Separator for secondary battery, method for manufacturing the same, secondary battery, battery module, battery pack, and electric device
By setting a nanofiber layer containing lithium replenishing agent, polymer and conductive material on the surface of the secondary battery separator substrate, the problems of low lithium replenishing agent utilization efficiency and lithium ion migration obstruction in the prior art are solved, thereby improving battery capacity and extending battery life.
Patent Information
- Application Number
- CN202280040851.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-01-30
AI Technical Summary
In existing composite separators for secondary batteries, the utilization efficiency of lithium replenishment agents is not high, and lithium ion migration is hindered, resulting in battery capacity decay and low initial coulombic efficiency.
A nanofiber layer is formed on the surface of the membrane substrate layer. The nanofiber layer contains lithium replenishing agent, polymer and conductive material, and is formed by electrospinning technology to ensure that the lithium replenishing agent is slowly released and participates in the negative electrode film formation reaction, thereby improving lithium ion mobility and utilization efficiency.
It significantly improves the initial coulombic efficiency of the secondary battery, reduces battery capacity decay, extends battery life, and enhances the battery's cycle performance and kinetic performance.
Smart Images

Figure CN117461203B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of secondary battery technology, and in particular to a separator for secondary batteries, a method for preparing the separator, and a secondary battery, battery module, battery pack, and power-consuming device including the separator. Background Technology
[0002] In recent years, with the increasingly widespread application of lithium-ion batteries, they have been widely used in energy storage power systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and many other fields. Due to the significant advancements in lithium-ion battery technology, higher requirements have been placed on its energy density, cycle performance, and safety performance.
[0003] Lithium replenishing agents have been applied to separators in rechargeable batteries to form composite separators including a lithium replenishing agent layer, aiming to improve the initial discharge capacity of rechargeable batteries, reduce capacity decay, and extend battery life. Currently, lithium replenishing agents can include a core and an organic-inorganic shell. The core comprises a lithium-rich compound, and the organic-inorganic shell can include polymers and inorganic compounds containing silicon-oxygen bonds. Coating the core surface of the lithium replenishing agent with an organic-inorganic shell serves two purposes: it provides a coating effect, isolating the core from air / oxygen, and it allows the core to be released after electrolyte injection. The lithium-rich compound in the core can participate in the negative electrode film formation reaction, forming an SEI film on the negative electrode surface, thereby reducing irreversible lithium consumption at the positive electrode and thus improving the initial discharge capacity. Simultaneously, the lithium-rich compound from the core can also act as active lithium. When active lithium is insufficient during cycling, this active lithium stored in the negative electrode can promptly participate in the electrochemical reaction, thereby reducing battery capacity decay and extending battery life.
[0004] However, in existing core-shell structures, the outer inorganic-organic shell layer hinders the electron conduction pathway of the lithium-rich compound in the core, making it difficult for the lithium-rich oxide to participate in the oxidation reaction during formation, resulting in low utilization efficiency of the lithium replenisher. Furthermore, in composite membranes, the lithium replenisher layer is coated on the surface of the membrane substrate, inevitably clogging the pores in the membrane substrate and hindering lithium ion migration within the membrane. Moreover, the organic-inorganic shell layer on the surface of the lithium replenisher swells / dissolves under the action of the electrolyte. While lithium ions in the core are gradually released to control the lithium replenishment rate, substances such as methyl orthosilicate, ethyl orthosilicate, and propyl orthosilicate also dissolve, increasing the viscosity of the electrolyte and thus hindering lithium ion migration within the electrolyte.
[0005] Therefore, existing composite separators still need improvement in terms of enhancing the utilization efficiency of lithium replenishment agents while ensuring adequate lithium-ion migration within the battery. Summary of the Invention
[0006] In view of the above-mentioned problems existing in the prior art, the purpose of this application is to provide a separator for secondary batteries that significantly improves the utilization efficiency of lithium replenishing agents and the migration rate of lithium ions, thereby improving the initial coulombic efficiency of secondary batteries using the separator and reducing battery capacity decay.
[0007] To achieve the above objectives, in one aspect, this application provides a separator for secondary batteries, comprising: Substrate layer; and A nanofiber layer disposed on one surface of the substrate layer. The nanofiber layer comprises a lithium supplement, a polymer, and an optional conductive material, wherein, relative to the total weight of the nanofiber layer, the lithium supplement contains 30.0 to 50.0% by weight, the polymer contains 50.0 to 70.0% by weight, and the conductive material contains 0 to 5.0% by weight.
[0008] Therefore, by providing a nanofiber layer comprising a lithium replenishing agent, a polymer, and optionally a conductive material as a lithium replenishing agent layer on one surface of the separator substrate layer, the separator of this application, when applied to a secondary battery, allows the lithium replenishing agent to be slowly released from the nanofiber layer during liquid injection formation and participate in the negative electrode film formation reaction, thus playing a lithium replenishing role. More importantly, in the separator for secondary batteries of this application, the nanofiber layer serving as the lithium replenishing agent layer has a unique nanofiber structure, which can fully ensure the continuous lithium-ion migration of the lithium replenishing agent in the nanofiber layer. The polymer in the nanofiber layer works synergistically with the lithium replenishing agent to improve the utilization efficiency of the lithium replenishing agent, thereby increasing the initial discharge capacity of the battery and reducing battery capacity decay. The optional conductive material in the nanofiber layer can increase the electronic pathway of the lithium replenishing agent within the nanofiber layer, further improving the utilization efficiency of the lithium replenishing agent, thereby further increasing the initial discharge capacity of the battery and further reducing battery capacity decay.
[0009] In any embodiment, the conductive material includes a zero-dimensional conductive material and optionally a one-dimensional conductive material, and the content of the zero-dimensional conductive material is 1.0 to 5.0% by weight relative to the total weight of the nanofiber layer, and the content of the one-dimensional conductive material is 0 to 0.3% by weight.
[0010] In any embodiment, the zero-dimensional conductive material has a particle size of 30-50 nm. Optionally, the zero-dimensional conductive material is selected from one or more of carbon black, acetylene black, and Ketjen black.
[0011] In any embodiment, the one-dimensional conductive material has an aspect ratio of 500 to 1000. Optionally, the one-dimensional conductive material is a carbon nanotube, which may be a single-arm nanotube, a multi-arm nanotube, or a combination of both.
[0012] In any embodiment, the lithium supplement is selected from Li₂C₂O₄, C₄BLiO₈, Li 15 Si4, Li4Sn, Li2NiO2, LiF, Li2TiO3, Li2CrO4, Li2Cr2O7, Li4SiO4, Li2SiO3, Li3AsO4, Li2SeO4, Li2SeO3, LiVO3, LiAlO2, Li3PO4, Li2B8O 13 One or more of Li2B4O7, LiBO2, Li3AlF6, Li2SnF6 and LiAsF6, and optionally one or more of Li2NiO2, Li4Sn and LiAsF6.
[0013] In any embodiment, the particle size of the lithium supplement is 50~200 nm, and can be selected as 80~150 nm.
[0014] In any embodiment, the amount of the lithium supplement is 40 to 100 parts by weight relative to 100 parts by weight of the polymer, optionally 60 to 80 parts by weight.
[0015] In any embodiment, the amount of the zero-dimensional conductive material is 1 to 12.5 parts by weight relative to 100 parts by weight of the lithium replenishing agent; and the amount of the one-dimensional conductive material is 0.15 to 0.75 parts by weight.
[0016] In any embodiment, the polymer is selected from one or more of polyvinylidene chloride, polyimide, polyacrylonitrile, and polystyrene.
[0017] In any embodiment, the diameter of the nanofibers in the nanofiber layer is 100~500 nm, and can be selected as 200~250 nm.
[0018] In any embodiment, the thickness of the nanofiber layer is 1.0~5.0 μm, and can be selected as 1.5~2.5 μm.
[0019] In any embodiment, the porosity of the nanofiber layer is above 80%.
[0020] In a second aspect, this application provides a method for preparing a separator for secondary batteries, comprising: The polymer is dissolved in a solvent to obtain a polymer solution; The polymer solution is added to a lithium supplement or a blend of a lithium supplement and a conductive material, and then dispersed at high speed to obtain a dispersion. The dispersion is attached to one surface of the substrate layer by electrospinning to form a nanofiber layer. In the nanofiber layer, relative to the total weight of the nanofiber layer, the content of the lithium supplement is 30.0~50.0% by weight, the content of the polymer is 50.0~70.0% by weight, and the content of the conductive material is 0~5% by weight.
[0021] In any embodiment, the solid content of the polymer solution is 20-40% by weight, optionally 20-25% by weight.
[0022] In any embodiment, the thickness of the nanofiber layer is 1.0~5.0 μm, and can be selected as 1.5~2.5 μm.
[0023] In a third aspect, this application provides a secondary battery comprising: positive electrode; negative electrode; Electrolytes; and The diaphragm of the first aspect of this application, wherein The nanofiber layer is disposed on the surface of the substrate layer facing the positive electrode.
[0024] In a fourth aspect, this application provides a battery module that includes the secondary battery of the third aspect of this application.
[0025] In a fifth aspect, this application provides a battery pack that includes the battery module of the fourth aspect of this application.
[0026] In a sixth aspect, this application provides an electrical device comprising at least one of the secondary battery of the third aspect of this application, the battery module of the fourth aspect of this application, and the battery pack of the fifth aspect of this application.
[0027] In the separator for secondary batteries of this application, by providing a nanofiber layer comprising a lithium replenisher, a polymer, and optionally a conductive material as a lithium replenisher layer in the form of a nanofiber layer with high porosity, the utilization efficiency of the lithium replenisher is significantly improved, and the migration rate of lithium ions is also increased, thereby significantly improving the initial coulombic efficiency of the secondary battery using the separator and reducing the capacity decay of the battery. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the diaphragm according to one embodiment of this application.
[0029] Figure 2 This is a schematic diagram of the nanofibers in the nanofiber layer of the diaphragm according to one embodiment of this application.
[0030] Figure 3 This is a schematic diagram of a secondary battery according to one embodiment of this application.
[0031] Figure 4 yes Figure 3 An exploded view of a secondary battery according to one embodiment of this application is shown.
[0032] Figure 5 This is a schematic diagram of a battery module according to one embodiment of this application.
[0033] Figure 6 This is a schematic diagram of a battery pack according to one embodiment of this application.
[0034] Figure 7 yes Figure 6 An exploded view of a battery pack according to one embodiment of this application is shown.
[0035] Figure 8 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.
[0036] Explanation of reference numerals in the attached figures: 1 battery pack 2 upper box 3 lower cabinets 4 battery modules 5 Secondary batteries 51 housing 52 Electrode Assembly 53 Top Cover Assembly 6 diaphragms 61 Substrate Layer 62 nanofiber layer 620 nanofibers 63 Lithium Supplement 64 polymer 651 Zero-dimensional conductive material 652 One-dimensional conductive material Detailed Implementation
[0037] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the separator for secondary batteries, its preparation method, secondary batteries, battery modules, battery packs, and power-consuming devices of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0038] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60~120 and 80~110 are listed for a specific parameter, it is also expected that ranges of 60~110 and 80~120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1~3, 1~4, 1~5, 2~3, 2~4, and 2~5. In this application, unless otherwise stated, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0~5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0039] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0040] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0041] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0042] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0043] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0044] In one embodiment of this application, a separator for a secondary battery is provided, comprising: Substrate layer; and A nanofiber layer disposed on one surface of the substrate layer. The nanofiber layer comprises a lithium supplement, a polymer, and an optional conductive material, wherein, relative to the total weight of the nanofiber layer, the lithium supplement contains 30.0 to 50.0% by weight, the polymer contains 50.0 to 70.0% by weight, and the conductive material contains 0 to 5.0% by weight.
[0045] Although the mechanism is not yet clear, the applicant unexpectedly discovered that: Figure 1 As shown, this application provides a separator (6) for secondary batteries by forming a nanofiber layer (62) comprising a lithium replenishing agent, a polymer, and optionally a conductive material on one surface of a substrate layer (61) as a lithium replenishing agent layer. When the separator is applied to a secondary battery, the lithium replenishing agent is slowly released from the nanofiber layer during liquid injection formation, thus playing a lithium replenishing role. Specifically, the released lithium replenishing agent can participate in the negative electrode film formation reaction, forming an SEI film on the negative electrode surface, reducing irreversible lithium consumption of the positive electrode, thereby significantly improving the initial discharge capacity of the battery. Furthermore, when the active lithium is insufficient during cycling, the active lithium stored in the negative electrode can participate in the electrochemical reaction in a timely manner, reducing the capacity decay of the battery.
[0046] More importantly, in the separator for secondary batteries of this application, the nanofiber layer has a composition of... Figure 2 The nanofibers (620) shown form a nanofiber structure, thus exhibiting a relatively high porosity. By providing the lithium replenishment layer in the form of this nanofiber layer, clogging of the substrate layer pores can be effectively avoided, lithium-ion transfer is not hindered, and the wettability and electrolyte retention of the separator are further improved, thereby ensuring continuous lithium-ion migration of the lithium replenishment agent within the nanofiber layer. In the nanofiber layer, the polymer and lithium replenishment agent work synergistically to improve the utilization efficiency of the lithium replenishment agent, thereby increasing the initial discharge capacity of the battery, improving the initial coulombic efficiency of the battery, reducing battery capacity decay, improving battery cycle performance, and extending battery life. Specifically, as... Figure 2As shown, the polymer (64) in the nanofiber layer can play a protective role, preventing the lithium replenishing agent (63) in the nanofiber layer from being deactivated by environmental influences; the polymer (64) can ensure the slow release of the lithium replenishing agent (63) through partial swelling. When the nanofiber layer includes conductive materials (e.g., such as...) Figure 2 When the zero-dimensional conductive material (651) and the one-dimensional conductive material (652) shown are fully mixed, the lithium replenishing agent and the conductive material can increase the electronic pathway of the lithium replenishing agent in the nanofiber layer, further improve the utilization efficiency of the lithium replenishing agent, thereby further improving the initial discharge capacity of the battery, greatly improving the first coulombic efficiency of the battery, further reducing the battery capacity decay, greatly improving the cycle performance of the battery, and extending the battery life.
[0047] Furthermore, the product of the lithium replenishing agent (63) reaction remains encapsulated within the polymer nanofibers (620), which can improve the strength of the nanofibers (620) and provide self-support. Moreover, in this application, the nanofiber layer serving as the lithium replenishing agent layer does not contain substances that affect the physical properties of the electrolyte, such as viscosity, thus avoiding the adverse effects of such substances dissolving on ion migration in the electrolyte and fully ensuring the battery's kinetic performance.
[0048] In the separator for secondary batteries of this application, the content of lithium replenishing agent is 30.0 to 50.0% by weight, the content of polymer is 50.0 to 70.0% by weight, and the content of conductive material is 0 to 5.0% by weight, relative to the total weight of the nanofiber layer. By maintaining the contents of lithium replenishing agent, polymer, and conductive material within the above ranges, the nanofiber layer can have good processing performance.
[0049] In some embodiments, the conductive material may include a zero-dimensional conductive material and optionally a one-dimensional conductive material. For example... Figure 2 As shown, the zero-dimensional conductive material (651) is dispersed inside the nanofibers (620) and thoroughly mixed with the lithium supplement (63), providing point-to-point electronic pathways. Therefore, the zero-dimensional conductive material (651) can promote electron migration within the nanofiber layer, increasing the electronic pathways of the lithium supplement, thereby improving the utilization efficiency of the lithium supplement. When the conductive material includes a one-dimensional conductive material, such as... Figure 2 As shown, the one-dimensional conductive material (652) can be partially exposed to the outside of the nanofibers (620), and the exposed portion of the one-dimensional conductive material (652) is not covered by the polymer (64). Therefore, when the separator is applied to a secondary battery with the nanofiber layer disposed on the positive electrode-facing surface of the substrate layer, the one-dimensional conductive material (652) can not only further promote electron migration within the nanofiber layer, but its partially exposed portion can also additionally promote electron migration between the nanofiber layer and the positive electrode active material, thereby further improving the utilization efficiency of the lithium replenishment agent.
[0050] Relative to the total weight of the nanofiber layer, the content of the zero-dimensional conductive material can be 1.0 to 5.0% by weight, and the content of the one-dimensional conductive material can be 0 to 0.3% by weight. By maintaining the contents of the zero-dimensional conductive material and the optional one-dimensional conductive material within the above ranges, it can be ensured that the conductive material fully exerts its above-mentioned function without adversely affecting the processing performance of the nanofiber layer.
[0051] In some embodiments, the zero-dimensional conductive material may have a particle size of 30-50 nm. When the zero-dimensional conductive material has a particle size within the above range, more point-to-point electronic pathways can be achieved with the same amount of addition, thereby further improving the utilization efficiency of the lithium supplement.
[0052] In this application, any zero-dimensional conductive material that can provide point-to-point electronic pathways as described above is acceptable; there are no specific limitations on the type of zero-dimensional conductive material, and those skilled in the art can select it according to actual needs. Optionally, the zero-dimensional conductive material may be one or more selected from carbon black, acetylene black, and Ketjen black.
[0053] In some embodiments, the one-dimensional conductive material may have an aspect ratio of 500 to 1000. When the one-dimensional conductive material has an aspect ratio within the above range, it can ensure that the one-dimensional conductive material fully exerts the additional effect of promoting electron migration between the nanofiber layer and the positive electrode active material, thereby further improving the utilization efficiency of the lithium supplement.
[0054] In this application, any one-dimensional conductive material that can perform the additional functions described above is acceptable; there are no specific limitations on the type of one-dimensional conductive material, and those skilled in the art can select it according to actual needs. Optionally, the one-dimensional conductive material can be carbon nanotubes, specifically single-arm nanotubes, multi-arm nanotubes, or a combination of both. Because carbon nanotubes have good conductivity and a small diameter, they can avoid occupying excessive volume.
[0055] In this application, any lithium replenishing agent that can perform the lithium replenishing function described above is acceptable; the type of lithium replenishing agent is not specifically limited, and those skilled in the art can select one according to actual needs. In some embodiments, the lithium replenishing agent is selected from Li₂C₂O₄, C₄BLiO₈, and Li₂. 15 Si4, Li4Sn, Li2NiO2, LiF, Li2TiO3, Li2CrO4, Li2Cr2O7, Li4SiO4, Li2SiO3, Li3AsO4, Li2SeO4, Li2SeO3, LiVO3, LiAlO2, Li3PO4, Li2B8O 13One or more of Li2B4O7, LiBO2, Li3AlF6, Li2SnF6 and LiAsF6, and optionally one or more of Li2NiO2, Li4Sn and LiAsF6.
[0056] In some embodiments, the particle size of the lithium replenishing agent is 50-200 nm, optionally 80-150 nm. When the lithium replenishing agent has a particle size within the above range, it can optimize the diameter of the nanofibers, so that the nanofiber layer has an optimized structure. This not only more effectively avoids clogging of the voids in the substrate layer, but also improves the wettability and electrolyte retention of the separator, and better promotes the migration of lithium ions in the lithium replenishing agent within the nanofiber layer.
[0057] In some embodiments, the amount of the lithium replenishing agent is 40 to 100 parts by weight relative to 100 parts by weight of the polymer, optionally 60 to 80 parts by weight. When the relative amount of the lithium replenishing agent to the polymer is within the above range, it can facilitate the synergistic effect between the polymer and the lithium replenishing agent, ensuring that the polymer can completely encapsulate the lithium replenishing agent, providing sufficient protection, while also ensuring the slow release of the lithium replenishing agent, thereby significantly improving the utilization efficiency of the lithium replenishing agent.
[0058] In some embodiments, the amount of the zero-dimensional conductive material is 1 to 12.5 parts by weight relative to 100 parts by weight of the lithium replenishing agent; and the amount of the one-dimensional conductive material is 0.15 to 0.75 parts by weight. When the relative amounts of the zero-dimensional conductive material and the one-dimensional conductive material relative to the lithium replenishing agent are within the above ranges, good electronic conductivity can be ensured while optimizing the amount of lithium replenishing agent, thereby significantly improving the utilization efficiency of the lithium replenishing agent.
[0059] In this application, any polymer that can be processed into a nanofiber material layer and is suitable for use in a separator for secondary batteries is acceptable; there are no specific limitations on the type of polymer, and those skilled in the art can select one according to actual needs. In some embodiments, the polymer is selected from one or more of polyvinylidene chloride, polyimide, polyacrylonitrile, and polystyrene.
[0060] In some embodiments, the diameter of the nanofibers in the nanofiber layer is 100-500 nm, optionally 200-250 nm. When the diameter of the nanofibers is within the above range, the formed nanofiber layer can have higher porosity, which can not only more effectively avoid clogging of the substrate layer voids, but also improve the wettability and liquid retention of the membrane to the electrolyte, and better promote the continuous lithium-ion migration of the lithium supplement within the nanofiber layer. In this application, the diameter of the nanofibers can be controlled by adjusting process parameters such as the extrusion speed of the dispersion used for electrospinning, the distance between the spinning head and the receiving end plate, and the voltage between the spinning head and the receiving end plate during the electrospinning process for preparing the nanofiber layer. Those skilled in the art can select according to actual needs.
[0061] In some embodiments, the thickness of the nanofiber layer is 1.0~5.0 μm, optionally 1.5~2.5 μm. When the thickness of the nanofiber layer is within the above range, it can ensure that the nanofiber layer contains a sufficient amount of lithium supplementing agent to achieve sufficient lithium supplementation, while not occupying too much space and adversely affecting the membrane performance. In this application, the thickness of the nanofiber layer can be controlled by adjusting the spinning time in the electrospinning process for preparing the nanofiber layer, and those skilled in the art can choose according to actual needs.
[0062] In some embodiments, the porosity of the nanofiber layer is above 80%. When the porosity of the nanofiber layer reaches above 80%, it can not only effectively avoid clogging of the voids in the substrate layer, but also improve the wettability and electrolyte retention of the membrane, ensuring continuous lithium-ion migration of the lithium replenishing agent within the nanofiber layer.
[0063] This application also provides a method for preparing a separator for secondary batteries, comprising: The polymer is dissolved in a solvent to obtain a polymer solution; The polymer solution is added to a lithium supplement or a blend of a lithium supplement and a conductive material, and then dispersed at high speed to obtain a dispersion. The dispersion is attached to one surface of the substrate layer by electrospinning to form a nanofiber layer. In the nanofiber layer, relative to the total weight of the nanofiber layer, the content of the lithium supplement is 30.0~50.0% by weight, the content of the polymer is 50.0~70.0% by weight, and the content of the conductive material is 0~5% by weight.
[0064] The preparation method of this application can effectively prepare the separator for secondary batteries according to the first aspect of this application.
[0065] In some embodiments, the solid content of the polymer solution can be 20-40% by weight, optionally 20-25% by weight. When the solid content of the polymer solution is within the above range, the dispersion obtained by adding the polymer solution to the lithium supplement agent or a blend of the lithium supplement agent and conductive material and dispersing it at high speed is suitable for the electrospinning process. This ensures that the diameter of the nanofibers produced by electrospinning is more uniform, the distribution of the lithium supplement agent and / or conductive material and the pore distribution of the nanofiber layer are more uniform, and the lithium supplementation effect of the lithium supplement agent and the performance of the separator are stabilized.
[0066] In some embodiments, the thickness of the nanofiber layer can be 1.0~5.0 μm, optionally 1.5~2.5 μm. In this application, the thickness of the nanofiber layer can be adjusted by adjusting the process parameters of the electrospinning step, and those skilled in the art can select according to actual needs.
[0067] This application also provides a secondary battery, comprising: positive electrode; negative electrode; Electrolytes; and The separator for secondary batteries of this application as described above, wherein The nanofiber layer is disposed on the surface of the substrate layer facing the positive electrode.
[0068] This application also provides a battery module that includes the secondary battery of this application as described above.
[0069] This application also provides a battery pack that includes the battery module of this application as described above.
[0070] This application also provides an electrical device, which includes at least one of the secondary battery, battery module, and battery pack described above.
[0071] In the secondary battery separator of this application, a nanofiber layer comprising a lithium replenishing agent, a polymer, and optionally a conductive material is disposed on one surface of the substrate layer as a lithium replenishing agent layer. When the separator of this application is applied to a secondary battery, during liquid injection formation, the lithium replenishing agent can be slowly released from the nanofiber layer and participate in the negative electrode film formation reaction, thus playing a lithium replenishing role. More importantly, the nanofiber layer has high porosity, which can effectively avoid clogging of the pores of the substrate layer, while improving the wettability and liquid retention of the separator to the electrolyte, thereby ensuring the continuous lithium-ion migration of the lithium replenishing agent in the nanofiber layer. Furthermore, the polymer in the nanofiber layer works synergistically with the lithium replenishing agent to improve the utilization efficiency of the lithium replenishing agent, thereby increasing the initial discharge capacity of the battery and reducing the battery capacity decay. The optional conductive material in the nanofiber layer can increase the electronic pathway of the lithium replenishing agent within the nanofiber layer, further improving the utilization efficiency of the lithium replenishing agent, thereby further increasing the initial discharge capacity of the battery and further reducing the battery capacity decay. Furthermore, the products of the lithium replenishment reaction remain encapsulated within the polymer nanofibers, enhancing their strength and providing self-support. Moreover, the nanofiber layer serving as the lithium replenishment layer does not contain substances that affect the viscosity or other physical properties of the electrolyte, thus avoiding the adverse effects of such substances dissolving and causing ion migration within the electrolyte, thereby fully ensuring the battery's kinetic performance.
[0072] The secondary battery, battery module, battery pack, and device of this application will be described below with appropriate reference to the accompanying drawings.
[0073] In one embodiment of this application, a secondary battery is provided.
[0074] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor of ions between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.
[0075] [Positive electrode plate] The positive electrode may include a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector. As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0076] The aforementioned positive electrode current collector can be a metal foil or a composite current collector. For example, aluminum foil can be used as the metal foil. The composite current collector can include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0077] The aforementioned positive electrode film layer includes a positive electrode active material, which includes, but is not limited to, lithium cobalt oxide, lithium nickel manganese cobalt oxide, lithium nickel manganese aluminum oxide, lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, lithium manganese silicate, spinel-type lithium manganese oxide, spinel-type lithium nickel manganese oxide, lithium titanate, etc. One or more of these materials can be used as the positive electrode active material.
[0078] The positive electrode film layer may optionally include a binder. However, there is no specific limitation on the type of binder, and those skilled in the art can select one according to actual needs. As an example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins.
[0079] The positive electrode film may optionally include a conductive agent. However, there is no specific limitation on the type of conductive agent, and those skilled in the art can select it according to actual needs. As an example, the conductive agent used for the positive electrode film may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0080] The positive electrode sheet can be prepared according to methods known in the art. As an example, the positive active material, conductive agent and binder can be dispersed in a solvent (e.g., N-methylpyrrolidone (NMP)) to form a uniform positive electrode slurry; the positive electrode slurry is coated on the positive current collector, and after drying, cold pressing and other processes, the positive electrode sheet is obtained.
[0081] [Negative electrode plate] The negative electrode sheet may include a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector, the negative electrode film layer comprising a negative electrode active material. As an example, the negative current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative current collector.
[0082] The aforementioned negative electrode current collector can be a metal foil or a composite current collector. For example, copper foil can be used as the metal foil. The composite current collector can include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0083] In the secondary battery of this application, the negative electrode film layer includes a negative electrode active material. The negative electrode active material can be any negative electrode active material commonly used in the art for preparing the negative electrode of a secondary battery. Examples of negative electrode active materials include artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. Silicon-based materials can be selected from one or more of elemental silicon, silicon oxide compounds (e.g., silicon suboxide), silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials can be selected from one or more of elemental tin, tin oxide compounds, and tin alloys.
[0084] In the secondary battery of this application, the negative electrode film layer may also include optional binders, optional conductive agents and other optional additives.
[0085] As an example, the conductive agent may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0086] As an example, the adhesive may be selected from one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0087] Other optional additives include thickeners (such as sodium carboxymethyl cellulose (CMC-Na)).
[0088] The negative electrode sheet can be prepared according to methods known in the art. As an example, the negative electrode active material, conductive agent, binder and any other components can be dispersed in a solvent (e.g., N-methylpyrrolidone (NMP) or deionized water) to form a uniform negative electrode slurry; the negative electrode slurry is coated onto the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet is obtained.
[0089] [Electrolytes] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.
[0090] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.
[0091] As an example, the electrolyte salt may be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).
[0092] As an example, the solvent may be selected from one or more of the following: fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butyl carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).
[0093] In some embodiments, the electrolyte may optionally include additives. For example, the electrolyte may include negative electrode film-forming additives, positive electrode film-forming additives, additives to improve battery overcharge performance, additives to improve battery high-temperature performance, additives to improve battery low-temperature performance, etc.
[0094] [Septum] The separator separates the positive and negative electrodes, preventing short circuits inside the battery, while allowing active ions to move between the positive and negative electrodes. In the secondary battery of this application, the separator used to perform the above-mentioned functions is the secondary battery separator of this application as described above, which has a nanofiber layer comprising a lithium replenishing agent, a polymer, and optionally a conductive material disposed on one surface of the substrate layer as a lithium replenishing layer.
[0095] This application does not impose any particular limitation on the type of substrate layer; any known substrate layer with good chemical and mechanical stability can be used. In some embodiments, any known porous membrane structure used in secondary batteries can be used as the substrate layer of the separator for secondary batteries in this application. For example, the substrate layer can be selected from glass fiber films, nonwoven films, polyethylene (PE) films, polypropylene (PP) films, polyvinylidene fluoride films, and one or more multilayer composite substrate layers comprising one or more of these. In some embodiments, polyolefin microporous membranes commonly used in the art can be used as the substrate layer of the separator for secondary batteries in this application.
[0096] The preparation method described in this application allows for the formation of a highly porosity nanofiber layer as a lithium replenishment layer on one surface of a substrate layer using an electrospinning process. In the electrospinning process for preparing the nanofiber layer, by adjusting process parameters such as the extrusion speed of the dispersion used for electrospinning, the distance between the spinning head and the receiving end plate, and the voltage between the spinning head and the receiving end plate, the diameter of the nanofibers can be controlled to be 100–500 nm, optionally 200–250 nm. By adjusting the spinning time, the thickness of the nanofiber layer can be controlled to be 1.0–5.0 μm, optionally 1.5–2.5 μm.
[0097] In some embodiments, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process. In this application, when assembling the electrode assembly, the nanofiber layer serving as the lithium replenishment layer faces the positive electrode surface, and the substrate layer faces the negative electrode surface.
[0098] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte as described above.
[0099] In some implementations, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0100] This application does not impose any particular limitation on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 3 This is an example of a square-structured secondary battery 5.
[0101] In some implementations, refer to Figure 4The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator may be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. The secondary battery 5 may contain one or more electrode assemblies 52, which can be selected by those skilled in the art according to specific practical needs.
[0102] In some implementations, the secondary batteries can be assembled into a battery module, and the number of secondary batteries contained in the battery module can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery module.
[0103] Figure 5 This is battery module 4, used as an example. (See reference...) Figure 5 In battery module 4, multiple secondary batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple secondary batteries 5 can be fixed in place using fasteners.
[0104] Optionally, the battery module 4 may also include a housing with a receiving space in which a plurality of secondary batteries 5 are received.
[0105] In some embodiments, the battery modules can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be selected by those skilled in the art based on the application and capacity of the battery pack.
[0106] Figure 6 and Figure 7 This is battery pack 1 as an example. (See reference...) Figure 6 and Figure 7 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0107] In addition, this application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in this application. The secondary battery, battery module, or battery pack can be used as the power source of the electrical device or as the energy storage unit of the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0108] As an electrical device, a secondary battery, battery module, or battery pack can be selected according to its usage requirements.
[0109] Figure 8 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.
[0110] Another example of an electrical device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use rechargeable batteries as their power source.
[0111] Example The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0112] Preparation of diaphragm A polyethylene microporous film with a thickness of approximately 7 μm is used as the substrate layer of the separator for secondary batteries in this application. A nanofiber layer comprising a lithium supplement, a polymer, and optionally a conductive material is formed on one surface of the substrate layer via an electrospinning process. The dispersion used for electrospinning is prepared as follows.
[0113] A polymer (e.g., one or more of polyvinylidene chloride, polyimide, polyacrylonitrile, and polystyrene) is dissolved in a solvent (e.g., one or more of N-methylpyrrolidone (NMP), dimethylacetamide (DMAC), and dimethylformamide (DMF)) and stirred to form a transparent and homogeneous polymer solution as component A. The solid content of component A is about 20-25% by weight. A lithium supplement is used as component B. Alternatively, the lithium supplement and conductive material are stirred and mixed under an inert gas atmosphere to form a homogeneous blend as component B. Component A is added to component B and stirred at a high speed of about 1000-1500 rpm / min for about 1-1.5 hours until a homogeneous dispersion for electrospinning is formed.
[0114] An electrospinning machine (ELITE, Beijing Yongkang Leyue Technology Development Co., Ltd.) was used. The applied voltage between the spinning head and the receiving end plate was set to 10-20 kV, and the distance between the spinning head and the receiving end plate was set to 10-30 cm. Under conditions of 20-35°C and 2-40% RH, the dispersion obtained in the above steps was sprayed onto one surface of the substrate layer through a spinning head with an inner diameter of 1-2 mm. The spray thickness was 1.0-5.0 μm, forming a nanofiber layer directly attached to one surface of the substrate layer. In the obtained nanofiber layer, the content of lithium supplementer was approximately 30.0-50.0% by weight, the content of polymer was approximately 50.0-70.0% by weight, and the content of conductive material was approximately 0-5% by weight, relative to the total weight of the nanofiber layer. After drying the obtained composite layer including the substrate layer and the nanofiber layer at a temperature of approximately 80-95°C, a separator with the nanofiber layer as the lithium supplement layer was obtained.
[0115] Cell manufacturing In the embodiments of this application, the battery cell is prepared using the following method.
[0116] (1) Preparation of positive electrode sheet The positive electrode active material Ni5Co2Mn3 (NCM523, Beijing Easpring Material Technology Co., Ltd.), conductive carbon (Super-P-Li, TIMCAL), and binder polyvinylidene fluoride (PVDF) (5130, Solvay, USA) were added to N-methylpyrrolidone (NMP) at a weight ratio of 97:1.5:1.5 and stirred thoroughly to obtain a positive electrode slurry with a solid content of 72%. Using conventional processes, the positive electrode slurry was coated using an extrusion coater or transfer coater at a coating density of 0.156 mg / mm². 2 The coating is evenly applied to the aluminum foil and dried at 100~130℃ to obtain the positive electrode sheet.
[0117] (2) Preparation of negative electrode sheet The negative electrode active material silicon suboxide (Xinjiang Jingshuo New Materials Co., Ltd.), conductive carbon (Super-P-Li, TIMCAL), and binder PVDF (5130, Solvay, USA) were added to NMP at a weight ratio of 95:2:3 and stirred thoroughly to obtain a uniformly mixed negative electrode slurry with a solid content of 52%. Using conventional processes, the negative electrode slurry was coated using an extrusion coater or transfer coater at a concentration of 0.106 mg / mm². 2 The coating is evenly applied to the copper foil and dried at 100~130℃ to obtain the negative electrode sheet.
[0118] (3) Battery preparation The positive and negative electrode sheets obtained in the above steps are manufactured to the corresponding dimensions required by the cell design. Then, the negative electrode sheet, separator, and positive electrode sheet are wound with the nanofiber layer of the separator facing the positive electrode surface to obtain a jelly roll, which is then assembled and filled with electrolyte. The electrolyte used is a solution of LiPF6 in a mixed solvent of dimethyl methacrylate (DMC), diethyl carbonate (DEC), and ethylene carbonate (EC) in a volume ratio of 1:1:1 (molar concentration 1 mol / L). After formation and capacity testing, a lithium-ion battery is obtained.
[0119] Performance testing (1) Porosity A membrane with a nanofiber layer is punched into a small disc with an area of S0. The disc is weighed and recorded as m2, and its thickness h1 is measured. Then, the disc is immersed in isobutanol (density ρ1) for 0.5 hours, removed, and weighed, recording the weight as m3. A substrate layer without a nanofiber layer is punched into a small disc with the same area of S1. The disc is weighed and recorded as m0, and its thickness h0 is measured. Then, the substrate disc is immersed in isobutanol (density ρ1) for 1 hour, removed, and weighed, recording the weight as m1. The porosity of the nanofiber layer is calculated using the following formula: Porosity = {[(m3-m2)-(m1-m0) ] / [ρ1 (h1-h0) ×S0]}×100% (2) First Coulomb efficiency The initial charge capacity of the batteries is designed to release 75 Ah. To measure the initial discharge capacity, the batteries were first fully charged to 4.2 V using a constant current of 0.33 C, and then charged to 0.05 C using a constant voltage. After resting for 1 hour, the batteries were discharged to 2.8 V using a constant current of 0.33 C. This discharge capacity is recorded as the initial discharge capacity C. The initial coulombic efficiency is calculated using the following formula: First Coulomb efficiency = (C / 75) × 100%.
[0120] (3) Capacity retention rate A fresh battery is charged and discharged at a rate of 0.33C at room temperature (25°C), and the discharge capacity at this time is recorded as the initial capacity C0. Then, the battery is cycled at a rate of 1C charging and discharging at room temperature (25°C) for 1800 cycles, and the discharge capacity after this is recorded as C1. The capacity retention rate is calculated using the following formula: Capacity retention rate = (C1 / C0) × 100%.
[0121] Example 1 Polyvinylidene chloride (PVDF) was added to NMP solvent at a mass ratio of 20:80 and stirred to form a transparent and homogeneous polymer solution, which was used as component A. Lithium supplementer Li₂NiO₂ with a particle size of 100 nm was used as component B. Under an inert atmosphere, component A was added to component B at a mass ratio of 15:2, and the mixture was stirred at a high speed of approximately 1000 rpm for about 1.2 hours until a homogeneous dispersion was formed for electrospinning.
[0122] Electrospinning was performed at a temperature of 25°C, a humidity of 15% RH, and an applied voltage of 15 kV. The dispersion was sprayed onto one surface of a polyethylene microporous film substrate layer with a thickness of approximately 7 μm through a spinning head with an inner diameter of 1 mm, yielding nanofibers with a diameter of 200 nm. By controlling the electrospinning time, a nanofiber layer with a thickness of approximately 1.5 μm was finally obtained as a lithium supplement layer. In this nanofiber layer, the lithium supplement content was approximately 30.0% by weight and the polymer content was approximately 70.0% by weight, relative to the total weight of the nanofiber layer. The resulting composite layer, including the substrate layer and the nanofiber layer, was dried at a temperature of approximately 110-130°C to obtain the separator of Example 1.
[0123] The porosity of the nanofiber layer of the diaphragm in Example 1 was measured using the test method described above.
[0124] A lithium-ion battery was prepared using the separator of Example 1 according to the method described above. Then, the initial coulombic efficiency and capacity retention of the battery prepared with the separator of Example 1 were measured using the test method described above.
[0125] Comparative Example 1 PVDF polymer was added to NMP solvent at a mass ratio of 20:80 to obtain a polymer solution. Lithium supplementer Li₂NiO₂ was added to the polymer solution at a mass ratio of 2:15 under an inert atmosphere. After stirring until homogeneous, the solution was filtered and dried to obtain polymer-coated composite particles. These composite particles were added to NMP solvent, mixed thoroughly, and then coated onto one surface of the same substrate layer as in Example 1, forming a coating of approximately 1.5 μm thickness as a lithium supplementer layer. No nanofiber structure was formed. In this coating, the lithium supplementer content was approximately 40.0% by weight and the polymer content was approximately 60.0% by weight relative to the total weight of the coating. The resulting composite layer, including the substrate layer and the coating, was dried at a temperature of approximately 80-95°C to obtain the separator of Comparative Example 1. In the separator of Comparative Example 1, the lithium supplementer layer was a conventional coating and did not possess a porous structure.
[0126] A lithium-ion battery was prepared using the separator of Comparative Example 1 through a method similar to that described above, wherein the coating of the separator was facing the positive electrode surface when the negative electrode, separator, and positive electrode were wound into a core. Then, the initial coulombic efficiency and capacity retention of the battery prepared using the separator of Comparative Example 1 were measured using the test method described above.
[0127] Examples 2-3 and Comparative Examples 2-3 The separator and secondary battery were prepared by essentially the same method as in Example 1, except that the content of lithium supplement and polymer relative to the total weight of the nanofiber layers in the prepared nanofibers are shown in Table 1.
[0128] Using the test methods described above, the porosity of the nanofiber layer of the separators in Examples 2-3 and Comparative Examples 2-3 was measured, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separators in Examples 2-3 and Comparative Examples 2-3.
[0129] The lithium supplement content and polymer content in the lithium supplement layer of Examples 1-3 and Comparative Examples 1-3, as well as the measured porosity, initial coulombic efficiency and capacity retention, are shown in Table 1.
[0130] Table 1 The results above show that, compared to Comparative Example 1, where the lithium replenishment layer is a non-porous coating comprising a lithium replenishing agent and a polymer, in Examples 1-3, the nanofiber layer comprising a lithium replenishing agent and a polymer formed on the substrate layer has a porosity of over 82%, preventing clogging of the voids in the substrate layer. Furthermore, the wettability and electrolyte retention of the separator are improved, ensuring continuous lithium-ion migration of the lithium replenishing agent. In particular, in Examples 1 and Comparative Example 1, the lithium replenishing agent layer comprises the same amount of lithium replenishing agent and the same amount of polymer; the only difference is that they have a nanofiber layer structure and a coating structure, respectively. In Examples 1-3, the polymer forming nanofibers effectively prevents lithium replenishing agent failure and allows for slow release of the lithium replenishing agent during the slow swelling process, thereby increasing the initial discharge capacity of the battery, raising the initial coulombic efficiency to over 90%, and improving the battery's cycle performance, with a capacity retention rate of over 83% after 1800 cycles.
[0131] Furthermore, in Comparative Examples 2 and 3, the initial discharge capacity and cycle performance of the batteries did not improve. This may be because in Comparative Examples 2 and 3, the lithium replenisher content and polymer content both exceeded the ranges of 30.0~50.0% by weight and 50.0~70.0% by weight, respectively. In Comparative Example 2, the lithium replenisher content was too low and the polymer content was too high, resulting in an excessively thick polymer coating on the lithium replenisher surface, which was detrimental to lithium ion extraction. Therefore, in Example 2, the initial discharge capacity and cycle performance of the battery deteriorated. In Comparative Example 3, the lithium replenisher content was too high and the polymer content was too low, making it difficult for the lithium replenisher surface to be completely coated by the polymer during electrospinning. This caused some of the lithium replenisher to deactivate due to exposure to air, failing to effectively provide lithium ions. Moreover, an excessively high lithium replenisher content also adversely affected the antistatic spinning process, resulting in insufficient porosity of the generated nanofiber layer. Therefore, in Example 2, the initial discharge capacity and cycle performance of the battery deteriorated.
[0132] Examples 4-8 The separator and secondary battery were prepared by essentially the same method as in Example 1, except that carbon black, a zero-dimensional conductive material with a particle size of about 40 nm, was added to component B, and the lithium supplement and conductive material were stirred and mixed in an inert atmosphere to form a uniformly mixed blend.
[0133] The amount of zero-dimensional conductive material added and the amounts of components A and B were adjusted so that the contents of lithium supplement, polymer and zero-dimensional conductive material relative to the total weight of the nanofiber layer in the prepared nanofiber are shown in Table 2.
[0134] Using the test methods described above, the porosity of the nanofiber layer of the separators in Examples 4-8, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separators in Examples 4-8, were measured respectively. The results are shown in Table 2.
[0135] Table 2 The results above show that, compared with Examples 1-3, in Examples 4-8, the addition of zero-dimensional conductive materials that provide point-to-point pathways to the nanofiber layer facilitates electron migration within the nanofiber layer, increasing the electronic pathways of the lithium replenisher and thus improving its utilization efficiency. In Examples 4-8, the initial discharge capacity of the battery is further improved, the initial coulombic efficiency is increased to over 91%, and the cycle performance is enhanced, with a capacity retention of over 85% after 1800 cycles.
[0136] Furthermore, compared to Examples 7 and 8, in Examples 4-6, the initial discharge capacity of the battery is further improved, the initial coulombic efficiency of the battery is increased to over 92%, and the cycle performance of the battery is improved, with a capacity retention rate of over 87% after 1800 cycles.
[0137] Examples 9-21 The separator and secondary battery were prepared by essentially the same method as in Example 4, except that a one-dimensional conductive material, a single-arm carbon nanotube with an aspect ratio of about 800, was also added to component B. The contents of lithium supplement, polymer, zero-dimensional conductive material and one-dimensional conductive material in the prepared nanofibers relative to the total weight of the nanofiber layers are shown in Table 3.
[0138] Using the test methods described above, the porosity of the nanofiber layer of the separators in Examples 9-21, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separators in Examples 9-21, were measured respectively. The results are shown in Table 3.
[0139] Table 3 The results above show that, compared to Examples 4-8, in Examples 9-21, the addition of a one-dimensional conductive material partially exposed to the outside of the nanofibers not only further promotes electron migration within the nanofiber layer, but also, due to the partially exposed portion, further promotes electron migration between the nanofiber layer and the positive electrode active material, thereby further improving the utilization efficiency of the lithium replenishment agent. As a result, in Examples 9-21, the initial discharge capacity of the battery is increased, the initial coulombic efficiency remains above 90%, and the cycle performance is significantly improved, with a capacity retention rate of over 89% after 1800 cycles.
[0140] In Examples 13 and 14, the lithium replenishing agent content was 77 parts by weight and 62.5 parts by weight, respectively, relative to 100 parts by weight of polymer, within the preferred range of 60-80 parts by weight. As a result, compared to Example 12, in which the lithium replenishing agent content was 50 parts by weight, the battery capacity retention after 1800 cycles was improved.
[0141] Examples 22-25 The separator and secondary battery were prepared using essentially the same method as in Example 4, except that the particle size of the zero-dimensional conductive material carbon black added to component B is shown in Table 4.
[0142] Using the test methods described above, the porosity of the nanofiber layer of the separators in Examples 22-25, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separators in Examples 22-25, were measured respectively. The results are shown in Table 4. For ease of comparison, the porosity of the nanofiber layer of the separator in Example 4, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separator in Example 4, are also listed in Table 4.
[0143] Table 4 The results above show that, compared with Examples 22 and 25, the particle size of the zero-dimensional conductive material in Examples 4, 23, and 24 is preferably within the range of 30-50 nm. Therefore, with the same amount added, more point-to-point electronic pathways can be achieved without adversely affecting the electrospinning process, thus ensuring a further improvement in the utilization efficiency of the lithium replenishment agent. As a result, in Examples 4, 23, and 24, the initial discharge capacity of the battery is improved, the initial coulombic efficiency of the battery reaches as high as 92%, and the cycle performance of the battery is improved, with a capacity retention rate of over 86% after 1800 cycles.
[0144] Examples 26-30 The separator and secondary battery were prepared using essentially the same method as in Example 4, except that a one-dimensional conductive material, single-arm carbon nanotubes with an aspect ratio as shown in Table 5, was added to component B. Furthermore, in the prepared nanofibers, the contents of lithium supplement, polymer, zero-dimensional conductive material, and one-dimensional conductive material, relative to the total weight of the nanofiber layers, were 39.8%, 59%, 1%, and 0.2%, respectively.
[0145] Using the test methods described above, the porosity of the nanofiber layer of the separators in Examples 26-30, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separators in Examples 26-30, were measured respectively. The results are shown in Table 5.
[0146] Table 5 The results above show that, compared with Examples 26 and 30, in Examples 27-29, the aspect ratio of the one-dimensional conductive material is within the preferred range of 500-1000 nm. Therefore, the one-dimensional conductive material can fully exert its additional effect of promoting electron migration between the nanofiber layer and the positive electrode active material, thereby ensuring a further improvement in the utilization efficiency of the lithium replenishment agent. As a result, in Examples 27-29, the initial discharge capacity of the battery is improved, the initial coulombic efficiency of the battery remains above 92%, and the cycle performance of the battery is improved, with a capacity retention rate of over 91% after 1800 cycles.
[0147] Examples 31-34 The separator and secondary battery were prepared using essentially the same method as in Example 4, except that the particle size of the lithium supplement was as shown in Table 6.
[0148] Using the test methods described above, the porosity of the nanofiber layer of the separators in Examples 31-34, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separators in Examples 31-34, were measured respectively. The results are shown in Table 6. For ease of comparison, the porosity of the nanofiber layer of the separator in Example 4, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separator in Example 4, are also listed in Table 6.
[0149] Table 6 The results above show that in Examples 4 and 31-34, the particle size of the lithium replenishing agent was within the preferred range of 50-200 nm, which optimized the diameter of the nanofibers, resulting in a better structure for the nanofiber layer. This effectively prevented blockage of the substrate layer's voids, improved the separator's wettability and electrolyte retention, and better promoted the continuous lithium-ion migration of the lithium replenishing agent within the nanofiber layer. Consequently, in Examples 4 and 31-34, the initial discharge capacity of the battery was improved, the initial coulombic efficiency of the battery reached over 89%, and the cycle performance of the battery was improved, with a capacity retention rate of over 82% after 1800 cycles.
[0150] In Examples 4, 32, and 33, the particle size of the lithium replenishing agent is in a further preferred range of 80 to 150 nm, the initial discharge capacity of the battery is further improved, the initial coulombic efficiency of the battery is as high as 90%, and the cycle performance of the battery is further improved, with a capacity retention rate of up to 85% after 1800 cycles.
[0151] Examples 35-39 The separator and secondary battery were prepared using essentially the same method as in Example 9, except that the inner diameter of the spinneret was adjusted during the electrospinning process so that the diameter of the nanofibers was as shown in Table 7. Furthermore, in the prepared nanofibers, the contents of lithium supplement, polymer, zero-dimensional conductive material, and one-dimensional conductive material, relative to the total weight of the nanofiber layers, were 39.8%, 59.0%, 1.0%, and 0.2%, respectively.
[0152] Using the test methods described above, the porosity of the nanofiber layer of the separators in Examples 35-39, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separators in Examples 35-39, were measured respectively. The results are shown in Table 7.
[0153] Table 7 The results above show that in Examples 35-39, the diameter of the nanofiber layer is preferably within the range of 100-500 nm, resulting in a superior structure that more effectively prevents blockage of the substrate layer's voids, improves the separator's wettability and electrolyte retention, and better promotes the continuous lithium-ion migration of the lithium replenishing agent within the nanofiber layer. Consequently, in Examples 35-39, the initial discharge capacity of the battery is significantly improved, the initial coulombic efficiency is over 91%, and the cycle performance is enhanced, with capacity retention remaining above 89% after 1800 cycles.
[0154] In Examples 36 and 37, the diameter of the nanofibers is in a further preferred range of 200-250 nm, the initial discharge capacity of the battery is further improved, the initial coulombic efficiency of the battery is as high as 94% or more, and the cycle performance of the battery is further improved, with the capacity retention rate remaining above 92% after 1800 cycles.
[0155] Examples 40-43 The separator and secondary battery were prepared by essentially the same method as in Example 14, except that the electrospinning time was adjusted in the electrospinning process so that the thickness of the formed nanofiber layer was as shown in Table 8.
[0156] Using the test methods described above, the porosity of the nanofiber layer of the separators in Examples 40-43, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separators in Examples 40-43, were measured respectively. The results are shown in Table 8. For ease of comparison, the porosity of the nanofiber layer of the separator in Example 14, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separator in Example 14, are also listed in Table 8.
[0157] Table 8 The results above show that in Examples 14 and 40-43, the thickness of the nanofiber layer is preferably within the range of 1.0-5.0 μm. This is beneficial because the nanofiber layer contains a sufficient amount of lithium replenishing agent, achieving adequate lithium replenishment without occupying excessive space and adversely affecting the separator performance. As a result, in Examples 14 and 40-43, the initial discharge capacity of the battery is significantly improved, the initial coulombic efficiency of the battery is over 94%, and the cycle performance of the battery is significantly improved, with the capacity retention rate remaining above 89% after 1800 cycles.
[0158] In Examples 14 and 41, the thickness of the nanofiber layer is in a further preferred range of 1.5 to 2.5 μm, the initial discharge capacity of the battery is further improved, the initial coulombic efficiency of the battery is as high as 96% or more, and the cycle performance of the battery is further improved, with a capacity retention rate of as high as 92% or more after 1800 cycles.
[0159] Examples 44-46 The separator and secondary battery were prepared by essentially the same method as in Example 9, except that in the preparation of component A, the polymer solution formed had the solid content shown in Table 9.
[0160] Using the test methods described above, the porosity of the nanofiber layer of the separators in Examples 44-46, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separators in Examples 44-46, were measured respectively. The results are shown in Table 9. For ease of comparison, the porosity of the nanofiber layer of the separator in Example 9, as well as the initial coulombic efficiency and capacity retention of the batteries prepared using the separator in Example 9, are also listed in Table 9.
[0161] Table 9 The results above show that in Examples 9 and 44-46, the solid content of the polymer solution in the preparation of the dispersion for electrospinning is preferably within the range of 20-40%. Therefore, after adding it to the lithium replenishing agent or a blend of the lithium replenishing agent and conductive material and dispersing it at high speed, the resulting dispersion is very suitable for the electrospinning process. This ensures that the diameter of the nanofibers produced by electrospinning is more uniform, the distribution of the lithium replenishing agent and / or conductive material, and the pore distribution of the nanofiber layer are more uniform, thus stabilizing the lithium replenishing effect of the lithium replenishing agent and the performance of the separator. As a result, in Examples 9 and 44-46, the battery exhibits excellent initial discharge capacity, a first coulombic efficiency of over 91%, and further improved cycle performance, with a capacity retention rate of over 90% after 1800 cycles.
[0162] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
[0163] Industrial application The separator of this application has a nanofiber layer comprising a lithium replenishing agent, a polymer, and optionally a conductive material as the lithium replenishing agent layer, which greatly improves the utilization efficiency of the lithium replenishing agent. When applied to secondary batteries, it significantly increases the initial discharge capacity of the battery, enhances the battery's cycle performance, and extends battery life. Therefore, this application is suitable for industrial applications.
Claims
1. A separator for a secondary battery, comprising: Substrate layer; and A nanofiber layer disposed on one surface of the substrate layer. The nanofiber layer comprises a lithium supplement, a polymer, and optionally a conductive material, wherein, relative to the total weight of the nanofiber layer, the lithium supplement comprises 30.0-50.0% by weight, the polymer comprises 50.0-70.0% by weight, and the conductive material comprises 0-5.0% by weight. The lithium supplement includes Li₂C₂O₄, C₄BLiO₈, and Li. 15 Si4, Li4Sn, Li2NiO2, LiF, Li2TiO3, Li2CrO4, Li2Cr2O7, Li4SiO4, Li2SiO3, Li3AsO4, Li2SeO4, Li2SeO3, LiVO3, LiAlO2, Li3PO4, Li2B8O 13 One or more of Li2B4O7, LiBO2, Li3AlF6, Li2SnF6, and LiAsF6; The polymer includes one or more of polyvinylidene chloride, polyimide, polyacrylonitrile, and polystyrene.
2. The diaphragm according to claim 1, wherein, The conductive material includes zero-dimensional conductive material and optional one-dimensional conductive material, and the content of the zero-dimensional conductive material is 1.0 to 5.0% by weight and the content of the one-dimensional conductive material is 0 to 0.3% by weight relative to the total weight of the nanofiber layer.
3. The diaphragm according to claim 2, wherein, The zero-dimensional conductive material has a particle size of 30~50 nm.
4. The diaphragm according to claim 3, wherein, The zero-dimensional conductive material is selected from one or more of carbon black, acetylene black, and Ketjen black.
5. The diaphragm according to any one of claims 2-4, wherein, The one-dimensional conductive material has an aspect ratio of 500 to 1000.
6. The diaphragm according to claim 5, wherein, The one-dimensional conductive material is a carbon nanotube.
7. The diaphragm according to claim 6, wherein, The one-dimensional conductive material is a single-arm nanotube, a multi-arm nanotube, or a combination of both.
8. The diaphragm according to any one of claims 1 to 7, wherein, The lithium supplement has a particle size of 50~200 nm.
9. The diaphragm according to claim 8, wherein, The lithium supplement has a particle size of 80~150 nm.
10. The diaphragm according to any one of claims 1 to 9, wherein, The amount of the lithium supplement is 40 to 100 parts by weight relative to 100 parts by weight of the polymer.
11. The separator according to claim 10, wherein the amount of the lithium supplement is 60 to 80 parts by weight relative to 100 parts by weight of the polymer.
12. The diaphragm according to any one of claims 2 to 7, wherein, The amount of the zero-dimensional conductive material is 1 to 12.5 parts by weight relative to 100 parts by weight of the lithium replenishing agent; and the amount of the one-dimensional conductive material is 0.15 to 0.75 parts by weight.
13. The diaphragm according to any one of claims 1 to 12, wherein, The nanofibers in the nanofiber layer have a diameter of 100~500 nm.
14. The diaphragm according to claim 13, wherein, The nanofibers in the nanofiber layer have a diameter of 200~250 nm.
15. The diaphragm according to any one of claims 1 to 14, wherein, The thickness of the nanofiber layer is 1.0~5.0 μm.
16. The diaphragm according to claim 15, wherein, The thickness of the nanofiber layer is 1.5~2.5 μm.
17. The diaphragm according to any one of claims 1 to 16, wherein, The porosity of the nanofiber layer is above 80%.
18. The diaphragm according to claim 1, wherein, The lithium supplement includes one or more of Li2NiO2, Li4Sn and LiAsF6.
19. A method for preparing a separator for a secondary battery, comprising: The polymer is dissolved in a solvent to obtain a polymer solution; The polymer solution is added to a lithium supplement or a blend of a lithium supplement and a conductive material, and then dispersed at high speed to obtain a dispersion. The dispersion is attached to one surface of the substrate layer by electrospinning to form a nanofiber layer. In the nanofiber layer, relative to the total weight of the nanofiber layer, the content of the lithium supplement is 30.0~50.0% by weight, the content of the polymer is 50.0~70.0% by weight, and the content of the conductive material is 0~5% by weight. The lithium supplement includes Li₂C₂O₄, C₄BLiO₈, and Li. 15 Si4, Li4Sn, Li2NiO2, LiF, Li2TiO3, Li2CrO4, Li2Cr2O7, Li4SiO4, Li2SiO3, Li3AsO4, Li2SeO4, Li2SeO3, LiVO3, LiAlO2, Li3PO4, Li2B8O 13 One or more of Li2B4O7, LiBO2, Li3AlF6, Li2SnF6, and LiAsF6; The polymer includes one or more of polyvinylidene chloride, polyimide, polyacrylonitrile, and polystyrene.
20. The method according to claim 19, wherein, The polymer solution has a solid content of 20-40% by weight.
21. The method according to claim 20, wherein, The solid content of the polymer solution is 20-25% by weight.
22. The method according to any one of claims 19-21, wherein, The thickness of the nanofiber layer is 1.0~5.0 μm.
23. The method of claim 22, wherein, The thickness of the nanofiber layer is 1.5~2.5 μm.
24. The method according to claim 19, wherein, The lithium supplement includes one or more of Li2NiO2, Li4Sn and LiAsF6.
25. A secondary battery, comprising: positive electrode; negative electrode; Electrolytes; and The diaphragm according to any one of claims 1 to 18, wherein The nanofiber layer is disposed on the surface of the substrate layer facing the positive electrode.
26. A battery module comprising the secondary battery of claim 25.
27. A battery pack comprising the battery module of claim 26.
28. An electrical device comprising at least one of the secondary battery of claim 25, the battery module of claim 26, and the battery pack of claim 27.
Citation Information
Patent Citations
Heat resisting separator having ultrafine fibrous layer and secondary battery having the same
US20100304205A1
Electrospinning of PVDF-HFP: novel composite polymer electrolytes (CPES) with enhanced ionic conductivities for lithium-sulfur batteries
US20200136113A1