A method, system, device, and medium for determining suitability of a hydrogen storage container material

By obtaining cyclic information to calculate the stress intensity factor, determine the crack propagation conditions, adjust material parameters, and utilize the critical value curve of material constants, the problem of inconsistent calculation of crack propagation life of hydrogen storage containers was solved, and a clear judgment and unified evaluation standard for material suitability was achieved.

CN117473738BActive Publication Date: 2026-11-20CHINA SPECIAL EQUIP INSPECTION & RES INST
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311417243.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-30
Publication Date
2026-11-20
Estimated Expiration
2043-10-30

AI Technical Summary

Technical Problem

The existing methods for calculating the crack propagation life of hydrogen storage containers are not uniform, which leads to ambiguity in the evaluation process and makes it impossible to clearly determine whether the material's properties meet the requirements under a certain hydrogen pressure.

Method used

A method for determining the suitability of hydrogen storage container materials is provided. This method involves obtaining cycle information, calculating the stress intensity factor, determining crack propagation conditions, adjusting material parameters, determining crack propagation life, and using a material constant critical value curve to determine the material suitability.

Benefits of technology

This enables a clear determination of whether hydrogen storage container materials meet usage requirements and are suitable, provides a unified evaluation standard, and improves the accuracy and consistency of the evaluation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117473738B_ABST
    Figure CN117473738B_ABST
Patent Text Reader

Abstract

The application discloses a hydrogen storage container material applicability determination method, system, device and medium, and relates to the field of material detection; the method comprises the following steps: obtaining the applicability information of the ith cycle and determining the stress intensity factor; determining whether the stress intensity factor of the ith cycle meets the crack propagation condition; if yes, determining the stress intensity factor ratio of the ith cycle, and then determining the crack propagation information of the ith cycle; determining whether the crack propagation depth of the ith cycle meets the critical preset condition; if yes, determining the crack propagation cycle number and the critical crack size, and then determining the cycle number of reaching the allowable crack size; then determining whether the crack propagation life design value requirement of the hydrogen storage container is met; further, the critical value curve graph of the material constant of the hydrogen storage container under different crack propagation life design values is obtained, and then it is directly determined whether the hydrogen storage container material is applicable through the curve graph; and the application can determine whether the hydrogen storage container material is applicable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials testing, and in particular to a method, system, equipment, and medium for determining the suitability of hydrogen storage container materials. Background Technology

[0002] The current standards for fatigue assessment of hydrogen storage containers are not uniform, the calculation methods are inconsistent, and the crack propagation life calculated by different methods also varies greatly.

[0003] There are three main differences in the calculation of crack propagation life of hydrogen storage containers: the method for calculating the stress intensity factor, the fatigue crack propagation rate model, and the fatigue assessment process.

[0004] Because existing calculation methods are inconsistent, and the crack propagation lifetimes calculated by different standards vary considerably, the evaluation process for hydrogen storage containers is rather vague, and there is no clear judgment process for whether the material properties meet the requirements under a certain hydrogen pressure. Summary of the Invention

[0005] The purpose of this invention is to provide a method, system, device, and medium for determining the suitability of hydrogen storage container materials, which can determine whether the characteristics of hydrogen storage container materials meet the usage requirements and thus have suitability.

[0006] To achieve the above objectives, the present invention provides the following solution:

[0007] A method for determining the suitability of hydrogen storage container materials, the method comprising:

[0008] Obtain applicable information for the i-th cycle; the applicable information includes: material information and load conditions; the material information includes: material parameters, crack depth size, crack depth-to-length ratio, and material yield strength; i≥1;

[0009] The stress intensity factor for the i-th cycle is determined based on the applicable information for the i-th cycle.

[0010] Determine whether the stress intensity factor of the i-th cycle satisfies the crack propagation condition, and obtain the first determination result;

[0011] If the first judgment result is yes, then the stress intensity factor ratio of the i-th cycle is determined based on the stress intensity factor of the i-th cycle.

[0012] The crack propagation information for the i-th cycle is determined based on the stress intensity factor ratio of the (i-1)-th cycle; the crack propagation information includes: crack propagation depth and crack propagation length; when i = 1, the initial crack propagation information is determined based on the initial stress intensity factor ratio.

[0013] Determine whether the crack propagation depth of the i-th cycle meets the critical preset condition to obtain the second judgment result; the critical preset condition is: the crack propagation depth of the i-th cycle is greater than the thickness of the wall by a set multiple or lower than the set value of the fatigue evaluation curve.

[0014] If the second judgment result is negative, adjust the material parameters and return to the "Determine the stress intensity factor of the i-th cycle based on the applicable information of the i-th cycle" step;

[0015] If the second judgment result is yes, then the number of cycles in the i-th cycle is determined as the number of crack propagation cycles, and the crack propagation depth in the i-th cycle is determined as the critical crack size;

[0016] The allowable crack size is determined based on the critical crack size, and the number of cycles required to reach the allowable crack size is determined based on the number of crack propagation cycles.

[0017] The crack propagation life is determined based on the number of crack propagation cycles and the number of cycles required to reach the allowable crack size;

[0018] Determine whether the crack propagation lifetime is not less than the design value of the crack propagation lifetime of the hydrogen storage container. If yes, determine that the material parameters of the hydrogen storage container are applicable; otherwise, adjust the material parameters and return to the "Get applicable information for the i-th cycle" step.

[0019] Determine the critical material constant curves of the hydrogen storage container under different design values ​​for crack propagation life, and determine the suitability of the hydrogen storage container material based on the critical material constant curves and the material information to be used.

[0020] Optionally, the stress intensity factor for the i-th cycle is determined based on applicable information for the i-th cycle, specifically including:

[0021] Based on the free surface correction coefficient table, the correction coefficient for the i-th cycle is determined by interpolation according to the material information of the i-th cycle.

[0022] Based on the load condition of the i-th cycle, a cubic polynomial is used to fit the circumferential stress of the crack to obtain the fitting coefficients for the i-th cycle.

[0023] The stress intensity factor for the i-th cycle is determined based on the correction coefficient for the i-th cycle, the fitting coefficient for the i-th cycle, and the crack depth size for the i-th cycle.

[0024] Optionally, the method for determining the fatigue assessment curve specifically includes:

[0025] The reference stress for the i-th cycle is determined based on the applicable information for the i-th cycle.

[0026] The load ratio for the i-th cycle is calculated based on the material yield strength and the reference stress for the i-th cycle.

[0027] The toughness ratio for the i-th cycle is determined based on the stress intensity factor of the i-th cycle.

[0028] The curve construction formula is determined based on the load ratio and toughness ratio of the i-th cycle.

[0029] The fatigue assessment curve is determined based on the curve construction formula.

[0030] Optionally, the expression for the curve construction formula is:

[0031]

[0032] Among them, K r The toughness ratio; This represents the load ratio.

[0033] Optionally, the formula for calculating the load ratio specifically includes:

[0034]

[0035] in, σ is the load ratio; ref R is the reference stress. el This represents the yield strength of the material.

[0036] A system for determining the suitability of hydrogen storage container materials, the system comprising:

[0037] The acquisition module is used to acquire applicable information for the i-th cycle; the applicable information includes: material information and load conditions; the material information includes: material parameters, crack depth size, crack depth-to-length ratio, and material yield strength; i≥1;

[0038] The stress intensity factor determination module is used to determine the stress intensity factor for the i-th cycle based on the applicable information for the i-th cycle.

[0039] The first judgment module is used to determine whether the stress intensity factor of the i-th cycle satisfies the crack propagation condition and obtain the first judgment result;

[0040] The first determining module is used to determine the stress intensity factor ratio of the i-th cycle based on the stress intensity factor of the i-th cycle if the first determination result is yes.

[0041] A crack propagation information determination module is used to determine the crack propagation information of the i-th cycle based on the stress intensity factor ratio of the (i-1)-th cycle; the crack propagation information includes: crack propagation depth and crack propagation length; when i=1, the initial crack propagation information is determined based on the initial stress intensity factor ratio;

[0042] The second judgment module is used to determine whether the crack propagation depth of the i-th cycle meets the critical preset condition and obtain the second judgment result; the critical preset condition is: the crack propagation depth of the i-th cycle is greater than the thickness of the wall by a set multiple or lower than the set value of the fatigue evaluation curve.

[0043] The second determining module is used to adjust the material parameters and return to the "stress intensity factor determining module" if the second determination result is negative.

[0044] The third determining module is used to determine the number of cycles in the i-th iteration as the number of crack propagation cycles and the crack propagation depth in the i-th iteration as the critical crack size if the second determination result is yes.

[0045] The fourth determining module is used to determine the allowable crack size based on the critical crack size, and to determine the number of cycles required to reach the allowable crack size based on the number of crack propagation cycles.

[0046] A crack propagation life determination module is used to determine the crack propagation life based on the number of crack propagation cycles and the number of cycles to reach the allowable crack size;

[0047] The third judgment module is used to determine whether the crack propagation life is not less than the design value of the crack propagation life of the hydrogen storage container. If so, it is determined that the material parameters of the hydrogen storage container are applicable; if not, the material parameters are adjusted and the module is returned to the "acquisition module".

[0048] The fifth determining module is used to determine the critical value curve of the material constant of the hydrogen storage container under different design values ​​of crack propagation life, and to determine whether the material of the hydrogen storage container is suitable based on the critical value curve of the material constant and the material information to be used.

[0049] An electronic device includes a memory and a processor, the memory storing a computer program, and the processor running the computer program to cause the electronic device to perform the above-described method for determining the suitability of hydrogen storage container materials.

[0050] A computer-readable storage medium storing a computer program that, when executed by a processor, implements the above-described method for determining the suitability of hydrogen storage container materials.

[0051] According to specific embodiments provided by the present invention, the present invention discloses the following technical effects:

[0052] This invention provides a method, system, device, and medium for determining the suitability of hydrogen storage container materials. The method involves obtaining suitability information from the i-th cycle to determine the stress intensity factor; determining whether the stress intensity factor of the i-th cycle meets the crack propagation condition; if so, determining the stress intensity factor ratio of the i-th cycle to determine the crack propagation information; determining whether the crack propagation depth of the i-th cycle meets the critical preset condition; if so, determining the number of crack propagation cycles and the critical crack size, and then determining the number of cycles required to reach the allowable crack size; and determining the suitability of the hydrogen storage container material based on the material constant critical value curve and crack propagation lifetime. Therefore, it is possible to determine whether the characteristics of the hydrogen storage container material meet the usage requirements and thus determine its suitability. Attached Figure Description

[0053] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0054] Figure 1 A flowchart illustrating the method for determining the suitability of hydrogen storage container materials provided in this embodiment of the invention;

[0055] Figure 2 A flowchart of the stress intensity factor calculation method provided in the embodiments of the present invention;

[0056] Figure 3 A flowchart of a crack propagation life calculation method provided in an embodiment of the present invention;

[0057] Figure 4 A flowchart for fatigue assessment provided in an embodiment of the present invention;

[0058] Figure 5 A flowchart for calculating material constants provided in an embodiment of the present invention;

[0059] Figure 6 This is a schematic diagram of an axial semi-elliptical crack on the inner wall of a hydrogen storage container provided in an embodiment of the present invention.

[0060] Figure 7 A schematic diagram showing the dimensions of a hydrogen storage container.

[0061] Figure 8 A fatigue assessment curve provided for an embodiment of the present invention;

[0062] Figure 9 This is a graph showing the critical values ​​of material constants for different service lives. Detailed Implementation

[0063] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0064] The purpose of this invention is to provide a method, system, device, and medium for determining the suitability of hydrogen storage container materials, which can determine whether the characteristics of hydrogen storage container materials meet the usage requirements and thus have suitability.

[0065] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.

[0066] Example 1

[0067] like Figure 1 As shown in the figure, an embodiment of the present invention provides a method for determining the suitability of hydrogen storage container materials, the method comprising:

[0068] Step 100: Obtain the applicable information for the i-th iteration. The applicable information includes: material information and load conditions; material information includes: material parameters, crack depth size, crack length-to-depth ratio, and material yield strength; i ≥ 1.

[0069] Step 200: Determine the stress intensity factor for the i-th cycle based on the applicable information for the i-th cycle.

[0070] Specifically, the stress intensity factor for the i-th cycle is determined based on the applicable information for the i-th cycle, including:

[0071] Based on the free surface correction coefficient table, the correction coefficient for the i-th cycle is determined by interpolation according to the material information of the i-th cycle.

[0072] Based on the load condition of the i-th cycle, a cubic polynomial is used to fit the circumferential stress of the crack to obtain the fitting coefficients for the i-th cycle.

[0073] The stress intensity factor for the i-th cycle is determined based on the correction coefficient for the i-th cycle, the fitting coefficient for the i-th cycle, and the crack depth size for the i-th cycle.

[0074] Step 300: Determine whether the stress intensity factor of the i-th cycle satisfies the crack propagation condition, and obtain the first judgment result.

[0075] Step 400: If the first judgment result is yes, then determine the stress intensity factor ratio of the i-th cycle based on the stress intensity factor of the i-th cycle.

[0076] Step 500: Determine the crack propagation information for the i-th cycle based on the stress intensity factor ratio of the (i-1)-th cycle. The crack propagation information includes the crack propagation depth and crack propagation length; when i = 1, determine the initial crack propagation information based on the initial stress intensity factor ratio.

[0077] Step 600: Determine whether the crack propagation depth in the i-th cycle meets the critical preset condition, and obtain the second judgment result. The critical preset condition is: the crack propagation depth in the i-th cycle is greater than a set multiple of the wall thickness or lower than the set value of the fatigue evaluation curve.

[0078] The method for determining the fatigue assessment curve specifically includes:

[0079] The reference stress for the i-th cycle is determined based on the applicable information for the i-th cycle.

[0080] The load ratio for the i-th cycle is calculated based on the material yield strength of the i-th cycle and the reference stress of the i-th cycle.

[0081] The formula for calculating the load ratio specifically includes:

[0082]

[0083] in, σ is the load ratio; ref R is the reference stress. el This represents the yield strength of the material.

[0084] The toughness ratio for the i-th cycle is determined based on the stress intensity factor of the i-th cycle.

[0085] The curve construction formula is determined based on the load ratio and toughness ratio of the i-th cycle.

[0086] The fatigue assessment curve is determined based on the curve construction formula.

[0087] Specifically, the expression for the curve construction formula is:

[0088]

[0089] Among them, K r The toughness ratio; This represents the load ratio.

[0090] Step 700: If the second judgment result is negative, adjust the material parameters and return to step 200.

[0091] Step 800: If the second judgment result is yes, then the number of cycles in the i-th cycle is determined as the number of crack propagation cycles, and the crack propagation depth in the i-th cycle is determined as the critical crack size.

[0092] Step 900: Determine the allowable crack size based on the critical crack size, and determine the number of cycles required to reach the allowable crack size based on the number of crack propagation cycles.

[0093] Step 1000: Determine the crack propagation life based on the number of crack propagation cycles and the number of cycles required to reach the allowable crack size.

[0094] Step 1100: Determine whether the crack propagation life is not less than the design value of the crack propagation life of the hydrogen storage container. If yes, determine that the material parameters of the hydrogen storage container are suitable; if not, adjust the material parameters and return to step 100. Then recalculate.

[0095] Step 1200: Determine the critical material constant curves for the hydrogen storage container under different crack propagation life design values, and determine the suitability of the hydrogen storage container material based on the critical material constant curves and the material information to be used. The critical material constant curves are curves determined based on material parameters and crack propagation life design values.

[0096] Specifically, the critical value curve of the material constant can be found in the curve graph based on the design crack propagation life of the hydrogen storage container. If the material performance parameter point to be used is within the triangular area enclosed by the critical value curve of the material constant and the horizontal and vertical axes, then the hydrogen storage container material is deemed suitable.

[0097] That is, if the crack propagation life is not less than the design value of the crack propagation life of the hydrogen storage container, or if the material information to be used, i.e., the material performance parameter point, is within the triangular area enclosed by the material constant critical value curve corresponding to the design value of the crack propagation life of the hydrogen storage container and the horizontal and vertical coordinate axes, then the hydrogen storage container material is deemed to be suitable.

[0098] If the crack propagation life is less than the design value of the crack propagation life of the hydrogen storage container, or if the material performance parameter point to be used is outside the triangular area enclosed by the material constant critical value curve corresponding to the design value of the crack propagation life of the hydrogen storage container and the horizontal and vertical coordinate axes, then the hydrogen storage container material is determined to be unsuitable.

[0099] In practical applications, when implementing the method provided by this invention, the various symbols that appear will first be explained:

[0100] a0 Initial crack depth dimension, mm; a Crack depth dimension, mm; a allow Allowable crack depth dimension, mm; a c Critical crack depth dimension, mm; A iA constant, obtained by fitting a cubic polynomial; P Pressure inside the container, MPa; c is half the crack length, mm; C is the material constant used in crack propagation calculations; G i Free surface correction factors in Tables D-401.1 and D-401.2 of ASME VIII-3; g reference stress bending parameter; K I Stress intensity factor, MPa; K IC Fracture toughness, MPa; l: crack length, mm; m: material constant in crack propagation calculation; M S Surface correction factor for surface cracks; M t Correction factor for penetrating cracks; N P The number of pressure cycles required for crack propagation to the critical crack size; N C The number of pressure cycles required for crack propagation to the allowable crack size; N: crack propagation life; P: internal pressure of the vessel, MPa; Q: defect shape factor; q y Plastic zone correction factor; Rel yield strength, MPa; R i Inner radius of container, mm; R0; Outer radius of container, mm; R K Stress intensity factor ratio; t: wall thickness, mm; x: distance measured from the defective surface across the wall thickness, mm; ΔK: stress intensity factor range; λ: shell parameter used to determine surface correction coefficient; α: reference stress parameter.

[0101] This invention summarizes a calculation process for the axial crack propagation life of the inner wall of a hydrogen storage container based on the crack propagation life calculation methods in three pressure vessel standards: ASME VIII-3, API 579, and GB / T 19624. The method for calculating the stress intensity factor is detailed below. Figure 2 For the method of calculating crack propagation life, see [link to relevant documentation]. Figure 3 . Figure 3 K in Ires This is the stress intensity factor under residual stress. Since this invention is carried out in a seamless spinning vessel for hydrogen storage, there is no residual stress, so it is 0; ΔK Ith This is the stress intensity factor threshold value; crack propagation will only occur when the stress intensity factor exceeds this threshold. The Fatigue Assessment Diagram (FAD) process can be found here. Figure 4 .

[0102] See the schematic diagram for the dimensions of the hydrogen storage container. Figure 7 .

[0103] Regarding the method for calculating the stress intensity factor: GB / T 19624 stipulates that for a semi-elliptical crack on the upper surface of an infinitely large plate, the Newman-Raju empirical formula method is used to calculate the stress intensity factor at the crack tip, as follows.

[0104]

[0105]

[0106]

[0107]

[0108]

[0109] For the axial semi-elliptical crack in the inner wall of the hydrogen storage container, a series of interpolation tables are provided for calculation. Since the hydrogen storage container in this case is a thin-walled container, it is approximately equivalent to an infinitely large flat plate for calculation.

[0110] ASME VIII-3 specifies that for axial semi-elliptical cracks inside the cylinder of a hydrogen storage container, the weighted function method should be used to calculate the stress intensity factor at the crack front. A schematic diagram of an axial semi-elliptical crack on the inner wall of a hydrogen storage container is shown below. Figure 6 The calculation formula is as follows.

[0111]

[0112]

[0113] API 579 specifies that for axial semi-elliptical cracks inside the cylinder of a hydrogen storage container, the stress intensity factor at the crack front should be calculated using the weighted function method. The calculation formula is as follows.

[0114]

[0115] This method of stress fitting differs from the method in ASME VIII-3. For the fatigue crack propagation rate model:

[0116] Regarding GB / T 19624:

[0117] da / dN=C(ΔK a ) m

[0118] da / dN=C(0.9×ΔK c ) m

[0119] In this case, a coefficient of 4 is added before the material constant C value.

[0120] For ASME VIII-3:

[0121] da / dN=f(R K )C(ΔK a ) m

[0122] dc / dN=f(R K)C(ΔK c ) m

[0123] API 579 and ASME VIII-3 methods are consistent. For fatigue assessment procedures, there are two main methods: the step-size iteration method and the successive accumulation method. GB / T 19624 uses the successive accumulation method, while ASME VIII-3 and API 579 use the step-size iteration method. The successive accumulation method calculates the crack depth and length direction expansion displacement during each load cycle, as well as the crack tip stress intensity factor value after expansion. This calculation is repeated until the crack fails the FAD assessment or the crack depth reaches the critical size. The step-size iteration method sets a crack expansion step size during crack expansion calculation, calculates the number of load cycles required for the crack depth direction to expand to this step size, calculates the crack length direction expansion size based on this number of cycles, and then calculates the crack tip stress intensity factor value. This calculation process is repeated until the crack fails the FAD assessment or the crack depth reaches the critical size.

[0124] In practical applications, the method for determining the suitability of hydrogen storage container materials provided by this invention can also include the following specific steps:

[0125] Step 1: Calculate the stress intensity factor: Assuming the initial crack depth a0 and the crack depth-to-length ratio a / l, determine the material yield strength R. el A cubic polynomial fitting was performed on the circumferential stress σ at the crack. Obtain the fitting coefficient A i A0 is the fitting coefficient for the constant term; A1 is the fitting coefficient for the linear term; A2 is the fitting coefficient for the quadratic term; and A3 is the fitting coefficient for the cubic term.

[0126] Based on the crack depth-to-length ratio and the crack and wall thickness dimensions, G is calculated by interpolation according to Tables D-401.1 and D-401.2 in ASME VIII-3. i coefficient.

[0127] Calculate the stress intensity factor

[0128] Step 2: Calculate crack propagation life: Based on material parameters, load conditions, and initial crack size, calculate the maximum internal pressure P. max Minimum internal pressure P min Stress intensity factor K Imax K Imin The stress intensity factor ratio R was obtained. K ;

[0129] According to Paris's formula (da / dN=C(ΔK)) m), calculate the distance (a) the crack depth direction and crack length direction propagation is per cycle of internal pressure in the container. i =a i-1 +Cf(R K ) i-1 (ΔK i-1 ) m c i =c i-1 +Cf(R K ) i-1 (ΔKc i-1 ) m ).

[0130] Repeat this extended calculation process until the crack depth reaches 0.8 times the wall thickness or the crack is assessed as failing via the FAD assessment chart. The calculation ends at this point. The total number of iterations used is denoted as N. P The crack depth at this point is the critical crack size a. c .

[0131] Therefore, the critical crack size a c Determine the allowable crack size a allow (a allow =a0 + 0.25 × (a c -a0)) calculates the number of cycles required for the crack to propagate to the allowable crack size, denoted as N. c .

[0132] The total number of iterations is N P / 2 and N c The smaller of the two.

[0133] Step 3, Fatigue Assessment (FAD Assessment): Based on the values ​​of stress, yield strength, tensile strength, fracture toughness, etc., calculate the reference stress under the principal stress.

[0134] The formula for calculating the reference stress is as follows:

[0135] Calculate the film stress:

[0136] Calculate bending stress:

[0137] Calculate the reference stress parameter: α=(a / t) / (1+t / c)

[0138] Calculate reference stress bending parameters:

[0139] Calculate shell parameters:

[0140] Calculate the correction factor for penetration cracks:

[0141] Calculate the surface correction factor for surface cracks:

[0142]

[0143] Calculate the load ratio based on this value.

[0144]

[0145] Calculate the stress intensity of the principal stresses and the stress intensity of secondary stress and residual stress

[0146] Since the seamless hydrogen storage spinning container only has principal stress, the stress intensity of secondary stress and residual stress is... No need to consider this. The stress intensity of the principal stress is the stress intensity factor value calculated in step one.

[0147] Calculate the interaction plasticity factor Φ. In this method, the interaction plasticity factor Φ is 1.

[0148] Calculate the toughness ratio K r .

[0149]

[0150] Then determine on the FAD diagram, see Figure 8 The evaluation method is as follows:

[0151] Figure 8 The curve formula is judge Corresponding toughness ratio K r Is it below the curve's K? r If the value is lower than the specified value, the crack propagation calculation can continue; if it is higher than the specified value, the crack is considered unqualified, and the crack propagation calculation should be stopped.

[0152] After calculating the stress intensity factor, calculate the crack propagation life, such as... Figure 3 When the crack depth reaches 0.8 times the wall thickness or the crack fails the FAD assessment, such as Figure 4 As shown, the calculation ends, and the crack propagation life is obtained.

[0153] The Paris formula (da / dN=C(ΔK)) used in crack propagation life calculations... mThe material constants C and m are related, with lnC and m showing a linear relationship. Furthermore, different materials or the same material under different heat treatments will yield different material constant values. Based on this relationship, the material constants C and m required to meet the service life requirements of hydrogen storage containers are calculated, forming a critical value curve. This curve is used to determine whether the material meets the usage requirements of the hydrogen storage container. The calculation process for the material constants required for the service life of hydrogen storage containers is described below. Figure 5 .

[0154] Step 4: Calculate the material constants.

[0155] The service life requirements for hydrogen storage containers are given, firstly by using the material constants C and m values ​​of similar materials, according to... Figure 5 After calculating a set of critical material constants, the process involves changing the value of m to calculate a second set of critical material constants, and so on, until five sets of critical values ​​are obtained. These five sets of values ​​are then fitted into a curve, which becomes the critical material constant curve. This curve can be used to determine whether the material can meet the lifespan requirements of a hydrogen storage container. The value of m is generally in the range of 1.3 to 7.

[0156] When calculating the critical value curve of material constants, the critical fracture toughness is calculated by taking the set of material constant values ​​with the smallest m value and calculating the fracture toughness value at which the crack propagates to the critical size.

[0157] First, choose the Paris formula (da / dN=C(ΔK)) which is similar to the material. m The material constants C and m are used to determine the fracture toughness K of similar materials. IC Determine the required service life N1 of the container and calculate the stress intensity factor K. I Calculate the crack propagation life N2. Determine if the crack propagation life N2 is equal to the required service life N1. If N2 ≠ N1, proceed according to... Continue the calculation by changing the material constant C until N2 = N1. At this point, C and m form a set of critical material constant values.

[0158] Change the value of m and repeat the above steps to continue the calculation until more than five sets of material constant critical values ​​are obtained. The final material constant critical value curves for different service lives are shown in the figure. Figure 9 .

[0159] Example 2

[0160] This invention provides a system for determining the suitability of hydrogen storage container materials, the system comprising:

[0161] The acquisition module is used to acquire applicable information for the i-th iteration. Applicable information includes: material information and load conditions. Material information includes: material parameters, crack depth size, crack depth-to-length ratio, and material yield strength. i ≥ 1.

[0162] The stress intensity factor determination module is used to determine the stress intensity factor for the i-th cycle based on the applicable information for the i-th cycle.

[0163] The first judgment module is used to determine whether the stress intensity factor of the i-th cycle satisfies the crack propagation condition and obtain the first judgment result.

[0164] The first determining module is used to determine the stress intensity factor ratio of the i-th cycle based on the stress intensity factor of the i-th cycle if the first judgment result is yes.

[0165] The crack propagation information determination module is used to determine the crack propagation information of the i-th cycle based on the stress intensity factor ratio of the (i-1)-th cycle. The crack propagation information includes crack propagation depth and crack propagation length. When i = 1, the initial crack propagation information is determined based on the initial stress intensity factor ratio.

[0166] The second judgment module is used to determine whether the crack propagation depth of the i-th cycle meets the critical preset condition and obtain the second judgment result; the critical preset condition is: the crack propagation depth of the i-th cycle is greater than the thickness of the wall by a set multiple or lower than the set value of the fatigue evaluation curve.

[0167] The second determination module is used to adjust the material parameters and return to the "stress intensity factor determination module" if the second judgment result is negative.

[0168] The third determining module is used to determine the number of cycles in the i-th iteration as the number of crack propagation cycles and the crack propagation depth in the i-th iteration as the critical crack size if the second determination result is yes.

[0169] The fourth determination module is used to determine the allowable crack size based on the critical crack size, and to determine the number of cycles required to reach the allowable crack size based on the number of crack propagation cycles.

[0170] The crack propagation life determination module is used to determine the crack propagation life based on the number of crack propagation cycles and the number of cycles required to reach the allowable crack size.

[0171] The third judgment module is used to determine whether the crack propagation life is not less than the design value of the crack propagation life of the hydrogen storage container. If so, it is determined that the material parameters of the hydrogen storage container are applicable; if not, the material parameters are adjusted and the module is returned to the "acquisition module".

[0172] The fifth determination module is used to determine the critical material constant curves of the hydrogen storage container under different crack propagation life design values, and to judge the suitability of the hydrogen storage container material based on the critical material constant curves and the material information to be used. The critical material constant curves are curves determined based on material parameters and crack propagation life design values.

[0173] Specifically, if the crack propagation life is not less than the design value of the crack propagation life of the hydrogen storage container, or if the material performance parameters to be used, i.e., the material information points, are within the triangular area enclosed by the material constant critical value curve corresponding to the design value of the crack propagation life of the hydrogen storage container and the horizontal and vertical coordinate axes, then the hydrogen storage container material is deemed to be suitable.

[0174] If the crack propagation life is less than the design value of the crack propagation life of the hydrogen storage container, or if the material performance parameter point to be used is outside the triangular area enclosed by the material constant critical value curve corresponding to the design value of the crack propagation life of the hydrogen storage container and the horizontal and vertical coordinate axes, then the material of the hydrogen storage container is determined to be unsuitable.

[0175] Example 3

[0176] This invention provides an electronic device, including a memory and a processor. The memory stores a computer program, and the processor runs the computer program to enable the electronic device to perform the hydrogen storage container material suitability determination method in Embodiment 1.

[0177] In one embodiment, the present invention also provides a computer-readable storage medium storing a computer program that, when executed by a processor, implements the method for determining the suitability of hydrogen storage container materials in Embodiment 1.

[0178] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on its differences from other embodiments. Similar or identical parts between embodiments can be referred to interchangeably. For the systems disclosed in the embodiments, since they correspond to the methods disclosed in the embodiments, the descriptions are relatively simple; relevant parts can be referred to the method section.

[0179] This document uses specific examples to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of the present invention. Furthermore, those skilled in the art will recognize that, based on the ideas of the present invention, there will be changes in the specific implementation methods and application scope. Therefore, the content of this specification should not be construed as a limitation of the present invention.

Claims

1. A method for determining the suitability of hydrogen storage container materials, characterized in that, The method includes: Get the i The applicable information for the next cycle includes: material information and load conditions; the material information includes: material parameters, crack depth size, crack depth-to-length ratio, and material yield strength. i ≥1; Material parameters include material constants C and m; According to the i The applicable information for the next iteration determines the first... i Stress intensity factor of the next cycle; Judge the first i The first judgment result is obtained by determining whether the stress intensity factor of the next cycle satisfies the crack propagation condition; If the first judgment result is yes, then according to the first... i The stress intensity factor of the second cycle is determined. i The ratio of stress intensity factor in each cycle; According to the i The stress intensity factor ratio of the -1st cycle determines the first cycle. i Crack propagation information for the next cycle; the crack propagation information includes: crack propagation depth and crack propagation length; when i When the stress intensity factor ratio is 1, the initial crack propagation information is determined based on the initial stress intensity factor ratio. Judge the first i The second judgment result is obtained by determining whether the crack propagation depth in the next cycle meets the critical preset condition; the critical preset condition is: the load ratio is higher than the set value of the fatigue evaluation curve or the... i The crack propagation depth in the next cycle is greater than the wall thickness by a set multiple; If the second judgment result is negative, then adjust the crack propagation information and return "According to the first..." i The applicable information for the next iteration determines the first... i The "stress intensity factor of the next cycle" step; If the second judgment result is yes, then the first... i The number of cycles is determined as the number of crack propagation cycles, and the number of cycles is... i The crack propagation depth of the next cycle is determined as the critical crack size; The allowable crack size is determined based on the critical crack size, and the number of cycles required to reach the allowable crack size is determined based on the number of crack propagation cycles. The crack propagation life is determined based on the number of crack propagation cycles and the number of cycles required to reach the allowable crack size; Determine whether the crack propagation life is not less than the design value of the crack propagation life of the hydrogen storage container. If yes, then the suitability of the hydrogen storage container material is determined; otherwise, adjust the material information and return to "Get the first...". i The "Applicable Information for the Next Loop" step; Determine the critical material constant curves for the hydrogen storage container under different design values ​​for crack propagation life, and determine the suitability of the hydrogen storage container material based on the critical material constant curves and the material constants corresponding to the proposed material information. Specifically, this includes: Selecting material constants C and m to determine crack propagation life Does this equal the required service life? ,like ,according to Continue the calculation by changing the material constant C until... Then, C and m at this point are a set of critical material constants; change the value of m and repeat the process of "selecting material constants C and m to determine crack propagation life". Does this equal the required service life? ,like ,according to Continue the calculation by changing the material constant C until... "The steps are repeated until more than five sets of material constant critical values ​​are obtained, and finally the material constant critical value curves under different service lives are obtained; The material constant is the value after the material constant C has been changed. If the crack propagation life is not less than the design value of the crack propagation life of the hydrogen storage container, or if the material constant corresponding to the material information to be used is within the triangular area enclosed by the critical value curve of the material constant corresponding to the design value of the crack propagation life of the hydrogen storage container and the horizontal and vertical axes, then the hydrogen storage container material is deemed to be suitable. If the crack propagation life is less than the design value of the crack propagation life of the hydrogen storage container, or if the material constant corresponding to the material information to be used is outside the triangular area enclosed by the critical value curve of the material constant corresponding to the design value of the crack propagation life of the hydrogen storage container and the horizontal and vertical axes, then the material of the hydrogen storage container is determined to be unsuitable.

2. The method for determining the suitability of hydrogen storage container materials according to claim 1, characterized in that, According to the i The applicable information for the next iteration determines the first... i The stress intensity factor for each cycle specifically includes: Based on the free surface correction coefficient table, according to the first i The material information for the next cycle is determined using interpolation. i Correction coefficient for the next cycle; According to the i For the load condition of the second cycle, a cubic polynomial fitting is performed on the circumferential stress of the crack to obtain the third... i The fitting coefficients for the next iteration; According to the i The correction coefficient of the second cycle, the first i The fitting coefficients of the second iteration and the first iteration i The crack depth size of the next cycle determines the first... i Stress intensity factor for each cycle.

3. The method for determining the suitability of hydrogen storage container materials according to claim 1, characterized in that, The method for determining the fatigue assessment curve specifically includes: According to the i The applicable information for the next iteration determines the first... i Reference stress for the next cycle; According to the i The material yield strength of the second cycle and the first cycle i The reference stress calculation for the next cycle i The load ratio of the next cycle; According to the i The stress intensity factor of the second cycle is determined. i The toughness ratio of the next cycle; According to the i The load ratio of the second cycle and the first cycle i Formula for constructing the toughness ratio curve in the next cycle; The fatigue assessment curve is determined based on the curve construction formula.

4. The method for determining the suitability of hydrogen storage container materials according to claim 3, characterized in that, The expression for the curve construction formula is: ; in, The toughness ratio; This represents the load ratio.

5. The method for determining the suitability of hydrogen storage container materials according to claim 3, characterized in that, The formula for calculating the load ratio specifically includes: ; in, The load ratio; For reference stress; This represents the yield strength of the material.

6. A system for determining the suitability of hydrogen storage container materials, characterized in that, The method for determining the suitability of hydrogen storage container materials according to any one of claims 1-5, wherein the system comprises: The acquisition module is used to acquire the first... i Applicable information for the next cycle; the applicable information includes: material information and load conditions; the material information includes: material parameters, crack depth size, crack depth-to-length ratio, and material yield strength; i ≥1; Material parameters include material constants C and m; The stress intensity factor determination module is used to determine the stress intensity factor based on the first i The applicable information for the next iteration determines the first... i Stress intensity factor of the next cycle; The first judgment module is used to judge the first... i The first judgment result is obtained by determining whether the stress intensity factor of the next cycle satisfies the crack propagation condition; The first determining module is configured to, if the first determining result is yes, then according to the first determining module... i The stress intensity factor of the second cycle is determined. i The stress intensity factor ratio of the next cycle; The crack propagation information determination module is used to determine the crack propagation information based on the first... i The stress intensity factor ratio of the -1st cycle determines the first cycle. i Crack propagation information for the next cycle; the crack propagation information includes: crack propagation depth and crack propagation length; when i When the stress intensity factor ratio is 1, the initial crack propagation information is determined based on the initial stress intensity factor ratio. The second judgment module is used to judge the first... i The second judgment result is obtained by determining whether the crack propagation depth in the next cycle meets the critical preset condition; the critical preset condition is: the load ratio is higher than the set value of the fatigue evaluation curve or the... i The crack propagation depth in the next cycle is greater than the wall thickness by a set multiple; The second determining module is used to adjust the crack propagation information and return to the "stress intensity factor determining module" if the second determination result is negative. The third determining module is used to, if the second determining result is yes, then... i The number of cycles is determined as the number of crack propagation cycles, and the number of cycles is... i The crack propagation depth of the next cycle is determined as the critical crack size; The fourth determining module is used to determine the allowable crack size based on the critical crack size, and to determine the number of cycles required to reach the allowable crack size based on the number of crack propagation cycles. A crack propagation life determination module is used to determine the crack propagation life based on the number of crack propagation cycles and the number of cycles to reach the allowable crack size; The third judgment module is used to determine whether the crack propagation lifetime is not less than the design value of the crack propagation lifetime of the hydrogen storage container. If so, it is determined that the hydrogen storage container material is suitable; if not, the material information is adjusted and the module is returned to the "acquisition module". The fifth determination module is used to determine the critical value curve of the material constant of the hydrogen storage container under different crack propagation life design values, and to determine whether the material of the hydrogen storage container is suitable based on the critical value curve of the material constant and the material constant corresponding to the material information to be used.

7. An electronic device, characterized in that, The device includes a memory and a processor, the memory being used to store a computer program, and the processor running the computer program to cause the electronic device to perform the method for determining the suitability of hydrogen storage container materials as described in any one of claims 1 to 5.

8. A computer-readable storage medium, characterized in that, It stores a computer program that, when executed by a processor, implements the method for determining the suitability of hydrogen storage container materials as described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Safety assessment method for high-temperature pressure pipeline with crack type defects