Coil component

By setting a first glass layer and ferrite layers on both sides on the substrate, the hole area ratio and crystal grain size difference are controlled, which solves the problem of insufficient adhesion between the dielectric glass layer and the magnetic layer and improves the overall performance of the coil component.

CN117476337BActive Publication Date: 2026-11-24MURATA MFG CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310939881.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-07-29
Filing Date
2023-07-27
Publication Date
2026-11-24
Estimated Expiration
2043-07-27

AI Technical Summary

Technical Problem

In existing laminated coil components, the adhesion between the dielectric glass layer and the magnetic layer is insufficient.

Method used

A first glass layer and two ferrite layers are set on the substrate. By controlling the hole area ratio and the difference in crystal grain size, the adhesion between the glass layer and the ferrite layer is improved.

Benefits of technology

This enhances the bonding strength between the glass layer and the ferrite layer, improving the overall performance of the coil components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117476337B_ABST
    Figure CN117476337B_ABST
Patent Text Reader

Abstract

The present application relates to a coil component. A coil component (1A) includes: a base body (10A) having a first glass layer (15a), a first ferrite layer (16a) adjacent to one main surface side of the first glass layer (15a), and a second ferrite layer (16b) adjacent to the other main surface side of the first glass layer (15a) in a stacking direction; a coil provided inside the first glass layer (15a); and an external electrode provided on a surface of the base body (10A) and electrically connected to the coil. In the first ferrite layer (16a), an area ratio of voids in a first inner side region (F1) is greater than an area ratio of voids in a first intermediate region (H1), and an average crystal grain size of ferrite in the first inner side region (F1) is smaller than an average crystal grain size of ferrite in the first intermediate region (H1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to coil components. Background Technology

[0002] Patent Document 1 discloses a stacked coil component in which a pair of magnetic body layers are formed on the two main surfaces of a first dielectric glass layer in which an internal conductor is embedded, and a pair of second dielectric glass layers are formed on the main surfaces of each pair of magnetic body layers. The component is characterized in that at least one of the pair of second dielectric glass layers has a thickness of 10 to 64 μm.

[0003] Patent Document 1: Japanese Patent Application Publication No. 2019-102507

[0004] However, after conducting research, the inventors of this invention discovered that in the laminated coil component described in Patent Document 1, there is a concern that the adhesion between the dielectric glass layer (also called the glass layer) and the magnetic layer (also called the ferrite layer) becomes insufficient. Summary of the Invention

[0005] The present invention was made to solve the above-mentioned problems, and its purpose is to provide a coil component with excellent adhesion between the glass layer and the ferrite layer.

[0006] The coil component of the present invention is characterized by comprising: a substrate having a first glass layer, a first ferrite layer adjacent to one main surface side of the first glass layer, and a second ferrite layer adjacent to the other main surface side of the first glass layer in a lamination direction; a coil disposed inside the first glass layer; and an external electrode disposed on the surface of the substrate and electrically connected to the coil. In the first ferrite layer, a first position is defined as the location of the main surface side of the first glass layer, a second position is defined as a position 10 μm away from the first position in the lamination direction, and a third position is defined as the location of the main surface opposite to the first glass layer. When the position of the main surface is set as the third position, the position 10 μm away from the third position in the stacking direction is set as the fourth position, the region between the first position and the second position is set as the first inner region, the region between the third position and the fourth position is set as the first outer region, and the region between the second position and the fourth position is set as the first middle region, the area ratio of the voids in the first inner region is greater than the area ratio of the voids in the first middle region, and the average crystal grain size of the ferrite in the first inner region is smaller than the average crystal grain size of the ferrite in the first middle region.

[0007] According to the present invention, a coil component with excellent adhesion between the glass layer and the ferrite layer can be provided. Attached Figure Description

[0008] Figure 1 This is a perspective schematic diagram showing an example of a coil component according to Embodiment 1 of the present invention.

[0009] Figure 2 It means Figure 1 A schematic cross-sectional view of an example of a section along line segment A1-A2 of the coil component shown.

[0010] Figure 3 It means Figure 1 A schematic cross-sectional view of an example of a section along line segment B1-B2 of the coil component shown.

[0011] Figure 4 It means Figure 1 A schematic cross-sectional view of an example of a section along line segment C1-C2 of the coil component shown.

[0012] Figure 5 It means to Figure 1 A three-dimensional schematic diagram of an example of the disassembled state of the coil component (but excluding the external electrodes).

[0013] Figure 6 This is a perspective schematic diagram showing an example of a coil component according to Embodiment 2 of the present invention.

[0014] Figure 7 It means Figure 6 A schematic cross-sectional view of an example of a section along line segment A3-A4 of the coil component shown.

[0015] Explanation of reference numerals in the attached figures

[0016] 1A, 1B...coil components; 10A, 10B...substrate; 11a...first end face of the substrate; 11b...second end face of the substrate; 12a...first main face of the substrate; 12b...second main face of the substrate; 13a...first side face of the substrate; 13b...second side face of the substrate; 15a...first glass layer; 15aa, 15ab, 15ac, 15ad, 15ae, 16aa, 16ab, 16ba, 16bb...insulating layer; 15b...second glass layer; 15c...third glass layer; 16a...first ferrite layer; 16b...second ferrite layer; 21...first external electrode; 22...second external electrode; 23...third external electrode; 24...fourth external electrode; 31...first coil; 32...second coil; 41a, 41b, 42a, 42b... Coil conductors; 51... First lead conductor; 52... Second lead conductor; 53... Third lead conductor; 54... Fourth lead conductor; 61a, 61b, 62a, 62b... Pad portions; 71a, 72a... Through-hole conductors; D1, D2... Coil shafts; E1... First position; E2... Second position; E3... Third position; E4... Fourth position; E5... Fifth position; E6... Sixth position; E7... Seventh position; E8... Eighth position; F1... First inner region; F2... Second inner region; G1... First outer region; G2... Second outer region; H1... First middle region; H2... Second middle region; L... Length direction; T... Height direction; W... Width direction. Detailed Implementation

[0017] The coil component of the present invention will now be described. Furthermore, the present invention is not limited to the following structures, and appropriate modifications can be made without departing from the spirit of the invention. Additionally, structures obtained by combining multiple preferred structures described below are also part of the present invention.

[0018] The embodiments shown below are illustrative, and of course, partial substitutions or combinations of the structures shown in different embodiments are possible. From Embodiment 2 onwards, descriptions of matters common to Embodiment 1 are omitted, and the differences are mainly explained. In particular, the same effects resulting from the same structure are not mentioned sequentially in each embodiment.

[0019] In the following description, unless otherwise specified, each embodiment will be referred to as "the coil component of the present invention".

[0020] In the following embodiments, a common-mode choke coil is shown as an example of a coil component of the present invention. The coil component of the present invention can also be applied to coil components other than common-mode choke coils.

[0021] The attached diagrams are schematic diagrams, and their dimensions, aspect ratios, and scales may sometimes differ from the actual product.

[0022] In this specification, terms indicating the relationship between elements (e.g., "parallel", "orthogonal", etc.) and terms indicating the shape of elements refer not only to strict forms as they are literally, but also to substantially equivalent ranges, such as ranges containing a few percent of differences.

[0023] The coil component of the present invention is characterized by comprising: a substrate having a first glass layer, a first ferrite layer adjacent to one main surface side of the first glass layer, and a second ferrite layer adjacent to the other main surface side of the first glass layer in a lamination direction; a coil disposed inside the first glass layer; and an external electrode disposed on the surface of the substrate and electrically connected to the coil. In the first ferrite layer, a first position is defined as the location of the main surface side of the first glass layer, a second position is defined as a position 10 μm away from the first position in the lamination direction, and a third position is defined as the location of the main surface opposite to the first glass layer. When the position of the main surface is set as the third position, the position 10 μm away from the third position in the stacking direction is set as the fourth position, the region between the first position and the second position is set as the first inner region, the region between the third position and the fourth position is set as the first outer region, and the region between the second position and the fourth position is set as the first middle region, the area ratio of the voids in the first inner region is greater than the area ratio of the voids in the first middle region, and the average crystal grain size of the ferrite in the first inner region is smaller than the average crystal grain size of the ferrite in the first middle region.

[0024] [Implementation Method 1]

[0025] In the coil component of Embodiment 1 of the present invention, the substrate has a first glass layer, a first ferrite layer adjacent to one main surface side of the first glass layer, and a second ferrite layer adjacent to the other main surface side of the first glass layer in the stacking direction.

[0026] Figure 1 This is a perspective schematic diagram showing an example of a coil component according to Embodiment 1 of the present invention.

[0027] Figure 1 The coil component 1A shown has a base 10A, a first external electrode 21, a second external electrode 22, a third external electrode 23, and a fourth external electrode 24. Although in Figure 1Not shown in the figure, but as described later, the coil component 1A also has a first coil and a second coil disposed inside the base 10A.

[0028] Coil component 1A is also known as a common-mode choke coil as a type of noise filter for circuits.

[0029] In this instruction manual, such as Figure 1 As shown, the length, height, and width directions are defined by L, T, and W, respectively. Here, the length direction L, height direction T, and width direction W are orthogonal to each other.

[0030] The substrate 10A has a first end face 11a and a second end face 11b opposite each other in the length direction L, a first main face 12a and a second main face 12b opposite each other in the height direction T, and a first side face 13a and a second side face 13b opposite each other in the width direction W, for example, it is cuboid or substantially cuboid.

[0031] The first end face 11a and the second end face 11b of the substrate 10A do not need to be strictly orthogonal to the length direction L. Furthermore, the first main face 12a and the second main face 12b of the substrate 10A do not need to be strictly orthogonal to the height direction T. Additionally, the first side face 13a and the second side face 13b of the substrate 10A do not need to be strictly orthogonal to the width direction W.

[0032] When the coil component 1A is mounted on the substrate, the first main surface 12a of the substrate 10A becomes the mounting surface.

[0033] Preferably, the substrate 10A has rounded corners and edges. The corners of the substrate 10A are the parts where three faces of the substrate 10A intersect. The edges of the substrate 10A are the parts where two faces of the substrate 10A intersect.

[0034] The substrate 10A has a first glass layer 15a, a first ferrite layer 16a, and a second ferrite layer 16b in the lamination direction. In the substrate 10A, the lamination direction of the first glass layer 15a, etc., is parallel to the height direction T. That is, in the substrate 10A, the lamination direction of the first glass layer 15a, etc., is orthogonal to the first main surface 12a of the substrate 10A, which serves as the mounting surface.

[0035] In the stacking direction (here, the height direction T), the first ferrite layer 16a is adjacent to one main surface of the first glass layer 15a, and the second ferrite layer 16b is adjacent to the other main surface of the first glass layer 15a. That is, in the substrate 10A, in the stacking direction (here, the height direction T), the first glass layer 15a is sandwiched between the first ferrite layer 16a and the second ferrite layer 16b.

[0036] In this specification, the stacking direction (here, the height direction) is referred to as the vertical direction, the first main surface of the substrate is referred to as the lower side, and the second main surface of the substrate is referred to as the upper side, but these directions are not limited and may be appropriately varied depending on the configuration of the coil components. For example, the substrate 10A may be such that the first ferrite layer 16a is located on the lower side in the vertical direction and the second ferrite layer 16b is located on the upper side in the vertical direction, or it may be such that the first ferrite layer 16a is located on the upper side in the vertical direction and the second ferrite layer 16b is located on the lower side in the vertical direction.

[0037] Although Figure 1 Not shown in the diagram, but as described later, a first coil and a second coil are disposed inside the first glass layer 15a.

[0038] The first glass layer 15a, for example, has a multilayer structure consisting of multiple insulating layers stacked in the stacking direction (here, the height direction T), as described later.

[0039] The first glass layer 15a is made of glass-ceramic material (also known as dielectric glass material).

[0040] The first glass layer 15a preferably comprises a glass material containing K, B, and Si. That is, the glass-ceramic material constituting the first glass layer 15a preferably comprises a glass material containing K, B, and Si.

[0041] The glass material contained in the first glass layer 15a preferably contains, when the total weight is set to 100% by weight, 0.5% to 5% by weight of K (calculated as K2O), 10% to 25% by weight of B (calculated as B2O3), 70% to 85% by weight of Si (calculated as SiO2), and 0% to 5% by weight of Al (calculated as Al2O3).

[0042] The first glass layer 15a preferably includes a filler containing at least one of quartz (SiO2) and alumina (Al2O3). That is, the glass-ceramic material constituting the first glass layer 15a preferably includes a filler containing at least one of quartz and alumina. The inclusion of quartz as a filler in the glass-ceramic material constituting the first glass layer 15a easily improves the high-frequency characteristics of the coil component 1A. Furthermore, the inclusion of alumina as a filler in the glass-ceramic material constituting the first glass layer 15a easily improves the mechanical strength of the substrate 10A.

[0043] When the glass-ceramic material constituting the first glass layer 15a includes quartz and alumina as fillers, the glass-ceramic material preferably includes, when the total weight is set to 100% by weight: 60% or more and 66% or less glass material, 34% or more and 37% or less quartz as filler, and 0.5% or more and 4% or less alumina as filler.

[0044] The first ferrite layer 16a and the second ferrite layer 16b each have a multilayer structure formed by stacking multiple insulating layers in the stacking direction (here, the height direction T), as described later.

[0045] The first ferrite layer 16a and the second ferrite layer 16b are preferably made of Ni-Cu-Zn based ferrite materials. In this case, the inductance of the coil component 1A tends to increase.

[0046] The Ni-Cu-Zn ferrite materials constituting the first ferrite layer 16a and the second ferrite layer 16b are preferably, when the total weight is set to 100 mol%, containing: 40 mol% or more and 49.5 mol% Fe (calculated as Fe2O3), 5 mol% or more and 35 mol% Zn (calculated as ZnO), 6 mol% or more and 12 mol% Cu (calculated as CuO), and 8 mol% or more and 40 mol% Ni (calculated as NiO).

[0047] The Ni-Cu-Zn ferrite materials constituting the first ferrite layer 16a and the second ferrite layer 16b may also contain additives such as Mn3O4, Co3O4, SnO2, Bi2O3, and SiO2.

[0048] The Ni-Cu-Zn ferrite materials constituting the first ferrite layer 16a and the second ferrite layer 16b may also contain unavoidable impurities.

[0049] The dimensions T along the height direction of the first glass layer 15a, the first ferrite layer 16a, and the second ferrite layer 16b can be the same, different, or partially different. When the dimensions T along the height direction of the first glass layer 15a, the first ferrite layer 16a, and the second ferrite layer 16b are different or partially different, their size relationship is not particularly limited.

[0050] The glass layer and ferrite layer are distinguished as follows. First, after sealing the coil component with resin as needed, the coil component is ground along a first direction (e.g., width direction) orthogonal to the lamination direction (e.g., height direction). This exposes a cross-section along a second direction (e.g., length direction) orthogonal to both the lamination direction and the first direction at approximately the center of the first direction. Next, for regions in the exposed cross-section of the substrate where different layers can be presumed to exist (e.g., regions where different layers can be presumed to exist based on differences in hue, etc.), the composition (the percentage of detected elements) is determined using scanning transmission electron microscopy-energy dispersive X-ray analysis (STEM-EDX). Then, the glass layer and ferrite layer are distinguished from the obtained composition by determining whether the constituent material of each layer is a glass-ceramic material or a ferrite material.

[0051] The first external electrode 21 is disposed on the surface of the substrate 10A. Figure 1 In the example shown, the first external electrode 21 extends from a portion of the first side surface 13a of the substrate 10A to portions of each of the first main surface 12a and the second main surface 12b.

[0052] The second external electrode 22 is disposed on the surface of the substrate 10A. Figure 1 In the example shown, the second external electrode 22 extends from a portion of the second side surface 13b of the substrate 10A to portions of each of the first main surface 12a and the second main surface 12b. Furthermore, the second external electrode 22 is positioned opposite the first external electrode 21 in the width direction W.

[0053] The third external electrode 23 is disposed on the surface of the substrate 10A. Figure 1 In the example shown, the third external electrode 23 is separated from the first external electrode 21 in the length direction L, extending from a portion of the first side surface 13a of the substrate 10A to a portion of each of the first main surface 12a and the second main surface 12b.

[0054] The fourth external electrode 24 is disposed on the surface of the substrate 10A. Figure 1 In the example shown, the fourth external electrode 24, separated from the second external electrode 22 in the length direction L, extends from a portion of the second side surface 13b of the substrate 10A to portions of each of the first main surface 12a and the second main surface 12b. Furthermore, the fourth external electrode 24 is positioned opposite the third external electrode 23 in the width direction W.

[0055] As described above, the first external electrode 21, the second external electrode 22, the third external electrode 23, and the fourth external electrode 24 are disposed at positions separated from each other on the surface of the substrate 10A.

[0056] As described above, when a portion of each of the first external electrode 21, the second external electrode 22, the third external electrode 23, and the fourth external electrode 24 is disposed on the first main surface 12a of the base 10A, which serves as the mounting surface, the mounting capability of the coil component 1A is easily improved.

[0057] Furthermore, the configuration of the first external electrode 21, the second external electrode 22, the third external electrode 23, and the fourth external electrode 24 is not limited to... Figure 1 As shown in the diagram.

[0058] The first external electrode 21, the second external electrode 22, the third external electrode 23, and the fourth external electrode 24 may each have a single-layer structure or a multi-layer structure.

[0059] When the first external electrode 21, the second external electrode 22, the third external electrode 23 and the fourth external electrode 24 each have a single-layer structure, the constituent materials of each external electrode may include, for example, Ag, Au, Cu, Pd, Ni, Al, and alloys containing at least one of these metals.

[0060] When the first external electrode 21, the second external electrode 22, the third external electrode 23 and the fourth external electrode 24 are all multilayer structures, each external electrode may also have, for example, a substrate electrode containing Ag, a Ni-plated electrode and a Sn-plated electrode sequentially from the surface side of the substrate 10A.

[0061] Figure 2 It means Figure 1 A schematic cross-sectional view of an example of a section along line segment A1-A2 of the coil component shown. Figure 3 It means Figure 1 A schematic cross-sectional view of an example of a section along line segment B1-B2 of the coil component shown. Figure 4 It means Figure 1 A schematic cross-sectional view of an example of a section along line segment C1-C2 of the coil component shown.

[0062] like Figure 2 , Figure 3 as well as Figure 4 As shown, the first glass layer 15a is formed by sequentially stacking insulating layers 15aa, 15ab, 15ac, 15ad, and 15ae in the stacking direction (here, the height direction T). More specifically, in the first glass layer 15a, insulating layers 15aa, 15ab, 15ac, 15ad, and 15ae are sequentially stacked from the first main surface 12a side of the substrate 10A toward the second main surface 12b side.

[0063] The insulating layers 15aa, 15ab, 15ac, 15ad, and 15ae are preferably made of the same material as each other, but they may also be different from each other or partially different.

[0064] In addition, Figure 2 , Figure 3 as well as Figure 4 For ease of explanation, the boundaries between the insulating layers constituting the first glass layer 15a are shown, but these boundaries are not actually clearly visible.

[0065] like Figure 2 , Figure 3 as well as Figure 4 As shown, the first ferrite layer 16a is formed by stacking insulating layers 16aa and 16ab in the stacking direction (here, the height direction T). More specifically, in the first ferrite layer 16aa and 16ab are stacked sequentially from the side of the first glass layer 15a.

[0066] In addition, Figure 2 , Figure 3 as well as Figure 4 For ease of explanation, the boundaries between the insulating layers constituting the first ferrite layer 16a are shown, but these boundaries are not actually clearly visible.

[0067] like Figure 2 , Figure 3 as well as Figure 4 As shown, the second ferrite layer 16b is formed by stacking insulating layers 16ba and 16bb in the stacking direction (here, the height direction T). More specifically, in the second ferrite layer 16b, insulating layers 16ba and 16bb are stacked sequentially from the side of the first glass layer 15a.

[0068] In addition, Figure 2 , Figure 3 as well as Figure 4 For ease of explanation, the boundaries between the insulating layers constituting the second ferrite layer 16b are shown, but these boundaries are not actually clearly visible.

[0069] A first coil 31 and a second coil 32 are disposed inside the first glass layer 15a.

[0070] The first coil 31 and the second coil 32 are insulated from each other.

[0071] For the first coil 31, more specifically, one end of the first coil 31 is via Figure 3 The first lead-out conductor 51 shown is electrically connected to the first external electrode 21. Figure 3In the example shown, the first lead conductor 51 is exposed on the first side 13a of the substrate 10A, and the first external electrode 21 is connected to the exposed portion of the first lead conductor 51.

[0072] For the first coil 31, more specifically, the other end of the first coil 31 is via Figure 3 The second lead-out conductor 52 shown is electrically connected to the second external electrode 22. Figure 3 In the example shown, the second lead conductor 52 is exposed on the second side 13b of the substrate 10A, and the second external electrode 22 is connected to the exposed portion of the second lead conductor 52.

[0073] For the second coil 32, more specifically, one end of the second coil 32 is via Figure 4 The third lead-out conductor 53 shown is electrically connected to the third external electrode 23. Figure 4 In the example shown, the third lead conductor 53 is exposed on the first side 13a of the substrate 10A, and the third external electrode 23 is connected to the exposed portion of the third lead conductor 53.

[0074] For the second coil 32, more specifically, the other end of the second coil 32 is via Figure 4 The fourth lead-out conductor 54 shown is electrically connected to the fourth external electrode 24. Figure 4 In the example shown, the fourth lead conductor 54 is exposed on the second side 13b of the substrate 10A, and the fourth external electrode 24 is connected to the exposed portion of the fourth lead conductor 54.

[0075] As described above, coil component 1A is a common-mode choke coil provided with a first coil 31 and a second coil 32 insulated from the first coil 31.

[0076] like Figure 2 As shown, the first coil 31 has a coil shaft D1. Figure 2 In the example shown, the coil axis D1 of the first coil 31 passes through the first main surface 12a and the second main surface 12b of the substrate 10A along the height direction T. That is, the direction of the coil axis D1 of the first coil 31 is orthogonal to the first main surface 12a of the substrate 10A, which serves as the mounting surface.

[0077] like Figure 2 As shown, the second coil 32 has a coil shaft D2. In Figure 2 In the example shown, the coil axis D2 of the second coil 32 passes through the first main surface 12a and the second main surface 12b of the substrate 10A along the height direction T. That is, the direction of the coil axis D2 of the second coil 32 is orthogonal to the first main surface 12a of the substrate 10A, which serves as the mounting surface.

[0078] Furthermore, the coil axis D1 of the first coil 31 and the coil axis D2 of the second coil 32 pass through the inner circumference of the first coil 31 and the inner circumference of the second coil 32 when viewed from the height direction T, respectively. For ease of explanation, in Figure 2 As shown in the image.

[0079] As described above, the stacking direction of the insulating layer constituting the first glass layer 15a, the direction of the coil axis D1 of the first coil 31, and the direction of the coil axis D2 of the second coil 32 are along the same height direction T and are orthogonal to the first main surface 12a of the substrate 10A, which serves as the mounting surface.

[0080] Figure 5 It means to Figure 1 A three-dimensional schematic diagram of an example of the disassembled state of the coil component (but excluding the external electrodes).

[0081] like Figure 5 As shown, the first coil 31 includes coil conductor 41a and coil conductor 41b.

[0082] The coil conductor 41a is disposed on the main surface of the insulating layer 15aa. The coil conductor 41a has a pad portion 61a at one end and is connected to the first lead conductor 51 at the other end.

[0083] The coil conductor 41b is disposed on the main surface of the insulating layer 15ab. The coil conductor 41b has a pad portion 61b at one end and is connected to the second lead conductor 52 at the other end.

[0084] When viewed from the height direction T, the pad portion 61a of the coil conductor 41a overlaps with the pad portion 61b of the coil conductor 41b.

[0085] In the insulating layer 15ab, a through-hole conductor 71a is provided at a position that overlaps with the pad portion 61a and the pad portion 61b when viewed from the height direction T.

[0086] In coil component 1A, insulating layers 15aa and 15ab are stacked along the stacking direction (here, the height direction T), thereby stacking and electrically connecting coil conductors 41a and 41b together with these insulating layers along the height direction T. More specifically, the pad portions 61a and 61b of coil conductors 41a and 41b are electrically connected via via conductors 71a. Thus, coil conductors 41a and 41b are electrically connected, thereby forming the first coil 31.

[0087] like Figure 5 As shown, the second coil 32 includes coil conductor 42a and coil conductor 42b.

[0088] The coil conductor 42a is disposed on the main surface of the insulating layer 15ac. The coil conductor 42a has a pad portion 62a at one end and is connected to the fourth lead conductor 54 at the other end.

[0089] The coil conductor 42b is disposed on the main surface of the insulating layer 15ad. The coil conductor 42b has a pad portion 62b at one end and is connected to the third lead conductor 53 at the other end.

[0090] When viewed from the height direction T, the pad portion 62a of the coil conductor 42a overlaps with the pad portion 62b of the coil conductor 42b.

[0091] In the insulating layer 15ad, a through-hole conductor 72a is provided at a position that overlaps with the pad portion 62a and the pad portion 62b when viewed from the height direction T.

[0092] In coil component 1A, insulating layers 15ac and 15ad are stacked along the stacking direction (here, the height direction T), thereby stacking and electrically connecting coil conductors 42a and 42b together with these insulating layers along the height direction T. More specifically, the pad portions 62a and 62b of coil conductors 42a and 42b are electrically connected via via conductors 72a. Thus, coil conductors 42a and 42b are electrically connected, thereby forming the second coil 32.

[0093] In the first glass layer 15a, relative to the stacked portions of insulating layers 15aa, 15ab, 15ac, and 15ad, an insulating layer 15ae, which does not contain coil conductors, lead conductors, or through-hole conductors, is further stacked on the second main surface 12b side of the substrate 10A. Thus, the first coil 31 and the second coil 32 (particularly the second coil 32) are disposed inside the first glass layer 15a.

[0094] Furthermore, in the first glass layer 15a, at least one insulating layer without conductors such as coil conductors, lead conductors, or via conductors may be further stacked on at least one side of the substrate 10A, on the first main surface 12a side and the second main surface 12b side, relative to the stacked portions of insulating layers 15aa, 15ab, 15ac, 15ad, and 15ae. That is, the number of insulating layers constituting the first glass layer 15a is not limited to [specific number of layers]. Figure 5 The methods shown (5).

[0095] Furthermore, the number of coil conductors constituting each of the first coil 31 and the second coil 32 is not limited to Figure 5 The methods shown are two.

[0096] When viewed from the stacking direction (here, the height direction T), each coil conductor can be Figure 5 The shape shown could consist only of straight sections, or it could consist only of curved sections, or it could consist of both straight and curved sections. That is, when viewed from the height direction T, the first coil 31 and the second coil 32 could respectively be... Figure 5 The shape shown can be composed only of straight lines, or it can be composed only of curved lines, or it can be composed of both straight lines and curved lines.

[0097] When viewed from the stack-up direction (here, the height direction T), each pad portion can be... Figure 5 The circular shape shown can also be a polygonal shape.

[0098] Each coil conductor may also have a pad at its end, not independently.

[0099] Materials used to construct the individual coil conductors, individual lead conductors, and individual through-hole conductors include, for example, Ag, Au, Cu, Pd, Ni, Al, and alloys containing at least one of these metals.

[0100] As described above, the first ferrite layer 16a is formed by stacking insulating layers 16aa and 16ab in the stacking direction (here, the height direction T).

[0101] Furthermore, the number of insulating layers constituting the first ferrite layer 16a is not limited to Figure 5 As shown (2 points). That is, the number of insulating layers constituting the first ferrite layer 16a can be either only one or multiple.

[0102] As described above, the second ferrite layer 16b is formed by stacking insulating layers 16ba and 16bb in the stacking direction (here, the height direction T).

[0103] Furthermore, the number of insulating layers constituting the second ferrite layer 16b is not limited to Figure 5 The method shown (2). That is, the number of insulating layers constituting the second ferrite layer 16b can be only one or multiple.

[0104] like Figure 2As shown, in the coil component 1A, in the first ferrite layer 16a, the position of the main surface on the side of the first glass layer 15a is set as the first position E1, the position 10 μm away from the first position E1 in the stacking direction (here, the height direction T) is set as the second position E2, the position of the main surface on the opposite side of the first glass layer 15a is set as the third position E3, the position 10 μm away from the third position E3 in the stacking direction (here, the height direction T) is set as the fourth position E4, the area between the first position E1 and the second position E2 is set as the first inner area F1, the area between the third position E3 and the fourth position E4 is set as the first outer area G1, and the area between the second position E2 and the fourth position E4 is set as the first middle area H1, satisfying the following features (1) and (2).

[0105] (1) The area ratio of the cavities (pores) in the first inner region F1 is greater than the area ratio of the cavities in the first middle region H1.

[0106] (2) The average crystal grain size of the ferrite in the first inner region F1 is smaller than the average crystal grain size of the ferrite in the first middle region H1.

[0107] In the coil component 1A, by satisfying both of the above features (1) and (2), the adhesion (e.g., bonding strength) between the first glass layer 15a and the first ferrite layer 16a is improved.

[0108] When the area ratio of the vacuoles in the first inner region F1 is set to 1, the area ratio of the vacuoles in the first intermediate region H1 is preferably 0.3 or more and 0.8 or less. In this case, the adhesion between the first glass layer 15a and the first ferrite layer 16a is significantly improved.

[0109] When the average crystal grain size of the ferrite in the first inner region F1 is set to 1, the average crystal grain size of the ferrite in the first intermediate region H1 is preferably 1.5 or more and 2.5 or less. In this case, the adhesion between the first glass layer 15a and the first ferrite layer 16a is significantly improved.

[0110] The area ratio of vacancies in the target region of the ferrite layer is determined as follows. First, after sealing the coil component with resin as needed, the coil component is ground along a first direction (e.g., width direction) orthogonal to the lamination direction (e.g., height direction), thereby exposing a cross-section along a second direction (e.g., length direction) orthogonal to both the lamination direction and the first direction at approximately the center of the first direction. At this time, for example, it can be made... Figure 2The cross-sections shown along the length and height directions can also be exposed along the width and height directions. Next, images of the exposed cross-sections were captured using a scanning electron microscope (SEM) at 5000x magnification with a field of view of 8 μm square. Then, the area ratio of voids in the target region of the ferrite layer was determined by image analysis software on the captured 8 μm square cross-sectional images. This void area ratio measurement was performed on cross-sectional images taken at five locations, and the average of the five measurements was determined as the void area ratio in the target region of the ferrite layer.

[0111] The average grain size of ferrite in the target region of the ferrite layer was determined as follows. First, by analyzing the 8μm square cross-sectional image used in determining the area ratio of holes using image analysis software, the area occupied by a single ferrite crystal particle in the target region of the ferrite layer was calculated, and the equivalent circle diameter was determined based on this area. Then, the equivalent circle diameter was measured for 20 ferrite crystal particles within the same cross-sectional image, and the average of the 20 measurements was determined as the average grain size of ferrite in the target region of the ferrite layer.

[0112] like Figure 2 As shown, in the coil component 1A, in the second ferrite layer 16b, the position of the main surface on the side of the first glass layer 15a is set as the fifth position E5, the position 10 μm away from the fifth position E5 in the stacking direction (here, the height direction T) is set as the sixth position E6, the position of the main surface on the opposite side of the first glass layer 15a is set as the seventh position E7, the position 10 μm away from the seventh position E7 in the stacking direction (here, the height direction T) is set as the eighth position E8, the area between the fifth position E5 and the sixth position E6 is set as the second inner area F2, the area between the seventh position E7 and the eighth position E8 is set as the second outer area G2, and the area between the sixth position E6 and the eighth position E8 is set as the second middle area H2. Preferably, the following features (3) and (4) are satisfied.

[0113] (3) The area ratio of the vacancy in the second inner region F2 is greater than that of the vacancy in the second middle region H2.

[0114] (4) The average crystal grain size of the ferrite in the second inner region F2 is smaller than that of the ferrite in the second middle region H2.

[0115] In the coil component 1A, by satisfying both of the above features (3) and (4), the adhesion (e.g., bonding strength) between the first glass layer 15a and the second ferrite layer 16b is improved.

[0116] When the area ratio of the vacuoles in the second inner region F2 is set to 1, the area ratio of the vacuoles in the second intermediate region H2 is preferably 0.3 or more and 0.8 or less. In this case, the adhesion between the first glass layer 15a and the second ferrite layer 16b is significantly improved.

[0117] When the average crystal grain size of the ferrite in the second inner region F2 is set to 1, the average crystal grain size of the ferrite in the second intermediate region H2 is preferably 1.5 or more and 2.5 or less. In this case, the adhesion between the first glass layer 15a and the second ferrite layer 16b is significantly improved.

[0118] The coil component 1A is manufactured, for example, by the following method.

[0119] <Processes for manufacturing glass-ceramic materials>

[0120] First, K2O, B2O3, SiO2, and Al2O3 are weighed to a specified ratio and mixed in a platinum crucible.

[0121] Next, the resulting mixture is heat-treated to melt it. The heat treatment temperature is, for example, above 1500°C and below 1600°C.

[0122] The resulting molten material is then rapidly cooled to produce glass.

[0123] The glass material preferably contains, when the total weight is set to 100 wt%, 0.5 wt% or more and 5 wt% K (equivalent to K2O), 10 wt% or more and 25 wt% B (equivalent to B2O3), 70 wt% or more and 85 wt% Si (equivalent to SiO2), and 0 wt% or more and 5 wt% Al (equivalent to Al2O3).

[0124] Next, glass powder is prepared by crushing the glass material. Regarding the median diameter D of the glass powder... 50 For example, the diameter can be 1 μm or larger, or 3 μm or smaller. Additionally, quartz powder and alumina powder are prepared as fillers. Regarding the median diameter D of the quartz powder and alumina powder... 50 For example, a diameter greater than 0.5 μm and less than 2.0 μm. Here, the median diameter D of glass powder, quartz powder, and alumina powder is... 50 It is the particle size when the cumulative probability of the volume reference is 50%.

[0125] Then, quartz powder and alumina powder are added as fillers to the glass powder to produce glass ceramic materials (dielectric glass materials: non-magnetic materials).

[0126] <Processes for making glass-ceramic sheets>

[0127] First, glass-ceramic materials, organic binders such as polyvinyl butyral resin, organic solvents such as ethanol and toluene, plasticizers, etc., are put into a ball mill and mixed together with PSZ media to produce glass-ceramic slurry.

[0128] Next, the glass-ceramic slurry is formed into a sheet of a specified thickness using a scraper method, and then punched into a specified shape to produce a glass-ceramic sheet. The thickness of the glass-ceramic sheet is, for example, 20 μm or more and 30 μm or less. The shape of the glass-ceramic sheet is, for example, rectangular.

[0129] <Process for manufacturing ferrite materials>

[0130] First, weigh Fe2O3, ZnO, CuO, and NiO to achieve the specified ratio. At this point, additives such as Mn3O4, Co3O4, SnO2, Bi2O3, and SiO2 can also be added.

[0131] Next, these weighed materials, pure water, dispersant, etc., are put into a ball mill along with the PSZ media and mixed before being pulverized.

[0132] Then, after drying the resulting pulverized material, it is pre-calcined. The pre-calcination temperature is, for example, above 700°C and below 800°C. The pre-calcination time is, for example, above 2 hours and below 3 hours.

[0133] In this way, powdered ferrite materials (magnetic materials) can be produced.

[0134] The ferrite material preferably contains, when the total weight is set to 100 mol%, 40 mol% or more and 49.5 mol% of Fe (calculated as Fe2O3), 5 mol% or more and 35 mol% of Zn (calculated as ZnO), 6 mol% or more and 12 mol% of Cu (calculated as CuO), and 8 mol% or more and 40 mol% of Ni (calculated as NiO).

[0135] In this process, by varying the degree of pulverization when obtaining the above-mentioned pulverized material, various ferrite materials with different specific surface areas (average particle sizes) are produced.

[0136] <Processes for manufacturing ferrite sheets>

[0137] First, powdered ferrite material, organic binders such as polyvinyl butyral resin, organic solvents such as ethanol and toluene, and PSZ media are put into a ball mill and mixed, and then pulverized to produce ferrite slurry.

[0138] Next, the ferrite slurry is formed into a sheet of a specified thickness using a scraper method, and then punched into a specified shape to produce a ferrite sheet. The shape of the ferrite sheet can be, for example, rectangular.

[0139] In this process, various ferrite sheets with different specific surface areas (average particle sizes) are produced by using various ferrite materials with different specific surface areas (average particle sizes). For example, a first ferrite sheet composed of a ferrite material with a relatively large specific surface area (relatively small average particle size) and a second ferrite sheet composed of a ferrite material with a relatively small specific surface area (relatively large average particle size) are produced.

[0140] <Process for forming conductor patterns>

[0141] By using methods such as screen printing, conductive pastes such as Ag paste are coated onto various glass-ceramic sheets to form a structure equivalent to... Figure 5 The coil conductor shown uses a conductor pattern, equivalent to... Figure 5 The lead-out conductor shown uses a conductor pattern, and is equivalent to... Figure 5 The conductive pattern for the through-hole conductor is shown. In forming the conductive pattern for the through-hole conductor, a through-hole is pre-formed by laser irradiation of a predetermined area on a glass-ceramic sheet, and then a conductive paste is filled into the through-hole.

[0142] <Process for fabricating laminated prefabricated components>

[0143] First, individual glass-ceramic sheets with conductor patterns are formed using... Figure 5 The order shown is Figure 5 The insulating layers 15aa, 15ab, 15ac, and 15ad are stacked in sequence along the stacking direction (here, the height direction). Then, as shown... Figure 5 As shown, on one principal plane of the resulting laminated body along the stacking direction (here, the height direction), i.e. Figure 5 The insulating layer 15ae shown is located where a glass-ceramic sheet without a conductor pattern is stacked.

[0144] Next, a predetermined number of ferrite sheets are stacked on the two main faces of the obtained glass-ceramic sheet laminate in the lamination direction (here, the height direction). For example, the first and second ferrite sheets are stacked sequentially from the glass-ceramic sheet laminate side, relative to the two main faces of the laminate. More specifically, in Figure 5 The first ferrite sheet is stacked at the positions of insulating layer 16aa and insulating layer 16ba shown. Figure 5 The second ferrite sheet is stacked at the positions of insulating layers 16ab and 16bb shown.

[0145] Then, the laminate of glass-ceramic sheets and ferrite sheets is pressed together by warm isostatic pressing (WIP) and other processes to produce a laminate preform.

[0146] <Processes for manufacturing the substrate and coil>

[0147] First, the laminated preform is cut into specified sizes using a cutting machine or similar equipment to create segmented chips.

[0148] Next, the segmented chips are calcined. The calcination temperature is, for example, above 860℃ and below 920℃. The calcination time is, for example, above 1 hour and below 2 hours.

[0149] The chip is calcined, thereby forming insulating layers from the glass-ceramic sheet and the ferrite sheet. As a result, the stacked portion of the glass-ceramic sheet becomes the first glass layer. Furthermore, the two stacked portions of the ferrite sheet, which hold the glass-ceramic sheet in the stacking direction (here, the height direction), become the first ferrite layer and the second ferrite layer, respectively. Additionally, the conductor patterns for the coil conductor, the lead conductor, and the via conductor become the coil conductor, the lead conductor, and the via conductor, respectively.

[0150] Thus, a substrate is fabricated having a structure in which a first glass layer is sandwiched between a first ferrite layer and a second ferrite layer in the stacking direction (here, the height direction), a first coil disposed inside the first glass layer, and a second coil disposed inside the first glass layer and insulated from the first coil. Here, a first lead conductor connected to one end of the first coil and a third lead conductor connected to one end of the second coil are exposed on a first side of the substrate. Furthermore, a second lead conductor connected to the other end of the first coil and a fourth lead conductor connected to the other end of the second coil are exposed on a second side of the substrate.

[0151] Here, in the above-mentioned <process of manufacturing laminated preform>, a first ferrite sheet and a second ferrite sheet are sequentially laminated from the laminated side of the glass-ceramic sheet. After calcination in this process, the thickness of the first ferrite sheet is adjusted so that the thickness of the first ferrite sheet is 10 μm and the thickness of the second ferrite sheet is greater than 10 μm. In the first ferrite layer obtained in this process, a first inner region from the first ferrite sheet, a first outer region from a portion of the second ferrite sheet, and a first middle region from the remaining portion of the second ferrite sheet are formed.

[0152] At this point, during the calcination of the segmented chips in this process, the ferrite material in the first ferrite sheet, which is in contact with the glass-ceramic sheet, has a relatively large specific surface area (relatively small average particle size). Therefore, the components of the glass-ceramic material easily diffuse from the glass-ceramic sheet to the first ferrite sheet. Consequently, the adhesion between the glass-ceramic sheet and the first ferrite sheet is improved through the diffusion of the glass-ceramic material. As a result, the adhesion between the first glass layer and the first ferrite layer obtained in this process is improved.

[0153] On the other hand, when the components of the glass-ceramic material readily diffuse from the glass-ceramic sheet to the first ferrite sheet, the sintering (crystallization) of the ferrite material is easily hindered within the first ferrite sheet. As a result, in the first ferrite layer obtained in this process, the average crystal grain size of the ferrite from the first inner region of the first ferrite sheet is smaller than the average crystal grain size of the ferrite from the first intermediate region of the second ferrite sheet. Furthermore, accompanying this, in the first ferrite layer obtained in this process, the area ratio of voids from the first inner region of the first ferrite sheet is greater than the area ratio of voids from the first intermediate region of the second ferrite sheet.

[0154] In the second ferrite layer obtained in this process, similarly to the first ferrite layer, a second inner region from the first ferrite sheet, a second outer region from a portion of the second ferrite sheet, and a second intermediate region from the remaining portion of the second ferrite sheet are formed.

[0155] At this point, based on the same principle as above, the adhesion between the first glass layer and the second ferrite layer obtained in this process is also improved.

[0156] On the other hand, based on the same principle as described above, in the second ferrite layer obtained in this process, the average crystal grain size of the ferrite from the second inner region of the first ferrite sheet is also smaller than the average crystal grain size of the ferrite from the second middle region of the second ferrite sheet. Furthermore, consequently, in the second ferrite layer obtained in this process, the area ratio of holes from the second inner region of the first ferrite sheet is greater than the area ratio of holes from the second middle region of the second ferrite sheet.

[0157] As described above, for example, by changing the degree of pulverization when obtaining the pulverized material in the above-mentioned <process of producing ferrite material>, and then changing the specific surface area (average particle size) of the ferrite material of the first ferrite sheet that becomes the inner region of the ferrite layer, it is possible to adjust the average crystal particle size of the ferrite in the inner region and the area ratio of the vacancies in the inner region for the ferrite layer obtained in this process.

[0158] For the substrate, for example, the substrate and the medium can be placed together in a rotary drum mill to perform drum grinding on the substrate, thereby giving the corners and edges rounded corners.

[0159] <Process for forming external electrodes>

[0160] First, a conductive paste containing Ag and glass frit is applied to at least four locations on the first side of the substrate where the first lead conductor is exposed, the second side of the substrate where the second lead conductor is exposed, the first side of the substrate where the third lead conductor is exposed, and the second side of the substrate where the fourth lead conductor is exposed.

[0161] Next, the obtained coatings are sintered to form a base electrode on the surface of the substrate.

[0162] Then, by means of electroplating, plating electrodes, such as Ni plating electrodes and Sn plating electrodes, are sequentially formed on the surface of each base electrode.

[0163] Thus, a first external electrode electrically connected to one end of the first coil via a first lead conductor, a second external electrode electrically connected to the other end of the first coil via a second lead conductor, a third external electrode electrically connected to one end of the second coil via a third lead conductor, and a fourth external electrode electrically connected to the other end of the second coil via a fourth lead conductor are formed on the surface of the substrate.

[0164] Thus, coil component 1A is manufactured.

[0165] [Implementation Method 2]

[0166] In the coil component of Embodiment 2 of the present invention, the substrate further includes a second glass layer adjacent to the first ferrite layer on the side opposite to the first glass layer, and a third glass layer adjacent to the second ferrite layer on the side opposite to the first glass layer. The coil component of Embodiment 2 of the present invention is identical to the coil component of Embodiment 1 of the present invention, except for this point.

[0167] Figure 6 This is a perspective schematic diagram showing an example of a coil component according to Embodiment 2 of the present invention.

[0168] exist Figure 6 In the coil component 1B shown, in addition to the structure of the substrate 10A, namely the first glass layer 15a, the first ferrite layer 16a and the second ferrite layer 16b, the substrate 10B also has a second glass layer 15b and a third glass layer 15c.

[0169] In the stacking direction (here, the height direction T), the second glass layer 15b is adjacent to the first ferrite layer 16a on the opposite side of the first glass layer 15a, and the third glass layer 15c is adjacent to the second ferrite layer 16b on the opposite side of the first glass layer 15a. That is, in the substrate 10B, in the stacking direction (here, the height direction T), the first ferrite layer 16a is sandwiched between the first glass layer 15a and the second glass layer 15b, and the second ferrite layer 16b is sandwiched between the first glass layer 15a and the third glass layer 15c.

[0170] The number of insulating layers constituting the second glass layer 15b is not particularly limited; it can be just one or more.

[0171] The second glass layer 15b is made of glass-ceramic material.

[0172] The second glass layer 15b preferably comprises a glass material containing K, B, and Si. That is, the glass-ceramic material constituting the second glass layer 15b preferably comprises a glass material containing K, B, and Si.

[0173] The glass material contained in the second glass layer 15b preferably contains, when the total weight is set to 100% by weight, 0.5% to 5% by weight of K (equivalent to K2O), 10% to 25% by weight of B (equivalent to B2O3), 70% to 85% by weight of Si (equivalent to SiO2), and 0% to 5% by weight of Al (equivalent to Al2O3).

[0174] The second glass layer 15b preferably includes a filler containing at least one of quartz and alumina. That is, the glass-ceramic material constituting the second glass layer 15b preferably includes a filler containing at least one of quartz and alumina. The inclusion of quartz as a filler in the glass-ceramic material constituting the second glass layer 15b easily improves the high-frequency characteristics of the coil component 1B. Furthermore, the inclusion of alumina as a filler in the glass-ceramic material constituting the second glass layer 15b easily improves the mechanical strength of the substrate 10B.

[0175] When the glass-ceramic material constituting the second glass layer 15b includes quartz and alumina as fillers, the glass-ceramic material preferably includes 60% to 66% glass material, 34% to 37% quartz as filler, and 0.5% to 4% alumina as filler when the total weight is set to 100% by weight.

[0176] The number of insulating layers constituting the third glass layer 15c is not particularly limited; it can be just one or more.

[0177] The third glass layer 15c is made of glass-ceramic material.

[0178] The third glass layer 15c preferably comprises a glass material containing K, B, and Si. That is, the glass-ceramic material constituting the third glass layer 15c preferably comprises a glass material containing K, B, and Si.

[0179] The glass material contained in the third glass layer 15c preferably contains, when the total weight is set to 100% by weight, 0.5% to 5% by weight of K (calculated as K2O), 10% to 25% by weight of B (calculated as B2O3), 70% to 85% by weight of Si (calculated as SiO2), and 0% to 5% by weight of Al (calculated as Al2O3).

[0180] The third glass layer 15c preferably includes a filler containing at least one of quartz and alumina. That is, the glass-ceramic material constituting the third glass layer 15c preferably includes a filler containing at least one of quartz and alumina. The inclusion of quartz as a filler in the glass-ceramic material constituting the third glass layer 15c easily improves the high-frequency characteristics of the coil component 1B. Furthermore, the inclusion of alumina as a filler in the glass-ceramic material constituting the third glass layer 15c easily improves the mechanical strength of the substrate 10B.

[0181] When the glass-ceramic material constituting the third glass layer 15c includes quartz and alumina as fillers, the glass-ceramic material preferably includes, when the total weight is set to 100% by weight: 60% or more and 66% or less glass material, 34% or more and 37% or less quartz as filler, and 0.5% or more and 4% or less alumina as filler.

[0182] The glass-ceramic materials constituting the first glass layer 15a, the second glass layer 15b, and the third glass layer 15c are preferably the same as each other, but they may also be different from each other or partially different.

[0183] The dimensions T along the height direction of the first glass layer 15a, the second glass layer 15b, the third glass layer 15c, the first ferrite layer 16a, and the second ferrite layer 16b can be the same, different, or partially different. When the dimensions T along the height direction of the first glass layer 15a, the second glass layer 15b, the third glass layer 15c, the first ferrite layer 16a, and the second ferrite layer 16b are different or partially different, their size relationship is not particularly limited.

[0184] Figure 7 It means Figure 6 A schematic cross-sectional view of an example of a section along line segment A3-A4 of the coil component shown.

[0185] like Figure 7 As shown, in coil component 1B, in the first ferrite layer 16a, when the position of the main surface on the side of the first glass layer 15a is designated as the first position E1, the position 10 μm away from the first position E1 in the stacking direction (here, the height direction T) is designated as the second position E2, the position of the main surface on the opposite side of the first glass layer 15a, i.e., the side of the second glass layer 15b, is designated as the third position E3, the position 10 μm away from the third position E3 in the stacking direction (here, the height direction T) is designated as the fourth position E4, the region between the first position E1 and the second position E2 is designated as the first inner region F1, the region between the third position E3 and the fourth position E4 is designated as the first outer region G1, and the region between the second position E2 and the fourth position E4 is designated as the first middle region H1, the features (1) and (2) above are satisfied in the same way as in coil component 1A. In addition, in coil component 1B, the following features (5) and (6) are preferably satisfied.

[0186] (5) The area ratio of the vacancy in the first outer region G1 is greater than that of the vacancy in the first middle region H1.

[0187] (6) The average crystal grain size of the ferrite in the first outer region G1 is smaller than the average crystal grain size of the ferrite in the first middle region H1.

[0188] In the coil component 1B, by satisfying both of the above features (5) and (6), the adhesion (e.g., bonding strength) between the second glass layer 15b and the first ferrite layer 16a is improved.

[0189] When the area ratio of the vacancy in the first outer region G1 is set to 1, the area ratio of the vacancy in the first middle region H1 is preferably 0.3 or higher and 0.8 or lower. In this case, the adhesion between the second glass layer 15b and the first ferrite layer 16a is significantly improved.

[0190] The area ratios of the cavities in the first inner region F1 and the first outer region G1 can be the same or different. When the area ratios of the cavities in the first inner region F1 and the first outer region G1 are different, their size relationship is not particularly limited.

[0191] When the average crystal grain size of the ferrite in the first outer region G1 is set to 1, the average crystal grain size of the ferrite in the first intermediate region H1 is preferably 1.5 or more and 2.5 or less. In this case, the adhesion between the second glass layer 15b and the first ferrite layer 16a is significantly improved.

[0192] The average crystal grain sizes of the ferrites in the first inner region F1 and the first outer region G1 can be the same or different. When the average crystal grain sizes of the ferrites in the first inner region F1 and the first outer region G1 are different, their size relationship is not particularly limited.

[0193] like Figure 7 As shown, in the coil component 1B, in the second ferrite layer 16b, when the position of the main surface on the side of the first glass layer 15a is set as the fifth position E5, the position 10 μm away from the fifth position E5 in the stacking direction (here, the height direction T) is set as the sixth position E6, the position of the main surface on the side opposite to the first glass layer 15a, i.e., the third glass layer 15c, is set as the seventh position E7, the position 10 μm away from the seventh position E7 in the stacking direction (here, the height direction T) is set as the eighth position E8, the area between the fifth position E5 and the sixth position E6 is set as the second inner area F2, the area between the seventh position E7 and the eighth position E8 is set as the second outer area G2, and the area between the sixth position E6 and the eighth position E8 is set as the second middle area H2, it is preferable to satisfy the following features (7) and (8).

[0194] (7) The area ratio of the vacancy in the second outer region G2 is greater than that of the vacancy in the second middle region H2.

[0195] (8) The average crystal grain size of the ferrite in the second outer region G2 is smaller than that of the average crystal grain size of the ferrite in the second middle region H2.

[0196] In the coil component 1B, by satisfying both of the above-mentioned features (7) and (8), the adhesion (e.g., bonding strength) between the third glass layer 15c and the second ferrite layer 16b is improved.

[0197] When the area ratio of holes in the second outer region G2 is set to 1, the area ratio of holes in the second middle region H2 is preferably 0.3 or higher and 0.8 or lower. In this case, the adhesion between the third glass layer 15c and the second ferrite layer 16b is significantly improved.

[0198] The area ratios of the cavities in the second inner region F2 and the second outer region G2 can be the same or different. When the area ratios of the cavities in the second inner region F2 and the second outer region G2 are different, their size relationship is not particularly limited.

[0199] When the average crystal grain size of the ferrite in the second outer region G2 is set to 1, the average crystal grain size of the ferrite in the second intermediate region H2 is preferably 1.5 or more and 2.5 or less. In this case, the adhesion between the third glass layer 15c and the second ferrite layer 16b is significantly improved.

[0200] The average crystal grain sizes of the ferrites in the second inner region F2 and the second outer region G2 can be the same or different. When the average crystal grain sizes of the ferrites in the second inner region F2 and the second outer region G2 are different, their size relationship is not particularly limited.

[0201] The coil component 1B is manufactured in the same manner as the coil component 1A, except that the process of manufacturing the laminated preform is performed as described below.

[0202] <Process for fabricating laminated prefabricated components>

[0203] First, individual glass-ceramic sheets with conductor patterns are formed using... Figure 5 The order shown is stacked along the stacking direction (here, the height direction). At this time, a predetermined number of glass-ceramic sheets without conductor patterns are stacked on at least one main surface of the resulting laminate along the stacking direction (here, the height direction).

[0204] Next, a predetermined number of ferrite sheets are stacked on the two main faces of the obtained glass-ceramic sheet stack in the stacking direction (here, the height direction). At this time, for example, the first ferrite sheet, the second ferrite sheet, and the first ferrite sheet are stacked sequentially from the glass-ceramic sheet stack side relative to the two main faces of the glass-ceramic sheet stack.

[0205] Next, a specified number of glass-ceramic sheets without conductor patterns are stacked along the stacking direction (here, the height direction) relative to the two stacked portions of the obtained ferrite sheet.

[0206] Then, the resulting laminate of glass-ceramic sheets and ferrite sheets is pressed together by a process such as warm isostatic pressing to produce a laminate preform.

[0207] Then, in the <Substrate and Coil Fabrication Process>, the wafer-sized chip is calcined, thereby forming the first glass layer from the inner layer of the glass-ceramic sheet. Additionally, the two ferrite sheet layers that hold the glass-ceramic sheet layer in the stacking direction (here, the height direction) become the first ferrite layer and the second ferrite layer, respectively. Furthermore, the two glass-ceramic sheet layers located on the outer sides of the two ferrite sheet layers become the second glass layer and the third glass layer, respectively.

[0208] Here, in the <process of fabricating the laminated preform>, a first ferrite sheet, a second ferrite sheet, and a third first ferrite sheet are sequentially laminated from the laminated side of the glass-ceramic sheet. After calcination in the <process of fabricating the substrate and coil>, the thickness of the two first ferrite sheets is adjusted to 10 μm. In the first ferrite layer obtained in the <process of fabricating the substrate and coil>, a first inner region from one of the first ferrite sheets, a first middle region from the second ferrite sheet, and a first outer region from the other first ferrite sheet are formed. Furthermore, in the second ferrite layer obtained in the <process of fabricating the substrate and coil>, a second inner region from one of the first ferrite sheets, a second middle region from the second ferrite sheet, and a second outer region from the other first ferrite sheet are formed.

[0209] At this point, in the <process of manufacturing the substrate and coil>, based on the same principle as above, the adhesion between the second glass layer and the first ferrite layer, as well as the adhesion between the third glass layer and the second ferrite layer, are also improved.

[0210] On the other hand, based on the same principle as described above, in the first ferrite layer obtained in the <process of fabricating the substrate and coil>, the average crystal grain size of the ferrite in the first outer region of the first ferrite sheet is smaller than the average crystal grain size of the ferrite in the first middle region of the second ferrite sheet. Furthermore, concurrently, in the first ferrite layer obtained in the <process of fabricating the substrate and coil>, the area ratio of voids in the first outer region of the first ferrite sheet is greater than the area ratio of voids in the first middle region of the second ferrite sheet.

[0211] Furthermore, based on the same principle as described above, in the second ferrite layer obtained in the <process of fabricating the substrate and coil>, the average crystal grain size of the ferrite in the second outer region of the first ferrite sheet is smaller than the average crystal grain size of the ferrite in the second middle region of the second ferrite sheet. Additionally, accompanyingly, in the second ferrite layer obtained in the <process of fabricating the substrate and coil>, the area ratio of voids in the second outer region of the first ferrite sheet is greater than the area ratio of voids in the second middle region of the second ferrite sheet.

[0212]

Example

[0213] The following describes specific embodiments of the coil component of the present invention. However, the present invention is not limited to these embodiments.

[0214] [Example 1]

[0215] As a coil component of Embodiment 1, the coil component of Embodiment 1 of the present invention is manufactured by the following method.

[0216] <Processes for manufacturing glass-ceramic materials>

[0217] First, K2O, B2O3, SiO2, and Al2O3 are weighed to a specified ratio and mixed in a platinum crucible.

[0218] Next, the resulting mixture is heat-treated to melt it. The heat treatment temperature is 1500°C.

[0219] The resulting molten material is then rapidly cooled to produce glass.

[0220] Next, glass powder is prepared by crushing the glass material. Regarding the median diameter D of the glass powder... 50 The diameter is between 1 μm and 3 μm. Additionally, quartz powder and alumina powder are prepared as fillers. Regarding the median diameter D of the quartz powder and alumina powder... 50 The size ranges from 0.5μm to 2.0μm.

[0221] Then, quartz powder and alumina powder are added as fillers to the glass powder to produce glass ceramic materials.

[0222] <Processes for making glass-ceramic sheets>

[0223] First, glass-ceramic materials, organic binders such as polyvinyl butyral resin, organic solvents such as ethanol and toluene, plasticizers, and PSZ media are put into a ball mill and mixed to produce a glass-ceramic slurry.

[0224] Next, the glass-ceramic slurry is formed into sheets using a scraper method, and then die-cut to produce glass-ceramic sheets. The thickness of the glass-ceramic sheets is between 20 μm and 30 μm. The shape of the glass-ceramic sheets is rectangular.

[0225] <Process for manufacturing ferrite materials>

[0226] First, weigh Fe2O3, ZnO, CuO, and NiO to make them into the specified ratio.

[0227] Next, these weighed materials, pure water, dispersant, and PSZ media were placed into a ball mill, mixed, and then pulverized.

[0228] Then, after drying the resulting pulverized material, it is pre-calcined. The pre-calcination temperature is 800℃, and the pre-calcination time is 2 hours.

[0229] This allows for the production of powdered ferrite materials.

[0230] In this process, by varying the degree of pulverization when obtaining the above-mentioned pulverized material, two ferrite materials with different specific surface areas (average particle size) are produced.

[0231] <Processes for manufacturing ferrite sheets>

[0232] First, powdered ferrite material, organic binders such as polyvinyl butyral resin, organic solvents such as ethanol and toluene, and PSZ media are put into a ball mill and mixed, and then pulverized to produce ferrite slurry.

[0233] Next, the ferrite slurry is formed into sheets using a scraper method, and then punched to produce ferrite sheets. The ferrite sheets are rectangular in shape.

[0234] In this process, two ferrite sheets with different specific surface areas (average particle sizes) are produced by using two ferrite materials with different specific surface areas (average particle sizes). More specifically, a first ferrite sheet composed of a ferrite material with a relatively large specific surface area (relatively small average particle size) and a second ferrite sheet composed of a ferrite material with a relatively small specific surface area (relatively large average particle size) are produced. The thickness of the first ferrite sheet is 10 μm after calcination in a subsequent process. The thickness of the second ferrite sheet is 20 μm after calcination in a subsequent process.

[0235] <Process for forming conductor patterns>

[0236] By using screen printing to coat Ag paste onto individual glass-ceramic sheets, a process equivalent to... Figure 5 The coil conductor shown uses a conductor pattern, equivalent to... Figure 5 The lead-out conductor shown uses a conductor pattern, and is equivalent to... Figure 5 The conductive pattern for the through-hole conductor is shown. In forming the conductive pattern for the through-hole conductor, a through-hole is pre-formed by laser irradiation of a specified area on a glass-ceramic sheet, and then Ag paste is filled into the through-hole.

[0237] <Process for fabricating laminated prefabricated components>

[0238] First, individual glass-ceramic sheets with conductor patterns are formed using... Figure 5 The order shown is Figure 5 The insulating layers 15aa, 15ab, 15ac, and 15ad are stacked in the order shown, along the stacking direction (here, the height direction). Then, as... Figure 5 As shown, on one principal plane of the resulting laminated body along the stacking direction (here, the height direction), i.e. Figure 5The insulating layer 15ae shown is located where a glass-ceramic sheet without a conductor pattern is stacked.

[0239] Next, with respect to the two principal faces of the resulting glass-ceramic sheet stack along the stacking direction (here, the height direction), the first ferrite sheet and the second ferrite sheet are sequentially stacked from the glass-ceramic sheet stack side. More specifically, in Figure 5 The first ferrite sheet is stacked at the positions of insulating layer 16aa and insulating layer 16ba shown. Figure 5 The second ferrite sheet is stacked at the positions of insulating layers 16ab and 16bb shown.

[0240] Then, the resulting laminate of glass-ceramic sheets and ferrite sheets is pressed together by warm isostatic pressing to produce a laminate preform. The pressing conditions are 80°C and 100 MPa.

[0241] <Processes for manufacturing the substrate and coil>

[0242] First, the laminated preform is cut into specified sizes using a cutting machine to create segmented chips.

[0243] Next, the segmented chips are calcined. The calcination temperature is 910℃, and the calcination time is 2 hours.

[0244] The chip is calcined, thereby forming insulating layers from the glass-ceramic sheet and the ferrite sheet. As a result, the stacked portion of the glass-ceramic sheet becomes the first glass layer. Furthermore, the two stacked portions of the ferrite sheet, which hold the glass-ceramic sheet in the stacking direction (here, the height direction), become the first ferrite layer and the second ferrite layer, respectively. Additionally, the conductor patterns for the coil conductor, the lead conductor, and the via conductor become the coil conductor, the lead conductor, and the via conductor, respectively.

[0245] Thus, a substrate is fabricated having a structure in which a first glass layer is sandwiched between a first ferrite layer and a second ferrite layer in the stacking direction (here, the height direction), a first coil disposed inside the first glass layer, and a second coil disposed inside the first glass layer and insulated from the first coil. Here, a first lead conductor connected to one end of the first coil and a third lead conductor connected to one end of the second coil are exposed on a first side of the substrate. Furthermore, a second lead conductor connected to the other end of the first coil and a fourth lead conductor connected to the other end of the second coil are exposed on a second side of the substrate.

[0246] In the first ferrite layer obtained in this process, a first inner region from the first ferrite sheet, a first outer region from a portion of the second ferrite sheet, and a first intermediate region from the remaining portion of the second ferrite sheet are formed.

[0247] In addition, the second ferrite layer obtained in this process has a second inner region from the first ferrite sheet, a second outer region from a portion of the second ferrite sheet, and a second middle region from the remaining portion of the second ferrite sheet.

[0248] Then, the substrate and the medium are placed together in a rotary drum mill to perform drum grinding on the substrate, thereby giving the corners and edges rounded corners.

[0249] <Process for forming external electrodes>

[0250] First, a conductive paste containing Ag and glass frit is applied to at least four locations on the first side of the substrate where a first lead conductor is exposed, a second lead conductor is exposed on the second side of the substrate, a third lead conductor is exposed on the first side of the substrate, and a fourth lead conductor is exposed on the second side of the substrate.

[0251] Next, the obtained coatings are sintered to form a base electrode on the surface of the substrate. The sintering temperature for each coating is 800°C.

[0252] Then, Ni-plated electrodes and Sn-plated electrodes are sequentially formed on the surface of each base electrode by electroplating.

[0253] Thus, a first external electrode electrically connected to one end of the first coil via a first lead conductor, a second external electrode electrically connected to the other end of the first coil via a second lead conductor, a third external electrode electrically connected to one end of the second coil via a third lead conductor, and a fourth external electrode electrically connected to the other end of the second coil via a fourth lead conductor are formed on the surface of the substrate.

[0254] Thus, the coil component of Embodiment 1 is manufactured.

[0255] The coil component of Example 1 has a length dimension of 0.65 mm, a height dimension of 0.30 mm, and a width dimension of 0.50 mm.

[0256] [Comparative Example 1]

[0257] In addition to the process of fabricating laminated prefabricated components, Figure 5 Except for all locations where the second ferrite sheet is laminated in the insulating layers 16aa, 16ab, 16ba, and 16bb shown, the coil component of Comparative Example 1 is manufactured in the same manner as the coil component of Example 1.

[0258] [evaluate]

[0259] For each of the coil component of Example 1 and the coil component of Comparative Example 1, as described above, after determining the first inner region, the first outer region, and the first intermediate region in the first ferrite layer, and after determining the second inner region, the second outer region, and the second intermediate region in the second ferrite layer, the following evaluation was performed. The results are shown in Tables 1 and 2.

[0260] <Area ratio of holes in ferrite layers>

[0261] First, after sealing the coil component with resin as needed, the coil component is ground along its width, thereby exposing a cross-section along its length and height at approximately the center of the width. Next, an image of the exposed cross-section is captured using a scanning electron microscope at 5000x magnification with a field of view of 8μm square. Then, the area ratio of holes in the target region of the ferrite layer is determined by image analysis software on the captured 8μm square cross-sectional image. More specifically, after binarizing the captured 8μm square cross-sectional image using the image analysis software "GIMP", the area ratio of holes in the target region of the ferrite layer (the proportion of pixels in the entire area where holes exist to the total number of pixels in the entire target region of the ferrite layer) is measured using "A-Image-kun" (registered trademark) manufactured by Asahi Kasei Engineering Co., Ltd. This measurement of the area ratio of holes is performed on cross-sectional images captured at five locations, and the average of the five measurements is determined as the area ratio of holes in the target region of the ferrite layer.

[0262] In addition, Tables 1 and 2 show, in addition to the measured values ​​of the area ratio of vacancies in the target region of each ferrite layer, the ratio of the area ratio of vacancies in the target region when the area ratio of vacancies in the inner region is set to 1 for the same ferrite layer.

[0263] <Average crystal grain size of ferrite in the ferrite layer>

[0264] First, the image analysis software "A-Image-kun" manufactured by Asahi Kasei Engineering Co., Ltd. was used to analyze the 8μm square cross-sectional image used in determining the area ratio of holes. This allowed the determination of the area occupied by a single ferrite crystal particle in the target region of the ferrite layer, and the equivalent circle diameter was then calculated based on this area. Next, the equivalent circle diameter was measured for 20 ferrite crystal particles within the same cross-sectional image. The average of these 20 measurements was determined as the average ferrite grain size in the target region of the ferrite layer.

[0265] In addition, Tables 1 and 2 show, in addition to the measured values ​​of the average crystal grain size of ferrite in the target region of each ferrite layer, the ratio of the average crystal grain size of ferrite in the target region when the average crystal grain size of ferrite in the inner region is set to 1 for the same ferrite layer.

[0266] <Adhesion between the glass layer and the ferrite layer>

[0267] In the coil component, the interface between the first glass layer and the first ferrite layer, as well as the vicinity of the interface between the first glass layer and the second ferrite layer, are observed using a microscope, and the adhesion between the glass layer and the ferrite layer is evaluated according to the following criteria.

[0268] ○ (Good): No gaps were found between the glass layer and the ferrite layer.

[0269] × (Defect): A gap was found between the glass layer and the ferrite layer.

[0270] Table 1

[0271]

[0272] Table 2

[0273]

[0274] As shown in Table 1, in the coil component of Embodiment 1, where the area ratio of holes in the first inner region is greater than that in the first middle region, and the average crystal grain size of the ferrite in the first inner region is smaller than that in the first middle region, the adhesion between the first glass layer and the first ferrite layer is good. Furthermore, in the coil component of Embodiment 1, where the area ratio of holes in the second inner region is greater than that in the second middle region, and the average crystal grain size of the ferrite in the second inner region is smaller than that in the second middle region, the adhesion between the first glass layer and the second ferrite layer is also good.

[0275] On the other hand, as shown in Table 2, in the coil component of Comparative Example 1, where the area ratio of holes in the first inner region is less than that in the first intermediate region, and the average crystal grain size of the ferrite in the first inner region is greater than that in the first intermediate region, the adhesion between the first glass layer and the first ferrite layer is insufficient. Furthermore, in the coil component of Comparative Example 1, where the area ratio of holes in the second inner region is less than that in the second intermediate region, and the average crystal grain size of the ferrite in the second inner region is greater than that in the second intermediate region, the adhesion between the first glass layer and the second ferrite layer is also insufficient.

[0276] The following information is disclosed in this specification.

[0277] <1> A coil component, characterized in that it comprises:

[0278] The substrate has a first glass layer, a first ferrite layer adjacent to one main surface of the first glass layer, and a second ferrite layer adjacent to the other main surface of the first glass layer in the stacking direction.

[0279] The coil is disposed inside the first glass layer; and

[0280] An external electrode is disposed on the surface of the substrate and is electrically connected to the coil.

[0281] In the first ferrite layer, the position of the main surface on the side of the first glass layer is designated as the first position; the position 10 μm away from the first position in the stacking direction is designated as the second position; the position of the main surface on the opposite side of the first glass layer is designated as the third position; the position 10 μm away from the third position in the stacking direction is designated as the fourth position; the region between the first and second positions is designated as the first inner region; the region between the third and fourth positions is designated as the first outer region; and the region between the second and fourth positions is designated as the first middle region.

[0282] The area ratio of cavities in the first inner region is greater than that in the first middle region.

[0283] The average crystal grain size of the ferrite in the first inner region is smaller than the average crystal grain size of the ferrite in the first middle region.

[0284] <2> Based on the coil components described in <1>,

[0285] When the area ratio of the cavities in the first inner region is set to 1, the area ratio of the cavities in the first middle region is 0.3 or more and 0.8 or less.

[0286] <3> According to the coil components described in <1> or <2>,

[0287] When the average crystal grain size of the ferrite in the first inner region is set to 1, the average crystal grain size of the ferrite in the first intermediate region is 1.5 or more and 2.5 or less.

[0288] <4> Based on any one of the coil components described in <1> to <3>,

[0289] In the second ferrite layer, the position of the main surface on the side of the first glass layer is designated as the fifth position, the position 10 μm away from the fifth position in the stacking direction is designated as the sixth position, the position of the main surface on the opposite side of the first glass layer is designated as the seventh position, the position 10 μm away from the seventh position in the stacking direction is designated as the eighth position, the region between the fifth and sixth positions is designated as the second inner region, the region between the seventh and eighth positions is designated as the second outer region, and the region between the sixth and eighth positions is designated as the second middle region.

[0290] The area ratio of cavities in the second inner region is greater than that in the second middle region.

[0291] The average crystal grain size of the ferrite in the second inner region is smaller than the average crystal grain size of the ferrite in the second middle region.

[0292] <5> Based on the coil components described in <4>,

[0293] When the area ratio of the cavities in the second inner region is set to 1, the area ratio of the cavities in the second middle region is 0.3 or more and 0.8 or less.

[0294] <6> According to the coil components described in <4> or <5>,

[0295] When the average crystal grain size of the ferrite in the second inner region is set to 1, the average crystal grain size of the ferrite in the second intermediate region is 1.5 or more and 2.5 or less.

[0296] <7> Based on any one of the coil components described in <1> to <6>,

[0297] The first glass layer mentioned above includes a filler containing at least one of quartz and alumina.

[0298] <8> Based on any one of the coil components described in <1> to <7>,

[0299] The substrate further comprises: a second glass layer adjacent to the first ferrite layer on the opposite side of the first glass layer; and a third glass layer adjacent to the second ferrite layer on the opposite side of the first glass layer.

[0300] <9> According to the coil components described in <8>,

[0301] The area ratio of cavities in the first outer region is greater than that in the first middle region.

[0302] The average crystal grain size of the ferrite in the first outer region is smaller than the average crystal grain size of the ferrite in the first middle region.

[0303] <10> According to the coil components described in <9>,

[0304] When the area ratio of the cavities in the first outer region is set to 1, the area ratio of the cavities in the first middle region is 0.3 or more and 0.8 or less.

[0305] <11> According to the coil components described in <9> or <10>,

[0306] When the average crystal grain size of the ferrite in the first outer region is set to 1, the average crystal grain size of the ferrite in the first middle region is 1.5 or more and 2.5 or less.

[0307] <12> Based on any one of the coil components described in <8> to <11>,

[0308] In the second ferrite layer, the position of the main surface on the side of the first glass layer is designated as the fifth position, the position 10 μm away from the fifth position in the stacking direction is designated as the sixth position, the position of the main surface on the opposite side of the first glass layer is designated as the seventh position, the position 10 μm away from the seventh position in the stacking direction is designated as the eighth position, the region between the fifth and sixth positions is designated as the second inner region, the region between the seventh and eighth positions is designated as the second outer region, and the region between the sixth and eighth positions is designated as the second middle region.

[0309] The area ratio of cavities in the second outer region is greater than that in the second middle region.

[0310] The average crystal grain size of the ferrite in the second outer region is smaller than the average crystal grain size of the ferrite in the second middle region.

[0311] <13> Based on the coil components described in <12>,

[0312] When the area ratio of the cavities in the second outer region is set to 1, the area ratio of the cavities in the second middle region is 0.3 or more and 0.8 or less.

[0313] <14> According to the coil components described in <12> or <13>,

[0314] When the average crystal grain size of the ferrite in the second outer region is set to 1, the average crystal grain size of the ferrite in the second middle region is 1.5 or more and 2.5 or less.

[0315] <15> Based on any one of the coil components described in <8> to <14>,

[0316] The second glass layer mentioned above contains a filler containing at least one of quartz and alumina.

[0317] <16> Based on any one of the coil components described in <8> to <15>,

[0318] The aforementioned third glass layer contains a filler comprising at least one of quartz and alumina.

[0319] <17> Based on any one of the coil components described in <1> to <16>,

[0320] The aforementioned coil component is a common-mode choke coil that is provided with a first coil and a second coil that is insulated from the first coil.

Claims

1. A coil component, characterized in that, have: The substrate has a first glass layer, a first ferrite layer adjacent to one main surface of the first glass layer, and a second ferrite layer adjacent to the other main surface of the first glass layer in the stacking direction. The coil is disposed inside the first glass layer; as well as An external electrode is disposed on the surface of the substrate and is electrically connected to the coil. In the first ferrite layer, the position of the main surface on the side of the first glass layer is designated as the first position; the position 10 μm away from the first position in the stacking direction is designated as the second position; the position of the main surface on the opposite side of the first glass layer is designated as the third position; the position 10 μm away from the third position in the stacking direction is designated as the fourth position; the region between the first position and the second position is designated as the first inner region; the region between the third position and the fourth position is designated as the first outer region; and the region between the second position and the fourth position is designated as the first middle region. The area ratio of cavities in the first inner region is greater than that in the first middle region. The average crystal grain size of the ferrite in the first inner region is smaller than the average crystal grain size of the ferrite in the first middle region.

2. The coil component according to claim 1, characterized in that, When the area ratio of the cavities in the first inner region is set to 1, the area ratio of the cavities in the first middle region is 0.3 or higher and 0.8 or lower.

3. The coil component according to claim 1, characterized in that, When the average crystal grain size of the ferrite in the first inner region is set to 1, the average crystal grain size of the ferrite in the first middle region is 1.5 or more and 2.5 or less.

4. The coil component according to claim 1, characterized in that, In the second ferrite layer, the position of the main surface on the side of the first glass layer is designated as the fifth position, the position 10 μm away from the fifth position in the stacking direction is designated as the sixth position, the position of the main surface on the opposite side of the first glass layer is designated as the seventh position, the position 10 μm away from the seventh position in the stacking direction is designated as the eighth position, the region between the fifth and sixth positions is designated as the second inner region, the region between the seventh and eighth positions is designated as the second outer region, and the region between the sixth and eighth positions is designated as the second middle region. The area ratio of cavities in the second inner region is greater than that in the second middle region. The average crystal grain size of the ferrite in the second inner region is smaller than that of the ferrite in the second middle region.

5. The coil component according to claim 4, characterized in that, When the area ratio of the cavities in the second inner region is set to 1, the area ratio of the cavities in the second middle region is 0.3 or higher and 0.8 or lower.

6. The coil component according to claim 4, characterized in that, When the average crystal grain size of the ferrite in the second inner region is set to 1, the average crystal grain size of the ferrite in the second middle region is 1.5 or more and 2.5 or less.

7. The coil component according to claim 1, characterized in that, The first glass layer contains a filler comprising at least one of quartz and alumina.

8. The coil component according to claim 1, characterized in that, The substrate further comprises: a second glass layer adjacent to the first ferrite layer on the opposite side from the first glass layer; and a third glass layer adjacent to the second ferrite layer on the opposite side from the first glass layer.

9. The coil component according to claim 8, characterized in that, The area ratio of holes in the first outer region is greater than that in the first middle region. The average crystal grain size of the ferrite in the first outer region is smaller than the average crystal grain size of the ferrite in the first middle region.

10. The coil component according to claim 9, characterized in that, When the area ratio of the cavities in the first outer region is set to 1, the area ratio of the cavities in the first middle region is 0.3 or higher and 0.8 or lower.

11. The coil component according to claim 9, characterized in that, When the average crystal grain size of the ferrite in the first outer region is set to 1, the average crystal grain size of the ferrite in the first middle region is 1.5 or more and 2.5 or less.

12. The coil component according to claim 8, characterized in that, In the second ferrite layer, the position of the main surface on the side of the first glass layer is designated as the fifth position, the position 10 μm away from the fifth position in the stacking direction is designated as the sixth position, the position of the main surface on the opposite side of the first glass layer is designated as the seventh position, the position 10 μm away from the seventh position in the stacking direction is designated as the eighth position, the region between the fifth and sixth positions is designated as the second inner region, the region between the seventh and eighth positions is designated as the second outer region, and the region between the sixth and eighth positions is designated as the second middle region. The area ratio of cavities in the second outer region is greater than that in the second middle region. The average crystal grain size of the ferrite in the second outer region is smaller than that of the ferrite in the second middle region.

13. The coil component according to claim 12, characterized in that, When the area ratio of the cavities in the second outer region is set to 1, the area ratio of the cavities in the second middle region is 0.3 or higher and 0.8 or lower.

14. The coil component according to claim 12, characterized in that, When the average crystal grain size of the ferrite in the second outer region is set to 1, the average crystal grain size of the ferrite in the second middle region is 1.5 or more and 2.5 or less.

15. The coil component according to claim 8, characterized in that, The second glass layer contains a filler comprising at least one of quartz and alumina.

16. The coil component according to claim 8, characterized in that, The third glass layer comprises a filler containing at least one of quartz and alumina.

17. The coil component according to any one of claims 1 to 16, characterized in that, The coil component is a common-mode choke coil consisting of a first coil and a second coil insulated from the first coil.

Citation Information

Patent Citations

  • Multilayer coil component

    JP2019102507A

  • Laminated coil component and method for manufacturing said laminated coil component

    CN103608876A

  • Ferrite composition and electronic device

    CN107879736A