Method for manufacturing glass article, glass article, cover glass, and display device
By setting parallel virtual lines on the glass plate and forming modified sections, the problem of high stress when cutting the glass plate was solved, enabling the manufacture of higher quality glass items.
Patent Information
- Application Number
- CN202280040916.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-06-11
- Filing Date
- 2022-06-02
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-06-02
AI Technical Summary
Existing technology requires high stress when cutting glass sheets, which can easily produce unwanted notches or cracks, leading to a decrease in the quality of glass products.
Multiple parallel virtual lines are set on the main surface of the glass plate. Lasers are irradiated along these virtual lines to form modified parts, and stress is applied to cut the glass plate. The interval between adjacent virtual lines is more than 2.0 μm and less than 30 μm.
It reduces the stress required to cut the glass sheet, decreases the occurrence of notches and cracks, and improves the quality of glass products.
Smart Images

Figure CN117480132B_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to a method for manufacturing glass articles, glass articles, glass covers, and display devices. Background Technology
[0002] Patent document 1 discloses a technique for forming a modified portion inside a glass plate by irradiating it with a laser. This allows the glass plate to be cut starting from the modified portion.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 2013-536081 Summary of the Invention
[0006] In the past, the stress required to cut glass sheets was high, sometimes resulting in unwanted notches or cracks. As a result, the quality of glass items was sometimes reduced.
[0007] One aspect of this disclosure provides a technique for reducing the stress required to cut a glass plate and improving the quality of glass articles.
[0008] One method of manufacturing a glass article according to the present disclosure has the following (A) to (C).
[0009] (A) Set multiple virtual lines that are parallel to each other on the main surface of the glass plate.
[0010] (B) Irradiate the multiple virtual lines with laser light to form modified sections on the glass plate along the multiple virtual lines.
[0011] (C) Apply stress to the glass plate and cut the glass plate along the virtual line.
[0012] The spacing between adjacent virtual lines is greater than 2.0 μm and less than 30 μm.
[0013] According to one aspect of this disclosure, multiple parallel virtual lines are set at intervals of 2.0 μm or more and less than 30 μm, and modified sections are formed along these virtual lines. This reduces the stress required to cut the glass plate and improves the quality of the glass articles. Attached Figure Description
[0014] Figure 1 This is a flowchart illustrating a method for manufacturing a glass article according to one embodiment of the present invention.
[0015] Figure 2 It is shown Figure 1 A stereoscopic view of an example of S1.
[0016] Figure 3 It is shown Figure 1 A stereoscopic view of an example of S2.
[0017] Figure 4 It is shown Figure 1 A stereoscopic view of an example of S3 midway.
[0018] Figure 5 It is shown Figure 1 A top view of an example at the end of S3.
[0019] Figure 6 It is shown Figure 1 A top view of an example of S5.
[0020] Figure 7 It is shown Figure 1 A three-dimensional diagram of an example of a glass object obtained in S5.
[0021] Figure 8 It is shown Figure 4 A three-dimensional diagram of a modified example.
[0022] Figure 9 This is a top view showing an example of a virtual line containing a curved section.
[0023] Figure 10 (A) is a side view showing an example of a four-point bending test. Figure 10 (B) is a top view showing an example of a test piece.
[0024] Figure 11 This is a graph showing the test results in Table 1.
[0025] Figure 12 This is a graph showing the test results in Table 2.
[0026] Figure 13 (A) is a microscope photograph showing the test piece of Example 12. Figure 13 (B) is a microscope photograph showing the test piece of Example 13. Figure 13 (C) is a microscope photograph showing the test piece of Example 14. Figure 13 (D) is a microscope photograph showing the test piece of Example 15. Figure 13 (E) is a microscope photograph showing the test piece of Example 16. Figure 13 (F) is a microscope photograph of the test piece shown in Example 17.
[0027] Figure 14 This is a graph showing the test results in Table 3.
[0028] Figure 15 (A) is a microscope photograph showing the test piece of Example 19. Figure 15 (B) is a microscope photograph showing the test piece of Example 20. Figure 15 (C) is a microscope photograph showing the test piece of Example 21. Figure 15 (D) is a microscope photograph showing the test piece of Example 22. Figure 15 (E) is a microscope photograph showing the test piece of Example 23. Figure 15 (F) is a microscope photograph of the test piece shown in Example 24.
[0029] Figure 16 This is a graph showing the test results in Table 4.
[0030] Figure 17 Photo (A) is a photograph taken under a microscope showing the cross-section of the test piece in Example 1 illuminated from the side. Figure 17 (B) is a photograph taken from above using a microscope, showing the cross-section of the test piece in Example 6 illuminated from the side.
[0031] Figure 18 This is a cross-sectional view showing an example of a modified section with virtual lines formed in the center and a modified section with virtual lines formed around the center. Detailed Implementation
[0032] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. It should be noted that symbols that are identical or corresponding in the drawings are sometimes omitted from the description. In the specification, the tilde “~” indicating a numerical range refers to the inclusion of the values described before and after it as a lower limit and an upper limit.
[0033] The method for manufacturing a glass article according to this embodiment is characterized by: setting multiple parallel virtual lines on the main surface of a glass plate; irradiating each of the multiple virtual lines with a laser to form modified portions in the glass plate along the multiple virtual lines; and applying stress to the glass plate to cut the glass plate along the virtual lines, wherein the interval between adjacent virtual lines is 2.0 μm or more and less than 30 μm.
[0034] First, refer to Figures 1 to 7 The method for manufacturing the glass article according to this embodiment will be described. The method for manufacturing the glass article is, for example, as follows: Figure 1 The method shown includes steps S1 to S5. It should be noted that the manufacturing method of glass articles only needs to include steps S1 to S3 and S5, and step S4 may be omitted.
[0035] In step S1, glass plate 10 is prepared. Glass plate 10 can be, for example, as shown in... Figure 2The glass plate shown is a flat plate, but it can also be a curved plate. It should be noted that when the glass plate 10 is a flat plate, it can also be bent into shape after step S5. The glass plate 10 has a first main surface 11 and a second main surface 12 facing opposite to the first main surface 11.
[0036] The shapes of the first main face 11 and the second main face 12 are, for example, rectangles. It should be noted that the shapes of the first main face 11 and the second main face 12 can be trapezoidal, circular, or elliptical, etc., but there are no particular limitations.
[0037] The glass plate 10 is used, for example, as automotive window glass, architectural window glass, substrate for display devices, or cover glass for display devices. The thickness of the glass plate 10 is appropriately set according to its application, for example, from 0.01 cm to 2.5 cm. When the glass plate 10 is used as a cover glass for an automotive display device, the thickness of the glass plate 10 is preferably 0.2 mm or more, more preferably 0.8 mm or more, and even more preferably 1 mm or more. When the glass plate 10 is used as a cover glass for an automotive display device, the thickness of the glass plate 10 is, for example, 5 mm or less, preferably 3 mm or less, and more preferably 2 mm or less.
[0038] Glass plate 10 can be laminated with other glass plates through an interlayer film after step S5, and used as laminated glass. Alternatively, glass plate 10 can be subjected to a strengthening process after step S5, and used as tempered glass.
[0039] Glass plate 10 may be, for example, soda-lime glass, alkali-free glass, or chemically strengthened glass. Chemically strengthened glass, after chemical strengthening treatment, may be used, for example, as a cover glass. Glass plate 10 may also be air-cooled strengthened glass.
[0040] In step S2, as Figure 3 As shown, multiple parallel virtual lines VL are set on the first main surface 11 of the glass plate 10. The setting of each virtual line VL is performed using a laser processing device. Each virtual line VL separates the first main surface 11 into two regions. Each virtual line VL can be configured as follows: Figure 3 The diagram shows only the straight section, but it can also be like... Figure 9 The diagram shows a straight section and a curved section, or it may only have a curved section.
[0041] Multiple virtual lines VL can be used as follows Figure 3 The glass plates are arranged with equal spacing, but they can also be arranged with unequal spacing; equal spacing is preferred. The interval d between adjacent virtual lines VL is 2.0 μm or more and less than 30 μm. If d is 2.0 μm or more and less than 30 μm, as described in the section on the embodiment, the stress required to cut the glass plate 10 can be reduced. Therefore, the generation of undesirable notches or cracks can be suppressed, and the quality of glass articles can be improved.
[0042] When the virtual line VL has a curved portion with a radius of curvature of 200 mm or less, the quality of the glass article can be significantly improved. Even if the radius of curvature of the curved portion is 200 mm or less, as long as the stress required to cut the glass plate 10 is low, the direction of crack propagation can easily change along the virtual line VL. The radius of curvature of the curved portion is preferably 50 mm or less. In addition, the radius of curvature of the curved portion is preferably 1 mm or more.
[0043] The spacing d between adjacent virtual lines VL is preferably 29 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, particularly preferably less than 20 μm, and extremely preferably 18 μm or less. The spacing d between adjacent virtual lines VL is preferably 2.5 μm or more, more preferably more than 3.5 μm, and even more preferably 7.0 μm or more.
[0044] The number n of virtual lines VL can be an even number of 2 or more, or an odd number of 3 or more, preferably an odd number of 3 or more. If n is an odd number of 3 or more, then there is one virtual line VL in the center of the multiple virtual lines VL. Therefore, as explained in the embodiment section, when cutting the glass plate 10 in step S5, the glass plate 10 can be cut at the central virtual line VL. In short, if n is an odd number of 3 or more, the cutting position can be determined.
[0045] When the number of virtual lines VL, n, is an odd number of 3 or more, it can also be as follows: Figure 3 The remaining virtual lines VL are arranged symmetrically with a virtual line VL sandwiched in the center. With this arrangement, it is easy to apply high stress to the central virtual line VL, and it is easy to cut the glass plate 10 at the central virtual line VL.
[0046] Multiple virtual lines (VL) can also be used as follows: Figure 3 The virtual lines VL are arranged at equal intervals as shown. It should be noted that when the number of virtual lines VL, n, is an odd number of 5 or more, the remaining virtual lines VL can also be arranged at unequal intervals, as long as they are arranged symmetrically with one virtual line VL as the center.
[0047] The more virtual lines VL there are, the more modified parts 13 are formed in step S3. From the viewpoint of reducing the number of modified parts 13, it is preferable that the number of virtual lines VL, n, is 3 or 5.
[0048] In step S3, as Figure 4 As shown, multiple virtual lines VL are irradiated with lasers LB, and modified sections 13 are formed on the glass plate 10 along the multiple virtual lines VL. Multiple virtual lines VL can be irradiated with multiple lasers LB simultaneously, or multiple virtual lines VL can be irradiated with one laser LB sequentially. The modified sections 13 are formed by laser LB, for example, through nonlinear absorption.
[0049] Nonlinear absorption is also known as multiphoton absorption. The probability of multiphoton absorption is nonlinear with respect to photon density (power density of laser LB); the higher the photon density, the higher the probability. For example, the probability of two-photon absorption is proportional to the square of the photon density.
[0050] The laser LB is, for example, pulsed light. Pulsed light preferably uses a wavelength range of 250 nm to 3000 nm and a pulse width of 10 fs to 1000 ns. Since lasers with a wavelength range of 250 nm to 3000 nm can pass through the glass plate 10 to some extent, nonlinear absorption can be generated inside the glass plate 10 to form the modified portion 13. The wavelength range is preferably 260 nm to 2500 nm. Furthermore, if a pulsed laser with a pulse width of 1000 ns or less is used, it is easier to increase the photon density, and nonlinear absorption can be generated inside the glass plate 10 to form the modified portion 13. The pulse width is preferably 100 fs to 100 ns.
[0051] The modified portion 13 is, for example, a portion of the glass whose density or refractive index has changed. The modified portion is a layer whose density or refractive index has changed through structural alteration or through melting and resolidification. The modified portion 13 may contain voids.
[0052] Laser LB is, for example, focused into a linear shape inside glass plate 10 to form the modified section 13. The light source of the laser LB can output a pulse group called a burst. A pulse group has multiple (e.g., 3 to 50) pulses, each with a pulse width of less than 10 nanoseconds. Within a pulse group, the energy of the pulses can be gradually reduced.
[0053] Pulsed light can also be focused into a line using self-focusing based on the nonlinear Kerr effect. Furthermore, pulsed light can also be focused into a line using an optical system. Specific optical systems include, for example, those using axicon lenses, those using birefringent materials, those using diffractive optical elements, or those utilizing optical aberrations.
[0054] Modification section 13, for example, Figure 4 As shown, it is formed throughout the thickness direction from the first main surface 11 to the second main surface 12. It should be noted that the modified part 13 may also be formed only in a part of the thickness direction, for example, it may be formed only on the side of the first main surface 11 from the center of the thickness.
[0055] When the number of virtual lines VL, n, is 3, for example, when n is 3... Figure 18 As an example, preferably at at least one central virtual line VL-2, the glass plate 10 is continuously or intermittently arranged within a range of 50% to 100% of its thickness. Figure 18The modified portion 13 is formed continuously in the middle. If the range of the modified portion 13 is within the range described above, it is easier to reduce the stress required for cutting. At the central virtual line VL-2, the range of the modified portion 13 formed is more preferably 75% to 100% of the thickness of the glass plate 10, and more preferably 100% of the thickness of the glass plate 10. In addition, as Figure 18 As shown, it is preferable to form the modified portion 13 starting from the first main surface 11. In this case, in the plate thickness direction, the second main surface 12 is set to 0%, and the first main surface 11 is set to 100%, and it is preferable to form the modified portion within the range described above.
[0056] On the other hand, when the number of virtual lines VL, n, is 3 or more, the virtual lines VL-1 and VL-3 around the center are preferably continuous or discontinuous within a range of 10% to 100% of the thickness of the glass plate 10. Figure 18 The modified portion 13 is formed continuously in the middle. If the range of the modified portion 13 is within the range described above, it is easier to reduce the stress required for cutting. At the virtual lines VL-1 and VL-3 around the center, the range of the modified portion 13 can be 100% of the thickness of the glass plate 10, less than 100%, less than 75%, less than 50%, or less than 30%.
[0057] When the number of virtual lines VL, n, is 3 or more, for example, when n is 3... Figure 18 As an example, compared to at least one central virtual line VL-2, it is preferable to form the modified portion 13 continuously or intermittently within a shorter range in the thickness direction of the glass plate 10 at the central peripheral virtual lines VL-1 and VL-3. By having the modified portion 13 with a shorter range in the thickness direction compared to at least one central virtual line VL-2, the laser output required for processing can be reduced, thus lowering costs. Furthermore, multiple modified portions 13 can be processed simultaneously using an optical system that branches a single laser beam into multiple beams, further shortening processing time.
[0058] It should be noted that when the number of virtual lines VL is 3 or more and is odd, the central virtual line VL refers to the (n+1) / 2th virtual line counted from one end. Furthermore, when the number of virtual lines VL n is 4 or more and is even, the central virtual line VL refers to both the n / 2th and n / 2+1th virtual lines counted from one end.
[0059] When the number of virtual lines VL, n, is 4 or more and is an even number, although not shown in the figure, it is preferable that the modified portion 13 is formed continuously or intermittently within a shorter range in the thickness direction of the glass plate 10 at the other central virtual lines VL compared to a single central virtual line VL. With the above configuration, the glass plate 10 can be cut along the desired central virtual line VL of the two central virtual lines VL.
[0060] The light source for laser LB can, for example, comprise a Nd-doped YAG crystal (Nd:YAG) that outputs pulsed light with a wavelength of 1064 nm. It should be noted that the wavelength of the pulsed light is not limited to 1064 nm. Nd:YAG second harmonic lasers (wavelength 532 nm) and Nd:YAG third harmonic lasers (wavelength 355 nm) can also be used.
[0061] The laser LB is irradiated onto the first main surface 11 through an optical system including a condenser lens. The modified part 13 is formed by moving its irradiation point along the virtual line VL and covering the entire virtual line VL.
[0062] The movement of the irradiation point can be achieved, for example, using a 2D or 3D electronic scanner. It should be noted that the movement of the irradiation point can be implemented by moving or rotating the stage holding the glass plate 10. For example, an XY stage, an XYθ stage, an XYZ stage, or an XYZθ stage can be used as the stage. The X, Y, and Z axes are orthogonal to each other, with the X and Y axes parallel to the first principal surface 11 and the Z axis perpendicular to the first principal surface 11.
[0063] like Figure 5 As shown, multiple modified portions 13 can be formed along the virtual line VL at intervals p ranging from 0.1 μm to 100 μm. The interval p is the average distance between the centers of 10 arbitrarily selected groups of adjacent modified portions 13. If the interval p is 100 μm or less, unwanted notches or cracks can be suppressed in step S5. If the interval p is 0.1 μm or more, the number of modified portions 13 can be reduced. The interval p is preferably 2 μm or more. The interval p is preferably 60 μm or less, more preferably 40 μm or less, further preferably 20 μm or less, and particularly preferably 10 μm or less.
[0064] like Figure 5 As shown, when viewed from a direction perpendicular to the first main surface 11, the diameter of the modified part 13 is... For example, greater than 0.1 μm and less than 60 μm. If the diameter If the diameter is less than 60 μm, the glass plate 10 can be cut with high precision along the virtual line VL in step S5. If the diameter... If the diameter is greater than 0.1 μm, the glass plate 10 can be easily cut at the virtual line VL. (Diameter) Preferably, it is 2μm or larger. Diameter Preferably, it is 40 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less.
[0065] It should be explained that, for example Figure 8 As shown, multiple modified sections 13 can be formed at intervals along the thickness direction from the virtual line VL. In this case, as... Figure 8 As shown, the laser LB can be focused into a point shape inside the glass plate 10, and the modified part 13 can be formed into a point shape. The laser LB source outputs a single pulse of light or a pulse group. The light wavelength and pulse width are adjusted so that multiphoton absorption occurs only near the focusing point.
[0066] like Figure 8 As shown, when the modified part 13 is formed into a point shape, multiple modified parts 13 are formed by repeatedly moving a focusing point within a plane at a certain depth from the first main surface 11 in two dimensions and changing the depth of the focusing point from the first main surface 11. The movement of the focusing point can be achieved using, for example, an XYZ stage, an XYZθ stage, or a 3D electronic scanner. When changing the depth of the focusing point by moving the stage, a 2D electronic scanner can also be used.
[0067] In step S4, although not shown, water is supplied to the virtual line VL of the glass plate 10. The water is supplied, for example, in a liquid state. The liquid water can be supplied in bulk or as a mist. Water can also be supplied in a gaseous state. By supplying water, the bonding strength of the glass can be reduced, thereby reducing the stress required to cut the glass plate 10 in step S5. The water supplied to the virtual line VL of the glass plate 10 can be removed before step S5.
[0068] In step S5, stress is applied to the glass plate 10, such as... Figure 6 As shown, the glass plate 10 is cut along the virtual line VL. The glass plate 10 is cut starting from the modified section 13. For example, stress is applied to the glass plate 10 by moving a roller along the virtual line VL while pressing it against the glass plate 10. Alternatively, although not shown, a spot beam of the second laser can be formed on the first main surface 11, and the spot beam can be moved along the virtual line VL to apply thermal stress to the glass plate 10.
[0069] The second laser primarily produces linear absorption by irradiating the glass plate 10. Primarily producing linear absorption means that the heat generated by linear absorption is greater than the heat generated by nonlinear absorption. Alternatively, almost no nonlinear absorption may be produced.
[0070] Linear absorption is also known as single-photon absorption. The probability of single-photon absorption is proportional to the photon density. In the case of single-photon absorption, according to Lambert-Beer's law, the following equation (1) holds.
[0071] I=I0×exp(-α×L)···(1)
[0072] In equation (1) above, I0 is the intensity of the second laser on the first principal surface 11, I is the intensity of the second laser on the second principal surface 12, L is the propagation distance of the second laser from the first principal surface 11 to the second principal surface 12, and α is the absorption coefficient of the glass for the second laser. α is the linear absorption coefficient, which is determined by the wavelength of the second laser and the chemical composition of the glass, etc.
[0073] If the temperature of the glass exceeds its slow cooling point, the glass is prone to plastic deformation, and the generation of thermal stress is limited. Therefore, the wavelength, output, and beam diameter of the first principal surface 11 are adjusted to bring the temperature of the glass below its slow cooling point.
[0074] The second laser is, for example, continuous wave light. The source of the second laser is not particularly limited; for example, it can be a carbon dioxide laser. A carbon dioxide laser, for example, outputs continuous wave light with a wavelength of 10600 nm. It should be noted that the second laser may also be pulsed light instead of continuous wave light.
[0075] The spot light of the second laser can also be formed on the first principal surface 11 in a manner that spans all virtual lines VL. The spot light of the second laser can also be circular on the first principal surface 11. Its diameter is, for example, 1 mm to 10 mm.
[0076] After step S5, a glass article 20 is obtained. The glass article 20 is characterized by having a main surface and end surfaces, and having multiple modified portions at a certain distance from at least one of the end surfaces. When viewed from a direction perpendicular to the main surface, the distance between the end surface at a certain distance from the center of the modified portions and the center of the modified portions is 2.0 μm or more and less than 30 μm. It should be noted that "at least one end surface" is an end surface formed by cutting the glass plate 10 along a virtual line.
[0077] More specifically, glass items 20, such as Figure 6 and Figure 7 The glass plate 10 has a first main surface 21, a second main surface 22 facing opposite to the first main surface 21, and four end surfaces 24 perpendicular to the first main surface 21 and the second main surface 22. The end surfaces 24 can be planar or curved. The number of end surfaces 24 is not limited to four; there can be multiple or a single end surface. The end surfaces 24 may also have at least one end surface 24a formed by cutting through the glass plate 10, and further include an end surface 24b other than the at least one end surface 24a formed by cutting through the glass plate 10, that is, an end surface 24b identical to the original end surface of the glass plate 10.
[0078] The glass article 20 has a plurality of modified portions 23 at a distance from at least one end face 24a. The modified portions 23 are, for example, the modified portions 13 formed in step S3. The modified portions 13 may also remain on at least one end face 24a.
[0079] It should be noted that the modified portion 23 can be formed by cutting out the glass article 20 using conventional methods and then irradiating the glass article 20 with laser LB. The glass article 20 may have multiple modified portions 23 at a certain distance from at least one end face 24a, or it may not have modified portions 23 at at least one end face 24a.
[0080] Viewed from a direction perpendicular to the first main surface 21, the distance D between the center of the modified part 23 and the end face 24a at a certain distance from the multiple modified parts is 2.0 μm or more and less than 30 μm.
[0081] In the embodiment section, a detailed description is provided. If D is 2.0 μm or more and less than 30 μm, when light is irradiated from the side onto at least one end face 24a with the first main surface 21 facing upwards, the outline of the end face 24a can be clearly observed from above. It should be noted that "from the side" refers to a direction orthogonal to the thickness direction of the plate. This is because the multiple modified parts 23 scatter the light. By being able to clearly observe the outline of at least one end face 24a, in addition to being suitable for end face quality management, for example, when using the glass article of this embodiment as the cover glass of a display device, the resolution of cameras, etc., is improved in subsequent processing steps, thus improving the positional accuracy of processing.
[0082] It should be noted that in step S2, when five virtual lines are set to cut the glass plate, and multiple modified parts 23 exist at different distances from the at least one end face 24a, it is sufficient that the center of the multiple modified parts 23 closest to the at least one end face 24a is at least 2.0 μm and less than 30 μm from the at least one end face 24a.
[0083] The spacing D is preferably 29 μm or less, more preferably 25 μm or less, even more preferably 20 μm or less, particularly preferably less than 20 μm, and extremely preferably 18 μm or less. Furthermore, the spacing D is preferably 2.5 μm or more, more preferably 7.0 μm or more.
[0084] When viewed from a direction perpendicular to the first main surface 21, the glass article 20 has a plurality of modified portions 23 along at least one end face 24a at a spacing P of 0.1 μm to 100 μm. The spacing P is the average of the distances between the centers of arbitrarily selected 10 groups of adjacent modified portions 23. If the spacing P is 100 μm or less, the outline of at least one end face 24a is easily observed. If the spacing P is 0.1 μm or more, the number of modified portions 23 can be reduced. The spacing P is preferably 2 μm or more. The spacing P is preferably 60 μm or less, more preferably 40 μm or less, further preferably 20 μm or less, and particularly preferably 10 μm or less.
[0085] Viewed from a direction perpendicular to the first main surface 21, the diameter Φ of the modified portion 23 is, for example, 0.1 μm or more and less than 60 μm. If the diameter Φ is less than 60 μm, light can be scattered along the rim of at least one end face 24a. If the diameter Φ is 0.1 μm or more, light scattering is possible. The diameter Φ is preferably 2 μm or more. The diameter Φ is preferably 40 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less.
[0086] Viewed from a direction perpendicular to the first main surface 21, at least one end surface 24a may have a curved portion with a radius of curvature of 200 mm or less. The radius of curvature of the curved portion is preferably 50 mm or less. Furthermore, the radius of curvature of the curved portion is preferably 1 mm or more.
[0087] The glass article 20 can be used as part of a display device, for example, as a cover glass. An anti-reflective film can be formed on the surface of the cover glass. The anti-reflective film suppresses light reflection and is, for example, a film formed by alternating layers of a high refractive index layer and a low refractive index layer with a refractive index lower than the high refractive index layer. The high refractive index layer is made of materials such as niobium oxide, titanium oxide, zirconium oxide, tantalum oxide, or silicon nitride. On the other hand, the low refractive index layer is made of materials such as silicon oxide, a mixed oxide of Si and Sn, a mixed oxide of Si and Zr, or a mixed oxide of Si and Al.
[0088] As described above, the following matters are disclosed in this specification.
[0089] [1] A method for manufacturing a glass article, comprising:
[0090] Multiple parallel virtual lines are set on the main surface of the glass plate.
[0091] Laser light is applied to each of the aforementioned virtual lines, and modified portions are formed along each of the aforementioned virtual lines in the glass plate.
[0092] Stress is applied to the glass plate, and the glass plate is cut along the virtual line.
[0093] The spacing between adjacent virtual lines is greater than 2.0 μm and less than 30 μm.
[0094] [2] In the method of manufacturing glass articles according to [1], the interval between adjacent virtual lines is more than 2.0 μm and less than 20 μm.
[0095] [3] In the method of manufacturing glass articles according to [1] or [2], the number of the above-mentioned virtual lines is an odd number of 3 or more.
[0096] [4] In the method of manufacturing glass articles according to [3], the number of the above-mentioned virtual lines is 3 or 5.
[0097] [5] In the method of manufacturing glass articles according to [3] or [4], the remaining virtual lines are arranged symmetrically with one of the virtual lines sandwiched between them.
[0098] [6] A method for manufacturing a glass article according to any one of [1] to [5], wherein the plurality of the above-mentioned virtual lines are arranged at equal intervals.
[0099] [7] A method for manufacturing a glass article according to any one of [1] to [6], wherein water is supplied to the virtual line after the modified part is formed and before the glass plate is cut.
[0100] [8] A method for manufacturing a glass article according to any one of [1] to [7], wherein a plurality of modified portions are formed at intervals in the thickness direction of the glass plate.
[0101] [9] A method for manufacturing a glass article according to any one of [1] to [8], wherein a plurality of the modified parts are formed along the virtual lines at intervals of 0.1 μm to 100 μm.
[0102]
[10] The method for manufacturing a glass article according to any one of [1] to [9], wherein, when viewed from a direction perpendicular to the main surface, the diameter of the modified part is 0.1 μm or more and less than 60 μm.
[0103]
[11] In the method of manufacturing a glass article according to any one of [1] to
[10] , the number of the above-mentioned virtual lines is three or more, and compared with at least one central virtual line, the above-mentioned modified part is continuously or intermittently formed in the virtual lines around the center within a shorter range in the thickness direction of the glass plate.
[0104]
[12] The method for manufacturing a glass article according to any one of [1] to
[11] , wherein the virtual line has a curved portion with a radius of curvature of 200 mm or less.
[0105]
[13] A glass article is a glass plate having a main surface and end surfaces.
[0106] The portion having multiple modified sections is located at a certain distance from at least one of the aforementioned end faces.
[0107] When viewed from a direction perpendicular to the main surface, the distance between the end face located at a certain distance from the multiple modified parts and the center of the modified part is 2.0 μm or more and less than 30 μm.
[0108]
[14] According to the glass article described in
[13] , when viewed from a direction perpendicular to the main surface, the distance between the end face and the center of the modified part is 2.0 μm or more and less than 20 μm.
[0109]
[15] The glass article according to
[13] or
[14] , wherein, when viewed from a direction perpendicular to the main surface, a plurality of the modified portions are provided along the end face at intervals of 0.1 μm to 100 μm.
[0110]
[16] The glass article according to any one of
[13] to
[15] , wherein, when viewed from a direction perpendicular to the main surface, the diameter of the modified part is 0.1 μm or more and less than 60 μm.
[0111]
[17] A glass article according to any one of
[13] to
[16] , wherein, when viewed from a direction perpendicular to the main surface, the end face has a curved portion with a radius of curvature of 200 mm or less.
[0112]
[18] A glass cover comprising any one of
[13] to
[17] .
[0113]
[19] A display device comprising any one of the glass articles described in
[13] to
[17] .
[0114] Example
[0115] The present invention will be specifically described below with examples, but the present invention is not limited thereto.
[0116] In Examples 1 to 28, the effects of (1) the number n of virtual lines VL, (2) the interval d between adjacent virtual lines VL, and (3) whether or not water is supplied to the virtual lines VL (step S4) on the stress required for cutting were investigated. Hereinafter, the stress required for cutting will also be referred to as fracture stress. In Examples 1 to 28, Examples 1 to 2, 10, 11 and 18 are comparative examples, and Examples 3 to 9, 12 to 17 and 19 to 28 are exemplary examples.
[0117] like Figure 10As shown, the fracture stress was measured using a four-point bending tester. The four-point bending tester used was an Autograph AGS-X 10kN manufactured by Shimadzu Corporation. The distance between the support points A was 30mm, and the distance between the load points B was 10mm. The descent speed of the upper rod was 1mm / min.
[0118] For the test piece 30 used in the four-point bending test, a rectangular plate (glass plate) with dimensions of 50 mm in length, 50 mm in width, and a thickness of 1.3 mm is prepared. n virtual lines VL are passed through the center of the distance between two opposing sides of the glass plate and are set to be parallel to the remaining two sides. When n is 2 or more, the n virtual lines VL are set at equal intervals.
[0119] The irradiation conditions of the laser LB forming the modified section 33 in each virtual line VL are as follows.
[0120] Oscillator: Picosecond pulsed laser (Rofin, StarPico3)
[0121] Oscillation mode: Pulse oscillation (burst pulse)
[0122] Wavelength: 1064nm
[0123] Output: 100%
[0124] Oscillation frequency: 18750Hz
[0125] In-plane scanning speed: 93.75 mm / s
[0126] In-plane irradiation spacing: 5μm.
[0127] In Examples 1 to 28, the test piece 30 was processed under the same processing conditions, except for (1) the number n of the virtual lines VL, (2) the interval d between adjacent virtual lines VL, and (3) whether water was supplied to the virtual lines VL (step S4). In Examples 1 to 28, the modified portion was continuously formed along the entire thickness direction of the glass plate in all virtual lines VL. The processing conditions and the results of the fracture stress measurements are shown in Tables 1 to 4.
[0128] [Table 1]
[0129]
[0130] [Table 2]
[0131]
[0132] [Table 3]
[0133]
[0134] [Table 4]
[0135]
[0136] In Tables 1 to 4, “AVE” represents the average value.
[0137] Reference Figure 11 The effect of setting the number of virtual lines VL n to 1 or 3 and supplying water to the virtual lines VL on the spacing d of adjacent virtual lines VL is explained. Figure 11 It can be seen that if multiple virtual lines VL are set at intervals d of 2.0 μm or more and less than 30 μm, the average fracture stress AVE can be reduced compared to when the number of virtual lines VL is 1. In particular, if the interval d is greater than 3.5 μm and less than 20 μm, the average fracture stress AVE can be significantly reduced. It should be noted that the same trend was observed in Examples 1 to 11, where water was supplied to the virtual lines VL, but not in the cases where water was not supplied to the virtual lines VL.
[0138] Reference Figure 12 and Figure 13 The effect of setting the interval d between adjacent virtual lines VL to 10 μm and supplying water to the virtual lines VL is explained. Based on... Figure 12 It is known that the more the number of virtual lines VL (n) increases, the more it reduces the average fracture stress AVE. This is believed to be because a higher number of virtual lines VL (n) allows water to penetrate more easily, thus promoting stress corrosion. Furthermore, according to... Figure 13 It can be seen that if n is an odd number greater than or equal to 3, the glass plate can be cut at the central virtual line VL. It should be noted that if n is an even number greater than or equal to 2, the glass plate will be cut by the weaker of the two central virtual lines VL.
[0139] Reference Figure 14 and Figure 15 The effect of setting the interval d between adjacent virtual lines VL to 10 μm and not supplying water to the virtual lines VL is explained. Based on... Figure 14 It can be seen that the more the number n of virtual lines VL increases, the more the average fracture stress AVE can be reduced. Furthermore, according to... Figure 15 It can be seen that if n is an odd number greater than or equal to 3, the glass plate can be cut at the central virtual line VL. It should be noted that when n is an even number greater than or equal to 2, the glass plate is cut by the weaker of the two central virtual lines VL.
[0140] Reference Figure 16 The impact of supplying water to the virtual line VL is explained. Figure 16 It can be seen that if water is supplied to the virtual line VL, the average value of the fracture stress AVE can be reduced compared with the case where water is not supplied to the virtual line VL.
[0141] Figure 17 (A) is a photograph taken under a microscope, showing the test piece 30 of Example 1 from above, with light shining from the side onto the cut surface 34. Figure 17 Photograph (B) is a microscopic view of the cut surface 34 of test piece 30 in Example 6 illuminated from the side. If compared... Figure 17 (A) and Figure 17 (B) indicates that if the modified part 33 is formed at a specified distance from the cut surface 34, the outline of the cut surface 34 can be clearly observed from above.
[0142] In Examples 29 and 30, (4) the effect of the formation range of the modified portion in the thickness direction of the glass plate on the stress required for cutting was investigated. Examples 29 and 30 are examples. As test pieces 30 for the four-point bending test, the same test pieces as those in Examples 1 to 28 were prepared. The irradiation conditions of the laser LB in which the modified portion 33 is formed at each virtual line VL are as follows.
[0143] Oscillator: Picosecond pulsed laser (Rofin, StarPico3)
[0144] Oscillation mode: Pulse oscillation (burst pulse)
[0145] Wavelength: 1064nm
[0146] Output: 100%
[0147] Oscillation frequency: 37500Hz
[0148] In-plane scanning speed: 187.5 mm / s
[0149] In-plane irradiation spacing: 5μm.
[0150] In Examples 29 and 30, three parallel virtual lines were established. At the central virtual line, a modified portion was continuously formed along the thickness of the glass plate. Conversely, at the virtual lines at the central periphery (both ends), a modified portion was continuously formed within approximately 36% (470 μm) or approximately 15% (200 μm) of the glass plate thickness (1.3 mm). Test piece 30 (reference) Figure 10 Starting from the upper surface of (A), the modified section is continuously formed to the desired depth. Table 5 shows the results of the processing conditions and fracture stress measurements. In Table 5, "AVE" represents the average value.
[0151] [Table 5]
[0152]
[0153] In Table 5, t / t0 (%) represents the ratio of the depth t of the modified portion of the virtual line formed at the central periphery (both ends) to the thickness t0 of the glass plate.
[0154] The average fracture stress AVE of Examples 29 and 30 is lower than that of Example 18. This shows that even if t / t0 (%) is less than 100%, the fracture stress can still be reduced.
[0155] While the manufacturing method, glass article, cover glass, and display device of the glass article disclosed above have been described, this disclosure is not limited to the above-described embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations can be made within the scope described in the patent claims. These, of course, also fall within the technical scope of this disclosure.
[0156] This application claims priority based on Japanese Patent Application No. 2021-098236, filed on June 11, 2021 with the Japan Patent Office, the entire contents of which are incorporated herein by reference.
[0157] Symbol Explanation
[0158] 10 glass plates
[0159] 11 Main side 1
[0160] 13 Quality Improvement Department
[0161] VL Virtual Line
[0162] LB Laser
Claims
1. A method for manufacturing a glass article, comprising: Multiple parallel virtual lines are set on the main surface of the glass plate. Laser light is applied to each of the multiple virtual lines, and modified sections are formed along the virtual lines on the glass plate. Stress is applied to the glass plate, cutting it along one of the central virtual lines; The spacing between adjacent virtual lines is greater than 2.0 μm and less than 30 μm. The number of virtual lines is an odd number of 3 or more. The modified portion is continuously formed along the virtual lines other than the central virtual line, starting from the main surface of the glass plate, within a range of 10% to 100% of the glass plate thickness. The following glass article is obtained: the glass article is a glass plate having a main surface and end surfaces, and having a plurality of modified parts at a certain distance from at least one of the end surfaces. The modified parts are continuously formed in the range of 10% to 100% of the thickness of the glass plate, starting from the main surface of the glass plate. When viewed from a direction perpendicular to the main surface, the distance between the end surface at a certain distance from the plurality of modified parts and the center of the modified part closest to the end surface is more than 2.0 μm and less than 30 μm.
2. The method for manufacturing glass articles according to claim 1, wherein, The spacing between adjacent virtual lines is greater than 2.0 μm and less than 20 μm.
3. The method for manufacturing glass articles according to claim 1, wherein, The number of virtual lines is 3 or 5.
4. The method for manufacturing glass articles according to claim 1, wherein, The remaining virtual lines are arranged symmetrically, with one of the virtual lines sandwiched between them.
5. The method for manufacturing glass articles according to claim 1, wherein, The virtual lines are arranged at equal intervals.
6. The method for manufacturing a glass article according to claim 1, wherein, It features: supplying water to the virtual line after the modified section is formed and before the glass plate is cut.
7. The method for manufacturing a glass article according to claim 1, wherein, It has the following features: a plurality of modified portions are formed at intervals along the thickness direction of the glass plate.
8. The method for manufacturing glass articles according to claim 1, wherein, It has the following features: a plurality of modified parts are formed along the virtual line at intervals of 0.1 μm to 100 μm.
9. The method for manufacturing a glass article according to claim 1, wherein, Viewed from a direction perpendicular to the main surface, the diameter of the modified part is 0.1 μm or more and less than 60 μm.
10. The method for manufacturing a glass article according to claim 1, wherein, Compared to at least one central virtual line, the modified portion is continuously formed in the virtual lines around the center within a shorter range in the thickness direction of the glass plate.
11. The method for manufacturing a glass article according to claim 1, wherein, The virtual line has a curved section with a radius of curvature of less than 200 mm.
12. A glass article comprising a glass plate having a main face and end faces. The portion having multiple modified sections is located at a certain distance from at least one of the end faces. The modified section is continuously formed within a range of 10% to 100% of the thickness of the glass plate, starting from the main surface of the glass plate. When viewed from a direction perpendicular to the main surface, the distance between the end face at a certain distance from the plurality of modified parts and the center of the modified part closest to the end face is more than 2.0 μm and less than 30 μm.
13. The glass article according to claim 12, wherein, When viewed from a direction perpendicular to the main surface, the distance between the end face and the center of the plurality of modified parts closest to the end face is more than 2.0 μm and less than 20 μm.
14. The glass article according to claim 12, wherein, Viewed from a direction perpendicular to the main surface, a plurality of modified portions are present along the end face at intervals of 0.1 μm to 100 μm.
15. The glass article according to claim 12, wherein, Viewed from a direction perpendicular to the main surface, the diameter of the modified part is 0.1 μm or more and less than 60 μm.
16. The glass article according to claim 12, wherein, Viewed from a direction perpendicular to the main surface, the end face has a curved portion with a radius of curvature of less than 200 mm.
17. A glass cover comprising a glass article according to any one of claims 12 to 16.
18. A display device comprising a glass article according to any one of claims 12 to 16.
Citation Information
Patent Citations
Material processing method by laser filament formation
JP2013536081A
Roll mold manufacturing method, roll mold manufacturing device, program, and microlens array
JP2021098236A
Method for manufacturing glass plate, glass plate, method for manufacturing glass article, glass article, and device for manufacturing glass article
CN107922259A
Method for manufacturing glass product and glass product
CN109641776A
Laser processing method and laser processing apparatus
JP2017174941A