilicon thin film (SIPOS film) and / or oxide layer on the surface. During the removal of the oxygen-doped polysilicon thin film and / or oxide layer on the surface, an oxide layer is left around the edge of each mesa to expose the silicon on the mesa and the silicon on the back side. Then, surface metallization is performed on the exposed silicon to obtain a solderable wafer with a glass passivation protective layer.
2. The method for preparing the glass passivation protective layer according to claim 1, characterized in that, Includes the following steps: (1) Material preparation: Prepare a mixture of photoresist and glass powder according to a weight ratio of (21~41):(38~58), wherein the photoresist has a density of 0.86~0.89 g / cm³. 3 Negative photoresist; glass powder with a thermal expansion coefficient of (41~46)×10 at 30~300℃. -7 The lead borosilicate glass powder has a softening point of 660~698℃, a particle size ≤44µm, and a density of 3.68~3.88g / cm³. 3 Photoresist and glass powder are mixed by grinding to obtain a glass-mixed adhesive. Prepare a silicon wafer substrate with a PN junction, wherein the silicon wafer substrate with a PN junction is a silicon wafer substrate with trenches exposed to expose the PN junction, and the trench depth is 70~200µm and the trench width is 200~500µm. (2) Coating: The glass mixed adhesive obtained in step (1) is coated onto the silicon wafer substrate with PN junction described in step (1) by printing. The coating thickness of the glass mixed adhesive on the mesa of the silicon wafer substrate is 20~60µm, and the coating thickness of the glass mixed adhesive in the trench is 40~120µm. (3) Soft baking: Place the wafer obtained after coating in step (2) into a soft oven at a temperature of 80-120°C and keep it at 80-120°C for 15-35 minutes to obtain the soft-baked wafer. (4) Photolithography and development: The wafer obtained in step (3) is placed on an exposure machine and exposed for 1 to 10 seconds. Then, it is developed and fixed using a spray developer. Finally, it is placed in an oven at 130 to 150°C for 25 to 50 minutes to obtain the developed wafer. (5) Photoresist removal, glass sintering and LTO deposition: The wafer obtained in step (4) is placed in a photoresist removal furnace. The temperature of the photoresist removal furnace is maintained at 500~510℃ and in an oxygen atmosphere for 50~60 minutes to remove the photoresist on the wafer and retain the glass powder. Then the wafer obtained after photoresist removal is directly transferred to a glass sintering furnace, heated to 800~840℃, and in a mixed atmosphere of oxygen and nitrogen for 5~30 minutes to perform glass sintering. After removal, the glass-sintered wafer is obtained. Then, an LTO oxide film is deposited on the surface of the wafer after glass sintering. (6) Surface metallization: The mesa and back side of the wafer obtained in step (5) are photolithographically and etched to remove the oxygen-doped polysilicon thin film (SIPOS film) or oxide layer on the surface. During the removal of the oxygen-doped polysilicon thin film or oxide layer on the surface, an oxide layer is left around the edge of each mesa to expose the silicon on the mesa and the silicon on the back side. Then, surface metallization is performed on the exposed silicon to obtain a solderable wafer with a glass passivation protective layer.
3. The method for preparing the glass passivation protective layer according to claim 1 or 2, characterized in that, In step (2), the glass-mixed adhesive obtained in step (1) is applied to the silicon wafer substrate with a PN junction described in step (1) using a printing method. Specifically, this includes the following steps: I. The silicon wafer substrate with PN junction is placed on a printing press, and a printing screen is placed on top, with the center position of the mesh of the printing screen corresponding to the center position of the silicon wafer substrate. II. Place the glass mixture obtained in step (1) on one side of the printing screen mesh, and use a screen brush to reciprocate once in the same direction. The printing amount is such that the coating thickness of the glass mixture on the mesa of the silicon wafer substrate is 20~60µm and the coating thickness in the trench is 40~120µm. III. Raise the printing screen and remove the wafer obtained after coating.
4. The method for preparing the glass passivation protective layer according to claim 1 or 2, characterized in that, In step (1), the specific method for obtaining the glass mixed adhesive by grinding and mixing photoresist and glass powder is as follows: First, the photoresist and glass powder in a weight ratio of (21~41):(38~58) and alumina balls are placed together in a grinding jar and sealed. Then, the whole assembly is placed on a grinding mill. The rotation speed of the grinding jar body is set to 36~45 rpm and the grinding time is 24~59 hours. Then, the glass mixed adhesive obtained by grinding and mixing is poured out to obtain the glass mixed adhesive.
5. The method for preparing the glass passivation protective layer according to claim 2, characterized in that, In step (1), the upper plane between two adjacent trenches in the silicon wafer substrate with PN junction is the mesa of the silicon wafer substrate. All trench surfaces and mesa surfaces in the silicon wafer substrate with PN junction are covered with oxygen-doped polycrystalline silicon thin films or are not covered with oxygen-doped polycrystalline silicon thin films.
6. The method for preparing the glass passivation protective layer according to claim 2, characterized in that, The lead borosilicate glass powder mentioned in step (1) has a particle size of 10~44µm and a density of 3.78g / cm³. 3 The coefficient of thermal expansion is 44×10. -7 / K and the softening point temperature is 680℃; After step (2), the amount of photoresist and glass powder mixture retained in the wafer coated with glass adhesive is 92~98 wt.% of the amount of glass adhesive used.
7. The method for preparing the glass passivation protective layer according to claim 1 or 2, characterized in that, The surface metallization process in step (6) is as follows: a metal layer is deposited on silicon by chemical plating with a thickness of 0.1-2.0µm. The plated wafer is then placed in an oven for baking. The baked wafer is then placed in a metal sintering furnace for sintering to form an alloy layer. After cleaning, chemical plating is repeated once with a thickness of 0.1-2.0µm. The plated wafer is then placed in an oven for baking and removed to complete the surface metallization process.
8. A solderable wafer with a glass passivation protective layer, characterized in that, The solderable wafer with a glass passivation protective layer is prepared by the preparation method according to any one of claims 1 to 7.
9. The solderable wafer with a glass passivation protective layer according to claim 8, characterized in that, The wafer includes a silicon wafer substrate with a PN junction, a surface metal layer, an oxide layer, and a glass passivation protective layer. The silicon wafer substrate with the PN junction includes a trench and a mesa. The glass passivation protective layer extends from the outer end of the center of the bottom of the trench to the edge of the mesa. The surface metal layer is attached to the mesa. The oxide layer is disposed between the glass passivation protective layer and the surface metal layer on the mesa. The distance from the edge of the glass passivation protective layer at the bottom of the trench to the center of the bottom of the trench is 20~160µm. The width of the glass passivation protective layer extending from the same side of the glass at the bottom of the trench to the mesa is 70~150µm.
10. A chip, characterized in that, The chip includes the solderable wafer with a glass passivation protective layer as described in claim 9.
Citation Information
Patent Citations
Rectifier diodes, chips and their fabrication methods
CN104465330B
Printing glass passivation process method
CN114334793A
Glass passivating method of silicon planar semiconductor device