A perfluorinated sulfonic acid resin slurry and a proton exchange membrane for a flow battery and a method of making the same
The preparation of perfluorosulfonic acid resin slurry using high-pressure homogeneous dispersion technology solved the flowability and dispersibility problems of proton exchange membranes in flow batteries, improved the mechanical properties and chemical stability of the membrane, reduced ion permeability, and enhanced the performance of flow batteries.
Patent Information
- Application Number
- CN202311225543.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-21
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-09-21
AI Technical Summary
Existing proton exchange membranes for flow batteries suffer from problems such as high thickness requirements, poor flowability of perfluorosulfonic acid resin slurry, low mechanical properties due to uneven dispersion, and high ion permeability.
High-solids-content perfluorosulfonic acid resin slurry is prepared using high-pressure homogenization dispersion technology. The semi-finished perfluorosulfonic acid resin slurry is subjected to high-speed collisions in a flow-limiting gap of a specific width using a high-pressure homogenizer, which de-entangles and disperses it uniformly, resulting in a uniform distribution and orientation of perfluorosulfonic acid resin molecular chain segments, thereby improving its flowability and dispersibility.
It improves the uniformity and flowability of perfluorosulfonic acid resin slurry, reduces viscosity, enhances the mechanical properties and chemical stability of proton exchange membranes, reduces ion permeability, and improves the long cycle life and energy efficiency of flow batteries.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of flow battery technology, specifically relating to a perfluorosulfonic acid resin slurry and a proton exchange membrane for flow batteries, as well as their preparation methods. Background Technology
[0002] Currently developed renewable energy sources, such as solar and wind power, are limited by the natural environment, exhibiting instability and intermittency. Therefore, building large-scale energy storage systems is crucial for establishing clean and renewable energy systems. Flow batteries are one of the most effective energy storage technologies in the field of clean and renewable energy. Compared with other new energy storage technologies, flow batteries offer advantages such as long cycle life, deep discharge capability, operational safety, fast response speed, low environmental pollution, and low cost.
[0003] The working principle of a flow battery is that the reactive materials in the positive and negative electrodes circulate and undergo redox reactions in two separate electrolyte tanks to achieve the charging and discharging process. The electrolytes at the positive and negative electrodes are separated by a proton exchange membrane (PEM). As a crucial component of the flow battery, the PEM not only separates the electrolytes at the positive and negative electrodes to prevent cross-contamination but also transports protons to form a closed circuit. Therefore, the conductivity, ion permeability, ion exchange capacity, chemical stability, and mechanical strength of the PEM directly affect the energy efficiency and operational stability of the flow battery.
[0004] Currently, the proton exchange membranes used in commercially available flow batteries are generally thick perfluorosulfonic acid homogeneous membranes, which possess good chemical stability and proton conductivity. However, these membranes suffer from drawbacks such as high cost and high ion permeability, limiting their application in flow batteries. Perfluorosulfonic acid composite membranes, on the other hand, can reduce cross-permeation of active materials in the electrolyte to a certain extent, and the introduction of a reinforcing layer allows for a reduction in the amount of perfluorosulfonic acid resin used, effectively lowering the cost of the composite membrane. Summary of the Invention
[0005] This invention is based on the inventors' discoveries and understanding of the following facts and problems: Currently, the thickness of proton exchange membranes used in flow batteries in China is concentrated between 50-60 μm. The preparation of thicker perfluorosulfonic acid composite membranes typically employs solution casting. The most critical issues in this process are the wetting of the reinforcing layer by the perfluorosulfonic acid resin slurry and the processability of the perfluorosulfonic acid resin slurry. However, the preparation of thicker perfluorosulfonic acid composite membranes using solution casting is limited by the solid content and viscosity of the perfluorosulfonic acid resin slurry: because the proton exchange membranes in flow batteries require high thickness, the solid content of the perfluorosulfonic acid resin slurry usually needs to be higher than 20 wt%. As the solid content of the solution increases, its viscosity also increases. When the viscosity exceeds a certain value, the processing fluidity of the solution is poor, and it is difficult to wet the reinforcing layer. Therefore, perfluorosulfonic acid resin slurries with high solid content and low viscosity are more conducive to the wetting of the reinforcing layer by the resin layer and the formation of thicker proton exchange membranes.
[0006] Furthermore, domestically produced perfluorosulfonic acid resins generally have a wide molecular weight distribution. When preparing high-solids-content perfluorosulfonic acid resin slurries, the slurry viscosity is high, and the flowability is poor. Additionally, some high molecular weight resins are difficult to dissolve, resulting in poor slurry dissolution and dispersion. If such high-solids-content, wide-molecular-weight perfluorosulfonic acid resin slurries are used directly for film formation, the resulting proton exchange membrane will have poor uniformity, low mechanical properties, and high ion permeability. Therefore, solving the dissolution and dispersion problem of high-solids-content, wide-molecular-weight perfluorosulfonic acid resin slurries is of great practical significance for the proton exchange membrane formation process.
[0007] This invention aims to at least partially solve one of the technical problems in related technologies. To this end, embodiments of this invention provide a perfluorosulfonic acid resin slurry and a proton exchange membrane for flow batteries, as well as a method for preparing the same.
[0008] This invention provides a method for preparing a perfluorosulfonic acid resin slurry, comprising the following steps:
[0009] (1) Dissolve and disperse perfluorosulfonic acid resin in a mixed solvent to obtain a semi-finished perfluorosulfonic acid resin slurry;
[0010] (2) The semi-finished perfluorosulfonic acid resin slurry is added to a high-pressure homogenizer for high-pressure homogenization to obtain perfluorosulfonic acid resin slurry.
[0011] The advantages and technical effects of the method for preparing perfluorosulfonic acid resin slurry according to embodiments of the present invention are as follows:
[0012] The preparation method of this invention uses high-pressure homogenization dispersion technology to prepare high-solids-content perfluorosulfonic acid resin slurry. The semi-finished perfluorosulfonic acid resin slurry is passed through a flow-limiting gap of a specific width and then collided at high speed in a homogenizing valve using a high-pressure homogenizer. This causes the perfluorosulfonic acid resin molecular chains to de-entangle and disperse uniformly under the effects of cavitation, collision, and shearing. The resulting perfluorosulfonic acid resin slurry has a uniformly distributed and oriented molecular chain segment, resulting in high uniformity, low viscosity, and good flowability. Furthermore, the preparation method of this invention is simple and easy to implement, facilitating the scale-up of casting production processes.
[0013] In some embodiments, in step (1), the mixed solvent is a mixture of water, alcohol and a high-boiling-point solvent, wherein the water is 30-70% by mass, the alcohol is 30-70% by mass, and the high-boiling-point solvent is 0-20% by mass, based on the total mass of the mixed solvent being 100%.
[0014] In some embodiments, in step (1), the alcohol is at least one of ethanol, isopropanol and n-propanol; the high-boiling solvent is dimethylacetamide and / or dimethyl sulfoxide.
[0015] In some embodiments, in step (1), the solid content of the semi-finished perfluorosulfonic acid resin slurry is 20-40 wt%, and the viscosity is 280-1000 mPa·s.
[0016] In some embodiments, in step (2), the working pressure of the high-pressure homogenizer is 400-1200 bar, the working temperature is 20-25°C; and / or, the number of high-pressure homogenization processes is 1-10.
[0017] In some embodiments, in step (2), the solid content of the perfluorosulfonic acid resin slurry is 20-40 wt%, and the viscosity is 100-800 mPa·s.
[0018] In addition, this embodiment of the invention also provides a perfluorosulfonic acid resin slurry, which is prepared by the preparation method of this embodiment of the invention.
[0019] The advantages and technical effects of the perfluorosulfonic acid resin slurry of this invention are as follows:
[0020] Compared with semi-finished perfluorosulfonic acid resin slurry that has not undergone high-pressure homogenization, the perfluorosulfonic acid resin slurry of the present invention has high uniformity of dispersion, low viscosity, and good fluidity because the molecular chain segments in the perfluorosulfonic acid resin slurry of the present invention are uniformly distributed and oriented.
[0021] In addition, this invention also provides a method for preparing a proton exchange membrane for a flow battery, comprising the following steps: coating the perfluorosulfonic acid resin slurry of this invention onto both sides of the reinforcing layer, and then performing heat treatment to obtain the proton exchange membrane.
[0022] The advantages and technical effects of the method for preparing the proton exchange membrane for flow batteries according to embodiments of the present invention are as follows:
[0023] Compared with direct coating of semi-finished perfluorosulfonic acid resin slurry without high-pressure homogenization, coating of film with perfluorosulfonic acid resin slurry according to the embodiments of the present invention is more conducive to the wetting of the resin layer on the reinforcing layer and the formation of a thicker proton exchange membrane.
[0024] In some embodiments, the coating method includes blade coating, roller coating, slot coating, or spray coating; the heat treatment temperature is 80-180°C, and the heat treatment time is 10-60 min; the thickness of the proton exchange membrane is 50-60 μm.
[0025] Furthermore, this invention also provides a proton exchange membrane for a flow battery, which is prepared by the preparation method of this invention.
[0026] The advantages and technical effects of the proton exchange membrane for flow batteries according to the embodiments of the present invention are as follows:
[0027] Compared with proton exchange membranes obtained by directly coating semi-finished perfluorosulfonic acid resin slurry without high-pressure homogenization, the proton exchange membranes of the present invention have a more compact structure, reduced swelling, and improved mechanical properties. While reducing ion permeation, they also improve the physicochemical stability of the membrane, which is beneficial to improving the long cycle life and energy efficiency of flow batteries. Detailed Implementation
[0028] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0029] This invention provides a method for preparing a perfluorosulfonic acid resin slurry, comprising the following steps:
[0030] (1) Dissolve and disperse perfluorosulfonic acid resin in a mixed solvent to obtain a semi-finished perfluorosulfonic acid resin slurry;
[0031] (2) The semi-finished perfluorosulfonic acid resin slurry is added to a high-pressure homogenizer for high-pressure homogenization to obtain perfluorosulfonic acid resin slurry.
[0032] The preparation method of this invention uses high-pressure homogenization dispersion technology to prepare high-solids-content perfluorosulfonic acid resin slurry. The semi-finished perfluorosulfonic acid resin slurry is passed through a flow-limiting gap of a specific width and then collided at high speed in a homogenizing valve using a high-pressure homogenizer. This causes the perfluorosulfonic acid resin molecular chains to de-entangle and disperse uniformly under the effects of cavitation, collision, and shearing. The resulting perfluorosulfonic acid resin slurry has a uniformly distributed and oriented molecular chain segment, resulting in high uniformity, low viscosity, and good flowability. Furthermore, the preparation method of this invention is simple and easy to implement, facilitating the scale-up of casting production processes.
[0033] The preparation method of perfluorosulfonic acid resin slurry in this embodiment of the invention does not particularly limit the type of mixed solvent in step (1). Any mixed solvent commonly used in perfluorosulfonic acid resin slurry in related technologies can be used, as long as it can dissolve and disperse the perfluorosulfonic acid resin. If a single solvent is used to dissolve the perfluorosulfonic acid resin, it will be difficult for the perfluorosulfonic acid resin slurry to form a film in the future. Therefore, a mixed solvent is selected in step (1) of the preparation method in this embodiment of the invention.
[0034] In some embodiments, in step (1), the mixed solvent is a mixture of water, alcohol, and a high-boiling-point solvent. Based on the total mass of the mixed solvent as 100%, the mass percentage of water is 30-70%, for example, 30%, 40%, 50%, 60%, 70%, etc.; the mass percentage of alcohol is 30-70%, for example, 30%, 40%, 50%, 60%, 70%, etc.; and the mass percentage of the high-boiling-point solvent is 0-20%, for example, 0%, 2%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, etc. Considering the film-forming performance of the proton exchange membrane, preferably, the mixed solvent is a mixture of water and alcohol, or the mixed solvent is a mixture of water, alcohol, and a high-boiling-point solvent. The mixed solvent of water and alcohol has good solubility for perfluorosulfonic acid resins. Optionally, the high-boiling-point solvent can further improve the solubility of perfluorosulfonic acid resins on the one hand, and improve the casting processability and film uniformity of the perfluorosulfonic acid resin slurry on the other hand. Because the high-boiling-point solvent accounts for a small proportion of the entire solvent system (0-20%), it can be completely volatilized through heat treatment during the subsequent preparation of the proton exchange membrane, and will not remain in the proton exchange membrane to affect its performance.
[0035] In some embodiments, in step (1), the alcohol is at least one of ethanol, isopropanol, and n-propanol. The mixed solvent also contains a high-boiling-point solvent, such as dimethylacetamide and / or dimethyl sulfoxide. The above-mentioned alcohols and high-boiling-point solvents have good solubility for perfluorosulfonic acid resins, which can effectively improve the casting processability and film uniformity of perfluorosulfonic acid resin slurries.
[0036] In some embodiments, in step (1), the solid content of the semi-finished perfluorosulfonic acid resin slurry is 20-40 wt%, such as 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, etc., and the viscosity is 280-1000 mPa·s, such as 280 mPa·s, 300 mPa·s, 400 mPa·s, 500 mPa·s, 600 mPa·s, 700 mPa·s, 800 mPa·s, 900 mPa·s, 1000 mPa·s, etc. After high-pressure homogenization, the semi-finished perfluorosulfonic acid resin slurry that meets the above conditions obtains a perfluorosulfonic acid resin slurry with a solid content of 20-40 wt% and a viscosity of 100-800 mPa·s. The perfluorosulfonic acid resin slurry with high solid content and low viscosity is more conducive to coating and forming a thicker proton exchange membrane.
[0037] In some embodiments, in step (2), the working pressure of the high-pressure homogenizer is 400-1200 bar, such as 400 bar, 500 bar, 600 bar, 700 bar, 800 bar, 900 bar, 1000 bar, 1100 bar, 1200 bar, etc., and the working temperature is 20-25℃, such as 20℃, 21℃, 22℃, 23℃, 24℃, 25℃, etc. When the working pressure of the high-pressure homogenizer is too low, it is not conducive to reducing the molecular weight distribution width of the perfluorosulfonic acid resin, and thus not conducive to improving the uniform dispersion and flowability of the perfluorosulfonic acid resin slurry and reducing the viscosity of the slurry. When the working pressure of the high-pressure homogenizer is too high, the improvement effect on the uniform dispersion, flowability and viscosity of the perfluorosulfonic acid resin slurry is no longer significantly improved, which is not conducive to cost reduction and efficiency improvement. When the operating temperature of the high-pressure homogenizer is too high, the mixed solvent may partially evaporate, which is not conducive to obtaining perfluorosulfonic acid resin slurry with the target solid content and viscosity range. Therefore, the operating temperature of the high-pressure homogenizer is preferably room temperature.
[0038] In some embodiments, the high-pressure homogenization process in step (2) is repeated 1-10 times, for example, 1 time, 2 times, 4 times, 6 times, 8 times, 10 times, etc. A single high-pressure homogenization process is sufficient to obtain the perfluorosulfonic acid resin slurry. However, repeating the process multiple times can further improve the homogenization and dispersion effect.
[0039] In some embodiments, in step (2), the solid content of the perfluorosulfonic acid resin slurry is 20-40 wt%, such as 20 wt%, 22 wt%, 24 wt%, 26 wt%, 28 wt%, 30 wt%, 32 wt%, 34 wt%, 36 wt%, 38 wt%, 40 wt%, etc., and the viscosity is 100-800 mPa·s, such as 100 mPa·s, 200 mPa·s, 300 mPa·s, 400 mPa·s, 500 mPa·s, 600 mPa·s, 700 mPa·s, 800 mPa·s, etc. The high solid content and low viscosity perfluorosulfonic acid resin slurry described above is more conducive to coating and forming a thicker proton exchange membrane.
[0040] In addition, this embodiment of the invention also provides a perfluorosulfonic acid resin slurry, which is prepared by the preparation method of this embodiment of the invention.
[0041] Compared with semi-finished perfluorosulfonic acid resin slurry that has not undergone high-pressure homogenization, the perfluorosulfonic acid resin slurry of the present invention has high uniformity of dispersion, low viscosity, and good fluidity because the molecular chain segments in the perfluorosulfonic acid resin slurry of the present invention are uniformly distributed and oriented.
[0042] In addition, this invention also provides a method for preparing a proton exchange membrane for a flow battery, comprising the following steps: coating the perfluorosulfonic acid resin slurry of this invention onto both sides of the reinforcing layer, and then performing heat treatment to obtain the proton exchange membrane.
[0043] Compared with direct coating of semi-finished perfluorosulfonic acid resin slurry without high-pressure homogenization, coating of film with perfluorosulfonic acid resin slurry according to the embodiments of the present invention is more conducive to the wetting of the resin layer on the reinforcing layer and the formation of a thicker proton exchange membrane.
[0044] The preparation method of the proton exchange membrane in this embodiment of the invention does not have any particular limitation on the coating method of the perfluorosulfonic acid resin slurry, as long as it can form a uniform film. For example, it can be coated by scraping, rolling, slot coating or spraying.
[0045] In some embodiments, the heat treatment temperature is 80-180°C, such as 80°C, 100°C, 120°C, 140°C, 160°C, 180°C, etc., and the heat treatment time is 10-60 minutes, such as 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, etc. Performing the heat treatment at these temperatures effectively volatilizes the mixed solvent in the coating layer, forming a resin layer on the reinforcing layer. It is understood that the specific heat treatment temperature can be set according to the type of mixed solvent in the perfluorosulfonic acid resin slurry. For example, when the mixed solvent consists of water and alcohol, the heat treatment can be performed at 80-110°C. When the mixed solvent contains a high-boiling-point solvent, the heat treatment can be performed at 160-180°C. The heat treatment time needs to be set according to the heat treatment temperature. For example, when the heat treatment temperature is relatively high, the heat treatment time can be relatively short; conversely, when the heat treatment temperature is relatively low, the heat treatment time can be relatively long.
[0046] In some embodiments, the thickness of the proton exchange membrane is 50-60 μm, such as 50 μm, 52 μm, 54 μm, 56 μm, 58 μm, 60 μm, etc. When the thickness of the proton exchange membrane is too small, it is detrimental to improving the chemical stability and proton conductivity of the proton exchange membrane. When the thickness of the proton exchange membrane is too large, it increases the ohmic impedance of the flow battery, which is detrimental to improving the charge-discharge performance of the flow battery.
[0047] Furthermore, this invention also provides a proton exchange membrane for a flow battery, which is prepared by the preparation method of this invention.
[0048] Compared with proton exchange membranes obtained by directly coating semi-finished perfluorosulfonic acid resin slurry without high-pressure homogenization, the proton exchange membranes of the present invention have a more compact structure, reduced swelling, and improved mechanical properties. While reducing ion permeability, they also improve the physicochemical stability of the membrane, which is beneficial to improving the long cycle life and energy efficiency of flow batteries.
[0049] The present invention will now be described in detail with reference to the embodiments.
[0050] Example 1
[0051] A perfluorosulfonic acid resin slurry and its preparation method, the preparation method comprising the following steps:
[0052] (1) Preparation of semi-finished perfluorosulfonic acid resin slurry: Weigh 9.2g of perfluorosulfonic acid resin and dissolve it in 30.8g of a mixed solvent composed of water, isopropanol and dimethyl sulfoxide (DMSO), wherein the mass ratio of water, isopropanol and DMSO is 1:1:0.5, and a semi-finished perfluorosulfonic acid resin slurry with a solid content of 23wt% is obtained.
[0053] (2) High-pressure homogenization process: The above semi-finished perfluorosulfonic acid resin slurry is added to a high-pressure homogenizer with a working pressure of 400 bar and a working temperature of 25°C and homogenized and dispersed once to obtain perfluorosulfonic acid resin slurry.
[0054] Application Example 1
[0055] A proton exchange membrane for flow batteries and its preparation method are disclosed. The preparation method includes the following steps: the perfluorosulfonic acid resin slurry obtained in Example 1 is coated onto a PET substrate with a doctor blade, covered with an expanded polytetrafluoroethylene membrane (ePTFE), dried at 80°C for 10 min, and then another layer of the perfluorosulfonic acid resin slurry obtained in Example 1 is coated on top. Finally, the membrane is heat-treated at 160°C for 20 min to obtain a proton exchange membrane with a thickness of 50 μm.
[0056] Example 2
[0057] A perfluorosulfonic acid resin slurry and its preparation method, the preparation method comprising the following steps:
[0058] (1) Preparation of semi-finished perfluorosulfonic acid resin slurry: Weigh 10g of perfluorosulfonic acid resin and dissolve it in 30g of a mixed solvent composed of water, isopropanol and dimethyl sulfoxide (DMSO), wherein the mass ratio of water, isopropanol and DMSO is 1:1:0.5, to obtain a semi-finished perfluorosulfonic acid resin slurry with a solid content of 25wt%.
[0059] (2) High pressure homogenization process: The above semi-finished perfluorosulfonic acid resin slurry is added to a high pressure homogenizer with a working pressure of 600 bar and a working temperature of 25°C, and the homogenization and dispersion are repeated 3 times to finally obtain the perfluorosulfonic acid resin slurry.
[0060] Application Example 2
[0061] A proton exchange membrane for flow batteries and its preparation method are disclosed. The preparation method includes the following steps: the perfluorosulfonic acid resin slurry obtained in Example 2 is coated onto a PET substrate with a doctor blade, covered with an expanded polytetrafluoroethylene membrane (ePTFE), dried at 80°C for 10 min, and then another layer of the perfluorosulfonic acid resin slurry obtained in Example 2 is coated on top. Finally, the membrane is heat-treated at 160°C for 20 min to obtain a proton exchange membrane with a thickness of 50 μm.
[0062] Comparative Example 1
[0063] A perfluorosulfonic acid resin slurry and its preparation method are disclosed. The preparation method includes the following steps: weighing 9.2g of perfluorosulfonic acid resin and dissolving it in 30.8g of a mixed solvent composed of water, isopropanol and dimethyl sulfoxide (DMSO), wherein the mass ratio of water, isopropanol and DMSO is 1:1:0.5, to obtain a perfluorosulfonic acid resin slurry with a solid content of 23wt%.
[0064] Application Comparative Example 1
[0065] A proton exchange membrane for flow batteries and its preparation method are disclosed. The preparation method includes the following steps: applying a perfluorosulfonic acid resin slurry prepared in Comparative Example 1 onto a PET substrate using a doctor blade, covering it with an expanded polytetrafluoroethylene membrane (ePTFE), drying it at 80°C for 10 min, applying another layer of the perfluorosulfonic acid resin slurry prepared in Comparative Example 1 on top, and then heat-treating it at 160°C for 20 min to finally obtain a proton exchange membrane with a thickness of 50 μm.
[0066] Comparative Example 2
[0067] A perfluorosulfonic acid resin slurry and its preparation method are disclosed. The preparation method includes the following steps: weighing 10g of perfluorosulfonic acid resin and dissolving it in a mixed solvent composed of 30g of water, isopropanol and dimethyl sulfoxide (DMSO), wherein the mass ratio of water, n-propanol and DMSO is 1:1:0.5, to obtain a perfluorosulfonic acid resin slurry with a solid content of 25wt%.
[0068] Application Comparative Example 2
[0069] A proton exchange membrane for flow batteries and its preparation method are disclosed. The preparation method includes the following steps: the perfluorosulfonic acid resin slurry prepared in Comparative Example 2 is coated onto a PET substrate using a doctor blade, covered with an expanded polytetrafluoroethylene membrane (ePTFE), dried at 80°C for 10 min, and then coated with another layer of the perfluorosulfonic acid resin slurry prepared in Comparative Example 2. Finally, the membrane is heat-treated at 160°C for 20 min to obtain a proton exchange membrane with a thickness of 50 μm.
[0070] Performance testing:
[0071] (1) The viscosity of the perfluorosulfonic acid resin slurries of Examples 1-2 and Comparative Examples 1-2 was tested. The slurry properties are shown in Table 1. The viscosity of the perfluorosulfonic acid resin slurry was tested by rheometer at a constant shear rate.
[0072] (2) The mechanical properties, swelling ratio and vanadium ion permeability of the proton exchange membranes of Application Examples 1-2 and Application Comparative Examples 1-2 were tested. The membrane properties are shown in Table 1.
[0073] Mechanical property testing: The prepared proton exchange membrane was cut at equal intervals along both the length (MD) and width (TD) of the test material, and cut into dumbbell shapes of a certain size according to GB / T1040.3. The edges of the samples should be smooth and without gaps. A universal testing machine was used for testing, with the tensile rate set to 50 mm / min. The mechanical properties of the samples were characterized by measuring the tensile strength, elastic modulus, tensile stress at break, and tensile strain at break. Three parallel tests were performed on the same sample, and the results were averaged.
[0074] Swelling rate test: Three samples of the prepared proton exchange membrane with an area of 4cm×4cm were cut, and their original length (TD) and width (MD) were measured under laboratory ambient temperature and humidity. Then, the samples were immersed in 3mol / L sulfuric acid at 80℃ for 1h, and their wet length (TD) and wet width (MD) were measured after removal, and the swelling rate was calculated.
[0075] Vanadium ion permeability test: The prepared proton exchange membrane was cut into 5cm × 5cm samples and assembled into a cavity with an effective volume of 4cm × 4cm × 5cm. One side of the cavity was filled with a 1.5 mol / L VOSO4 and 3 mol / L H2SO4 aqueous solution, and the permeation side cavity was filled with a 1.5 mol / L Mg2SO4 and 3 mol / L H2SO4 aqueous solution. 3 mL of solution was taken from the permeation side and added to a cuvette. The VO ion permeability of the sample was analyzed using a UV-Vis spectrophotometer. 2+ The concentration of vanadium ions was measured. After the test, the solution was poured back to the osmotic side of the conduction cell. Data was recorded every 30 minutes initially, and then every 20 minutes thereafter, for a total of 6 data points over 2 hours. The change in vanadium ion concentration in the right semi-osmotic cell was obtained through sampling tests, and the VO2+ of the proton exchange membrane was calculated. 2+ Penetration rate.
[0076] Table 1. Slurry properties and applications of perfluorosulfonic acid resin slurries in Examples 1-2 and Comparative Examples 1-2. Membrane properties of proton exchange membranes in Examples 1-2 and Comparative Examples 1-2.
[0077]
[0078] From the comparison of Example 1 and Comparative Example 1 in Table 1, and the comparison of Example 2 and Comparative Example 2, it can be seen that Examples 1-2 use high-pressure homogenization technology to homogenize and disperse the semi-finished perfluorosulfonic acid resin slurry, which solves the film formation problem of thick perfluorosulfonic acid composite films. Moreover, the method is simple and easy to scale up for production. It can obtain a uniformly dispersed perfluorosulfonic acid resin slurry with suitable viscosity without adding any additives.
[0079] From the comparison of Application Example 1 and Application Comparative Example 1 in Table 1, and the comparison of Application Example 2 and Application Comparative Example 2, it can be seen that compared with the proton exchange membranes prepared by Application Comparative Examples 1-2 using slurry without high-pressure homogenization, the proton exchange membranes prepared by Application Examples 1-2 using perfluorosulfonic acid resin slurry obtained after high-pressure homogenization have significantly improved mechanical properties due to the uniform distribution and orientation of perfluorosulfonic acid resin molecular chain segments. Among them, the tensile strength and elastic modulus are greatly increased, and the ion permeability and swelling rate of the proton exchange membrane are significantly reduced. The above performance improvements are beneficial to the long-cycle durability of proton exchange membranes used in flow batteries.
[0080] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0081] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a perfluorosulfonic acid resin slurry for a proton exchange membrane in a flow battery, characterized in that, Includes the following steps: (1) Dissolve and disperse perfluorosulfonic acid resin in a mixed solvent to obtain a semi-finished perfluorosulfonic acid resin slurry; wherein the solid content of the semi-finished perfluorosulfonic acid resin slurry is 20-40 wt% and the viscosity is 280-1000 mPa·s. (2) The semi-finished perfluorosulfonic acid resin slurry is added to a high-pressure homogenizer for high-pressure homogenization to obtain perfluorosulfonic acid resin slurry; wherein the working pressure of the high-pressure homogenizer is 400-1200 bar.
2. The method for preparing perfluorosulfonic acid resin slurry according to claim 1, characterized in that, In step (1), the mixed solvent is a mixture of water, alcohol and high-boiling-point solvent. Based on the total mass of the mixed solvent as 100%, the mass percentage of water is 30-70%, the mass percentage of alcohol is 30-70%, and the mass percentage of high-boiling-point solvent is 0-20%.
3. The method for preparing perfluorosulfonic acid resin slurry according to claim 2, characterized in that, In step (1), the alcohol is at least one of ethanol, isopropanol and n-propanol; the high-boiling solvent is dimethylacetamide and / or dimethyl sulfoxide.
4. The method for preparing perfluorosulfonic acid resin slurry according to claim 1, characterized in that, In step (2), the operating temperature of the high-pressure homogenizer is 20-25 ℃; and / or, the number of high-pressure homogenization processes is 1-10.
5. The method for preparing perfluorosulfonic acid resin slurry according to claim 1 or 4, characterized in that, In step (2), the solid content of the perfluorosulfonic acid resin slurry is 20-40 wt%, and the viscosity is 100-800 mPa·s.
6. A perfluorosulfonic acid resin slurry, characterized in that, It is prepared by the preparation method according to any one of claims 1-5.
7. A method for preparing a proton exchange membrane for a flow battery, characterized in that, The process includes the following steps: applying the perfluorosulfonic acid resin slurry of claim 6 to both sides of the reinforcing layer, and then performing heat treatment to obtain the proton exchange membrane.
8. The method for preparing a proton exchange membrane for a flow battery according to claim 7, characterized in that, The coating method includes scraping, roller coating, slot coating or spraying; the heat treatment temperature is 80-180 ℃, the heat treatment time is 10-60 min; the thickness of the proton exchange membrane is 50-60 μm.
9. A proton exchange membrane for use in a flow battery, characterized in that, It is prepared by the preparation method described in claim 7 or 8.
Citation Information
Patent Citations
Inorganic-organic self-repairing proton exchange membrane for fuel cells and preparation method
CN108336385A
Perfluorosulfonic acid composite membrane as well as preparation method and application thereof
CN115663391A