An antibacterial tissue patch and a preparation method and application thereof
By preparing antimicrobial tissue patches with a Janus structure, the problems of imprecise and time-consuming application of bioadhesives on tissue surfaces were solved, achieving a combination of strong adhesion and antimicrobial properties, and improving biocompatibility.
Patent Information
- Application Number
- CN202311399822.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-26
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-10-26
AI Technical Summary
In the existing technology, bio-adhesives and gel materials have problems such as being difficult to apply precisely, being time-consuming and laborious, being difficult to form strong adhesion to tissue surfaces, and lacking antibacterial properties when applied to tissue surfaces.
An antimicrobial tissue patch with a Janus structure comprises a carrier layer and an antimicrobial tissue adhesion layer. The antimicrobial adhesion layer is composed of polylysine, maleimide acrylate, N-vinylpyrrolidone, and acrylic acid, and is prepared by coating and ultraviolet irradiation to form asymmetric adhesion and antimicrobial properties.
It achieves strong adhesion to tissue surfaces and good antibacterial activity, exhibits good biocompatibility, and avoids the shortcomings of traditional materials.
Smart Images

Figure CN117482276B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of pharmaceutical technology, and in particular to an antibacterial tissue patch, its preparation method, and its application. Background Technology
[0002] Wound infection is a long-standing public health problem. Effectively controlling bacterial growth and improving people's quality of life makes antibacterial products a promising area for development. Conventional methods for treating wounds rely primarily on mechanical connections to the tissue surface using sutures or U-shaped staples. However, for soft tissues, conventional methods can lead to air leakage (e.g., in lung wounds) and fluid exudation, subsequently causing inflammatory reactions and bacterial growth.
[0003] Currently, alternatives to traditional methods include bio-adhesives and gels. These materials are produced in the form of liquids or gels with a certain viscosity, or are premixed before use and applied to tissue surfaces using specialized syringes or other devices. However, if these bio-adhesives or gels are low in viscosity, there is a risk of them spreading from the application area to other areas, making it difficult to apply them precisely to the desired tissue region; if the viscosity is high, they are difficult to prepare; even if premixed before use, it is obviously time-consuming and laborious, and also requires the use of auxiliary equipment. Therefore, an ideal tissue sealing product should be a material with good biocompatibility, good tissue adhesion, no tissue irritation, and good antibacterial properties.
[0004] Janus interface materials refer to materials with asymmetric physical or chemical structures on both sides. In recent years, materials with Janus structures have attracted increasing attention from researchers in the fields of structural and functional design. Compared with other single homogeneous materials, Janus structures can bring bifunctional benefits or functional synergies, and therefore can be applied in many fields. Janus films can be obtained through a simple sequential stacking method, but since the two sides of the film are different materials, the interfacial compatibility between the different materials cannot be guaranteed. Summary of the Invention
[0005] The problem the invention aims to solve
[0006] In view of the shortcomings of the prior art, the purpose of this invention is to provide an antibacterial tissue patch and its preparation method, so that the tissue patch can form a strong adhesion to the tissue surface and has antibacterial activity and good biocompatibility.
[0007] Solution for solving the problem
[0008] The present invention provides an antibacterial tissue patch, the tissue patch comprising a carrier layer and an antibacterial tissue adhesion layer, the antibacterial tissue adhesion layer comprising an antibacterial component and an adhesion component, the antibacterial component comprising polylysine.
[0009] Preferably, the polylysine is acryloyl polylysine.
[0010] Preferably, the adhesive component is selected from one or more of succinimide ester, isocyanate, acrylate, maleimide, and epoxide; more preferably, the adhesive component is selected from maleimide; even more preferably, the adhesive component is maleimide acrylate.
[0011] Preferably, the antimicrobial tissue adhesion layer further comprises N-vinylpyrrolidone and acrylic acid; more preferably, the antimicrobial tissue adhesion layer is composed of acryloyl polylysine, maleimide acrylate, N-vinylpyrrolidone and acrylic acid.
[0012] Preferably, the carrier layer is a film-forming polymer; more preferably, the carrier layer is a copolymer prepared from one or more selected from polylactic acid, polyglycolic acid, polycaprolactone, and polyhydroxyalkanoate; even more preferably, the carrier layer is a lactic acid-glycolic acid copolymer.
[0013] Preferably, the molar ratio of acrylic acid to maleimide acrylate is 10:1 to 1:10; more preferably, the molar ratio of acrylic acid to maleimide acrylate is 4:1 to 1:4; and even more preferably, the molar ratio of acrylic acid to maleimide acrylate is 1:1.
[0014] Preferably, the molar ratio of N-vinylpyrrolidone to maleimide acrylate is 10:1-1:1; more preferably, the molar ratio of N-vinylpyrrolidone to maleimide acrylate is 5:1-5:4; and even more preferably, the molar ratio of N-vinylpyrrolidone to maleimide acrylate is 2:1.
[0015] Preferably, the amount of acryloyl polylysine added is 0.05%-2% of the sum of the mass of N-vinylpyrrolidone, acrylic acid, and maleimide acrylate; more preferably, the amount of acryloyl polylysine added is 0.1%-0.9% of the sum of the mass of N-vinylpyrrolidone, acrylic acid, and maleimide acrylate; even more preferably, the amount of acryloyl polylysine added is 0.7% of the sum of the mass of N-vinylpyrrolidone, acrylic acid, and maleimide acrylate.
[0016] The present invention also provides a method for preparing the tissue patch, characterized in that the method includes:
[0017] (a) Preparation of the carrier layer;
[0018] (b) Preparation of an antibacterial tissue adhesion layer;
[0019] (c) Preparation of antimicrobial tissue patches.
[0020] Preferably, step (b) includes:
[0021] (b1) Preparation of maleimide acrylate;
[0022] (b2) Preparation of acryloyl polylysine;
[0023] (b3) Prepare an antibacterial tissue adhesion layer solution.
[0024] Preferably, the preparation of the carrier layer in step (a) involves coating the film-forming polymer solution into a carrier layer and then drying it.
[0025] Preferably, the preparation of maleimide acrylate in step (b1) involves adding acrylic monomer to tetrahydrofuran, adding a dicyclohexylcarbodiimide solution of tetrahydrofuran while stirring, adding a hydroxyethylmaleimide solution dissolved in tetrahydrofuran after stirring, filtering under reduced pressure after the reaction is complete, rotary evaporating, adding diethyl ether, filtering again, rotary evaporating, and then drying.
[0026] Preferably, the preparation of acryloyl polylysine in step (b2) involves adding polylysine and acrylic acid monomer to MES buffer, dissolving them, then adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide in MES buffer. After the reaction is complete, the mixture is dialyzed with purified water and then dried.
[0027] Preferably, the preparation of the antibacterial tissue adhesion layer solution in step (b3) involves adding N-vinylpyrrolidone, acrylic acid, maleimide acrylate and acryloyl polylysine to purified water in a certain proportion, stirring until uniform, adding a photoinitiator, and stirring until uniform in the dark.
[0028] Preferably, the preparation of the antibacterial tissue patch in step (c) involves coating the antibacterial tissue adhesion layer solution prepared in step (b3) onto the carrier layer prepared in step (a), irradiating it with ultraviolet light, and then drying it.
[0029] The present invention also provides an application of the tissue patch in the preparation of tissue and organ repair products for humans or animals.
[0030] The effects of the invention
[0031] The antibacterial tissue patch of this invention is made of synthetic polymer material, is safe and non-toxic, and has good biocompatibility. The asymmetric adhesion of the tissue patch also gives it an anti-adhesion effect. At the same time, the addition of polylysine component enables the antibacterial tissue patch to form strong adhesion to the tissue surface and also has good antibacterial activity. Attached Figure Description
[0032] Figure 1 Infrared absorption spectrum of antibacterial tissue patch #1.
[0033] Figure 2 This is cell survival data for L929 cells. Detailed Implementation
[0034] To make the technical solution and beneficial effects of the present invention more apparent and understandable, a detailed description is provided below by listing specific embodiments. The accompanying drawings are not necessarily drawn to scale, and local features may be enlarged or reduced to more clearly show the details of the local features; unless otherwise defined, the technical and scientific terms used herein have the same meanings as those in the technical field to which this application pertains.
[0035] Unless otherwise specified, the experimental methods used in this invention are conventional methods. Unless otherwise specified, the materials, reagents, and standards used in the following examples are commercially available.
[0036] As used herein, the term "tissue patch" refers to a patch that is bonded to a tissue surface by van der Waals forces or hydrogen bonds, or by the reaction of tissue reactive functional groups with the tissue surface.
[0037] As used herein, the term “adhesion layer” or “adhesion component” refers to a substance that has an affinity for tissue surfaces, i.e., adheres to the surface by forming bonds, which are typically non-covalent and are formed by interaction with tissue and / or underlying cells.
[0038] As used herein, the term "antimicrobial" is used in its general sense to refer to the property of a compound, product, composition, or article to prevent or slow the growth, spread, formation, or other means of survival of organisms (e.g., bacteria, viruses, protozoa, fungi, or other organisms that may cause decay or infection).
[0039] As used herein, the term "polylysine" refers to an antimicrobial polypeptide produced by Streptomyces, which is polymerized from 25-35 lysine residues and, as a natural antimicrobial material, possesses broad-spectrum antimicrobial activity. Preferably, in this invention, acryloyl polylysine is used.
[0040] As used herein, the term "maleimide" refers to the ability of the double bond in maleimide acrylate to undergo a Michael addition reaction with thiol groups on the tissue surface to form a chemical bond. Preferably, in this invention, maleimide acrylate is used.
[0041] As used herein, the term "copolymer" refers to a polymer formed by the polymerization of two or more monomers.
[0042] As used herein, the terms “lactic acid glycolic acid copolymer” and “lactide glycolide copolymer” are used interchangeably.
[0043] As used herein, the term "coating" refers to a method of preparing a film by applying a polymer solution onto a substrate.
[0044] As used in this article, the term "vacuum filtration" refers to a method that uses air extraction to reduce the pressure in a filtration flask to achieve solid-liquid separation.
[0045] As used herein, the term "MES buffer" refers to an acidic buffer solution prepared from 2-(N-morpholine)ethanesulfonic acid monohydrate at a concentration of 20 mM.
[0046] As used in this article, the term "dialysis" refers to a separation and purification technique that separates small molecules from biological macromolecules by diffusing them through a semipermeable membrane into water (or a buffer solution).
[0047] As used in this article, the term "photoinitiator" refers to a compound that can absorb energy of a certain wavelength in the ultraviolet (250–420 nm) or visible (400–800 nm) region, generate free radicals, cations, etc., and thus initiate monomer polymerization, cross-linking, and curing.
[0048] As used herein, the term "Janus" or "Janus film" refers to a material with an asymmetric physical or chemical structure on both sides.
[0049] As used in this article, the term "asymmetric adhesion" refers to an antimicrobial tissue patch that reacts with one side of the tissue surface while the other side does not.
[0050] The present invention provides an antibacterial tissue patch, the tissue patch comprising a carrier layer and an antibacterial tissue adhesion layer, the antibacterial tissue adhesion layer comprising an antibacterial component and an adhesion component, the antibacterial component comprising polylysine.
[0051] In some embodiments, the polylysine is acryloyl polylysine.
[0052] In some embodiments, the antimicrobial tissue patch is an asymmetrically adhered Janus antimicrobial tissue patch.
[0053] In some embodiments, the adhesive component is selected from one or more of succinimide esters, isocyanates, acrylates, maleimide, and epoxides.
[0054] In some embodiments, the adhesive component is selected from maleimide.
[0055] In some embodiments, the adhesive component is maleimide acrylate.
[0056] In some embodiments, the groups that form initial adhesion forces (e.g., hydrogen bonds, van der Waals forces, etc.) with the tissue are one or more of carboxyl, carbonyl, and hydroxyl groups.
[0057] In some implementations, maleimide provides groups that form a long-lasting adhesion to tissue.
[0058] In some implementations, the long-lasting adhesion is achieved by reacting with the protein structure on the tissue surface to form stable covalent bonds.
[0059] In some implementations, maleimide can undergo a Michael addition reaction with thiol groups to obtain stable thioether bonds, thereby providing long-lasting adhesion.
[0060] In some embodiments, the antimicrobial tissue adhesion layer further includes N-vinylpyrrolidone and acrylic acid.
[0061] In some embodiments, the antimicrobial tissue adhesion layer is composed of acryloyl polylysine, maleimide acrylate, N-vinylpyrrolidone, and acrylic acid.
[0062] In some embodiments, the carrier layer is a film-forming polymer.
[0063] In some embodiments, the carrier layer is a copolymer prepared from one or more selected from polylactic acid, polyglycolic acid, polycaprolactone, and polyhydroxyalkanoates.
[0064] In some embodiments, the carrier layer is a lactic acid-glycolic acid copolymer.
[0065] In some embodiments, the molar ratio of acrylic acid to maleimide acrylate is 10:1 to 1:10.
[0066] In some embodiments, the molar ratio of acrylic acid to maleimide acrylate is 4:1 to 1:4.
[0067] In some embodiments, the molar ratio of acrylic acid to maleimide acrylate is 1:1.
[0068] In some embodiments, the molar ratio of N-vinylpyrrolidone to maleimide acrylate is 10:1 to 1:1.
[0069] In some embodiments, the molar ratio of N-vinylpyrrolidone to maleimide acrylate is 5:1 to 5:4.
[0070] In some embodiments, the molar ratio of N-vinylpyrrolidone to maleimide acrylate is 2:1.
[0071] In some embodiments, the molar ratio of N-vinylpyrrolidone:maleimide acrylate:acrylic acid is 2:1:1.
[0072] In some embodiments, the amount of acryloyl polylysine added is 0.05%-2% of the sum of the mass of N-vinylpyrrolidone, acrylic acid, and maleimide acrylate.
[0073] In some embodiments, the amount of acryloyl polylysine added is 0.1% to 0.9% of the sum of the mass of N-vinylpyrrolidone, acrylic acid, and maleimide acrylate.
[0074] In some embodiments, the amount of acryloyl polylysine added is 0.7% of the sum of the mass of N-vinylpyrrolidone, acrylic acid, and maleimide acrylate.
[0075] The present invention also provides a method for preparing the tissue patch, characterized in that the method includes:
[0076] (a) Preparation of the carrier layer;
[0077] (b) Preparation of an antibacterial tissue adhesion layer;
[0078] (c) Preparation of antimicrobial tissue patches.
[0079] In some implementations, step (b) includes:
[0080] (b1) Preparation of maleimide acrylate;
[0081] (b2) Preparation of acryloyl polylysine;
[0082] (b3) Prepare an antibacterial tissue adhesion layer solution.
[0083] In some embodiments, the preparation of the carrier layer in step (a) involves coating a film-forming polymer solution onto a carrier layer and then drying it.
[0084] In some embodiments, the preparation of the carrier layer in step (a) involves coating a lactide-glycolic acid copolymer solution onto a polyoxymethylene board and then drying it at 30°C for 60 min.
[0085] In some embodiments, the preparation of the carrier layer in step (a) involves dissolving 15g of a lactide-glycol copolymer (50% lactide and 50% glycolide, Mw = 100kDa) in 100mL of acetone to prepare a 15% w / v solution. The solution is then coated onto a polyoxymethylene board using a laboratory coater to achieve a layer thickness of approximately 15μm. The board is then placed in a vacuum drying oven and dried at 30°C for 60min.
[0086] In some embodiments, the preparation of maleimide acrylate in step (b1) involves adding an acrylic monomer to tetrahydrofuran, adding a dicyclohexylcarbodiimide solution of tetrahydrofuran while stirring, adding a hydroxyethylmaleimide solution dissolved in tetrahydrofuran after stirring, filtering under reduced pressure after the reaction is complete, rotary evaporating, adding diethyl ether, filtering again, rotary evaporating, and then drying.
[0087] In some embodiments, the preparation of maleimide acrylate in step (b1) involves adding distilled and purified acrylic acid monomer to a flask containing 100 mL of tetrahydrofuran, adding 100 mL of a dicyclohexylcarbodiimide solution of tetrahydrofuran under magnetic stirring, stirring for 30 min to ensure thorough mixing, then adding a hydroxyethylmaleimide solution dissolved in 200 mL of tetrahydrofuran, reacting at room temperature for 24 h, removing the reaction byproduct dicyclohexylurea by vacuum filtration after the reaction is complete, rotary evaporating the filtrate to dryness, adding diethyl ether, filtering again to remove insoluble matter, rotary evaporating the filtrate to dryness, and drying the product in a vacuum drying oven for 24 hours to obtain maleimide acrylate.
[0088] In some embodiments, the preparation of acryloyl polylysine in step (b2) involves adding polylysine and acrylic acid monomer to a MES buffer, dissolving them, then adding a MES buffer of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide. After the reaction is complete, the mixture is dialyzed with purified water and then dried.
[0089] In some embodiments, the preparation of acryloyl polylysine in step (b2) involves adding 10g of polylysine and 5g of purified acrylic acid monomer to a flask containing 20ml of MES buffer, dissolving them, and then adding 13.3g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 12g of N-hydroxysuccinimide in MES buffer. The reaction is carried out at room temperature for 24 hours. After the reaction is completed, the product is dialyzed with purified water for 5 days, with the water being changed every 8-16 hours. Then, the product is dried to obtain acryloyl polylysine.
[0090] In some embodiments, the preparation of the antimicrobial tissue adhesion layer solution in step (b3) involves adding N-vinylpyrrolidone, acrylic acid, maleimide acrylate and acryloyl polylysine to purified water, stirring until homogeneous, adding a photoinitiator, and stirring until homogeneous in the dark.
[0091] In some embodiments, the preparation of the antimicrobial tissue adhesion layer solution in step (b3) involves purifying N-vinylpyrrolidone and acrylic acid by vacuum distillation, then adding 2.94 g of N-vinylpyrrolidone, 1.9 g of acrylic acid, 5.16 g of maleimide acrylate and 0.07 g of acryloyl polylysine to 20 mL of purified water, stirring evenly at room temperature, then adding 0.1 g of photoinitiator, stirring evenly in the dark to obtain the antimicrobial tissue adhesion layer solution.
[0092] In some embodiments, the preparation of the antimicrobial tissue patch in step (c) involves coating the antimicrobial tissue adhesion layer solution prepared in step (b3) onto the carrier layer prepared in step (a), irradiating it with ultraviolet light, and then drying it.
[0093] In some embodiments, the preparation of the antimicrobial tissue patch in step (c) involves coating the antimicrobial tissue adhesion layer solution prepared in step (b3) onto the dried carrier layer prepared in step (a) using a laboratory coater, irradiating it with a UV lamp for 180 seconds, and then placing it in a vacuum drying oven and drying it at 70°C for 48 hours to obtain an asymmetric adhesive Janus antimicrobial tissue patch with a thickness of 40 μm.
[0094] The present invention also provides an application of the tissue patch in the preparation of tissue and organ repair products for humans or animals.
[0095] Example 1: Preparation of antibacterial tissue patch #1
[0096] The antibacterial tissue patch of the present invention is prepared by the following steps:
[0097] 1. Preparation of the carrier layer
[0098] 15g of lactide-glycolic acid copolymer (containing 50% lactide and 50% glycolide, Mw = 100kDa) solid was dissolved in 100mL of acetone to prepare a 15% w / v solution. The 15% w / v lactide-glycolic acid copolymer solution was then coated onto a polyoxymethylene (POM) board using a coater. The coating was approximately 15μm thick and did not peel off from the POM board. The board was then placed in a vacuum drying oven and dried at 30°C for 60min.
[0099] 2. Preparation of antibacterial tissue adhesion layer solution
[0100] (a) Preparation of maleimide acrylate: Acrylic acid monomer (10 g, 0.139 mol) purified by vacuum distillation was added to a flask containing 100 mL of tetrahydrofuran. A solution of dicyclohexylcarbodiimide (43 g, 0.208 mol) dissolved in 100 mL of tetrahydrofuran was added under magnetic stirring. The mixture was stirred for 30 min to ensure thorough mixing. Finally, a solution of hydroxyethylmaleimide (23.5 g, 0.167 mol) dissolved in 200 mL of tetrahydrofuran was slowly added. The reaction was carried out at room temperature for 24 hours. After the reaction was complete, the byproduct dicyclohexylurea was removed by vacuum filtration. The filtrate was then evaporated to dryness by rotary evaporation. An appropriate amount of diethyl ether was added, and the mixture was filtered again to remove insoluble matter. The filtrate was then evaporated to dryness by rotary evaporation. The final product was dried in a vacuum drying oven for 24 hours to obtain maleimide acrylate.
[0101] (b) Preparation of acryloylpolylysine: 10 g of polylysine (Mw = 4 kDa) and 5 g of purified acrylic acid monomer were added to a flask containing 20 mL of MES buffer. After complete dissolution, MES buffer containing 13.3 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 12 g of N-hydroxysuccinimide was added, and the reaction was carried out at room temperature for 24 hours. After the reaction was completed, the product was dialyzed with purified water for 5 days, with the water being changed every 8-16 hours. After drying, acryloylpolylysine was obtained.
[0102] (c) Preparation of antibacterial tissue adhesion layer solution: N-vinylpyrrolidone and acrylic acid were purified by vacuum distillation. Then, 2.94 g of N-vinylpyrrolidone, 1.9 g of acrylic acid, 5.16 g of maleimide acrylate and 0.07 g of acryloyl polylysine were added to 20 mL of purified water and stirred evenly at room temperature. Then, 0.1 g of photoinitiator (lithium phenyl-2,4,6-trimethylbenzoylphosphonate) was added and stirred evenly in the dark to obtain the antibacterial tissue adhesion layer solution.
[0103] 3. Preparation of antibacterial tissue adhesion layer: The antibacterial tissue adhesion layer solution was coated onto the dried carrier layer using a laboratory coating machine, irradiated under a UV lamp for 180s, and then placed in a vacuum drying oven and dried at 70℃ for 48 hours to prepare an asymmetric adhesion Janus antibacterial tissue patch #1 with a thickness of 40μm.
[0104] 4. Infrared spectroscopy detection
[0105] The prepared asymmetric adhered Janus antibacterial tissue patch was subjected to infrared spectroscopy using ATR-FTIR, and its infrared absorption spectrum is shown below. Figure 1 As shown. The infrared characteristic absorption peak corresponding to the antibacterial tissue adhesion layer is as follows: 2943.36 cm⁻¹ -1 The characteristic absorption peak of acrylic acid (CH) is 1731.23 cm⁻¹. -1The characteristic absorption peak for vinylpyrrolidone C=O is 1651.49 cm⁻¹. -1 The characteristic absorption peak for CN of acryloyl polylysine is 693.54 cm⁻¹. -1 The peak represents the characteristic absorption peak of maleimide acrylate C=C.
[0106] Example 2: Preparation of antibacterial tissue patch #2
[0107] The preparation method was the same as in Example 1, except that the molar ratio of acrylic acid to maleimide acrylate was adjusted to 4:1, and the composition of each component of the antibacterial tissue adhesion layer was shown in Table 1. An asymmetric adhesion Janus antibacterial tissue patch #2 with a thickness of 40 μm was prepared.
[0108] Example 3: Preparation of antibacterial tissue patch #3
[0109] The preparation method was the same as in Example 1, except that the molar ratio of acrylic acid to maleimide acrylate was adjusted to 4:1, and the composition of each component of the antibacterial tissue adhesion layer was shown in Table 1. An asymmetric adhesion Janus antibacterial tissue patch #3 with a thickness of 40 μm was prepared.
[0110] Example 4: Preparation of antibacterial tissue patch #4
[0111] The preparation method was the same as in Example 1, except that the amount of acryloyl polylysine added was adjusted to 0.1% of the sum of the mass of N-vinylpyrrolidone, acrylic acid and maleimide acrylate. The composition of each component of the antimicrobial tissue adhesion layer is shown in Table 1. An asymmetric adhesion Janus antimicrobial tissue patch #4 with a thickness of 40 μm was prepared.
[0112] Example 5: Preparation of antibacterial tissue patch #5
[0113] The preparation method was the same as in Example 1, except that the amount of acryloyl polylysine added was adjusted to 0.3% of the sum of the mass of N-vinylpyrrolidone, acrylic acid and maleimide acrylate. The composition of each component of the antimicrobial tissue adhesion layer is shown in Table 1. An asymmetric adhesion Janus antimicrobial tissue patch #5 with a thickness of 40 μm was prepared.
[0114] Example 6: Preparation of antibacterial tissue patch #6
[0115] The preparation method was the same as in Example 1, except that the amount of acryloyl polylysine added was adjusted to 0.5% of the sum of the mass of N-vinylpyrrolidone, acrylic acid and maleimide acrylate. The composition of each component of the antimicrobial tissue adhesion layer is shown in Table 1. An asymmetric adhesion Janus antimicrobial tissue patch #6 with a thickness of 40 μm was prepared.
[0116] Example 7: Preparation of antibacterial tissue patch #7
[0117] The preparation method was the same as in Example 1, except that the amount of acryloyl polylysine added was adjusted to 0.9% of the sum of the mass of N-vinylpyrrolidone, acrylic acid and maleimide acrylate. The composition of each component of the antimicrobial tissue adhesion layer is shown in Table 1. An asymmetric adhesion Janus antimicrobial tissue patch #7 with a thickness of 40 μm was prepared.
[0118] Comparative Example 1: Preparation of Antibacterial Tissue Patch #8
[0119] The preparation method is the same as in Example 1, except that acryloyl polylysine is not added. The composition of each group of the antibacterial tissue adhesion layer is shown in Table 1. An asymmetric adhesion Janus antibacterial tissue patch #8 with a thickness of 40 μm was prepared.
[0120] Example 8: Adhesion Strength Test
[0121] The adhesive strength of the asymmetrically adhered Janus antimicrobial tissue patch #1-8 was tested according to YY / T 0729.3-2009 "Test Methods for Adhesive Properties of Tissue Adhesives - Part 3: Tensile Strength". The specific steps are as follows:
[0122] Using cyanoacrylate adhesive, tissue patches and fresh pigskin, each measuring 2.5cm x 2.5cm, were bonded to the test substrate. After the cyanoacrylate adhesive cured, the tissue patches and pigskin were bonded together, and a force of 2N was applied to the bonding area. Tensile strength tests were then performed using a testing machine. The testing speed was a constant 10mm / min, and the samples were loaded until failure. The maximum load at which the tissue patches and pigskin failed was the adhesive strength. The results are shown in Table 1.
[0123] Table 1. Distribution ratio and adhesive strength of each component in the tissue patch
[0124]
[0125] The results showed that the adhesive strength of the tissue patch increased with the increase of the maleimide acrylate content. When the maleimide acrylate content reached a certain proportion, the effect on the adhesive strength was not particularly significant. With the increase of the acryloyl polylysine content, the adhesive strength showed an increasing trend, but when the acryloyl polylysine content reached a certain proportion, the effect on the adhesive strength was not particularly significant.
[0126] Example 9: Cytotoxicity Evaluation Test
[0127] L929 cells were cultured in DMEM medium containing 10% fetal bovine serum and 1% penicillin-dextrose antibiotics at 37°C in a 5% CO2 incubator. Cells were digested with 0.25% trypsin to prepare a single-cell suspension. The cell suspension was centrifuged, and the cells were then redispersed in the culture medium, adjusting the cell density to 1*102. 5Cell suspension was prepared at 100 μL / mL. The cell suspension was seeded into 96-well plates at 100 μL per well and incubated at 37°C with 5% CO2 for 24 h. After the cells formed a monolayer, the original culture medium was aspirated, and 100 μL of the sample extracts from Examples 1-7, Comparative Example 1, blank control, negative control (high-density polyethylene) extract, and positive control (DMSO) were added. The plates were incubated at 37°C with 5% CO2 for 24 h. After 24 hours of incubation, the original culture medium was aspirated, and 50 μL of MTT was added to each well. The plates were incubated at 37°C with 5% CO2 for 2 h. The supernatant was aspirated, and 100 μL of isopropanol was added to dissolve the crystals. The absorbance at 570 nm was measured using a microplate reader, and cell viability was calculated. The cell viability results are shown below. Figure 2 As shown.
[0128] The results showed that the cell viability of L929 cells cultured from the tissue patches prepared in Examples 1-7 and Comparative Example 1 was all above 90%, indicating that the tissue patches prepared in Examples 1-7 and Comparative Example 1 had good biocompatibility.
[0129] Example 10: Antibacterial Performance Evaluation Test
[0130] The antibacterial properties of tissue patches prepared in Examples 1-7 and Comparative Example 1 were tested using the inhibition zone method. After sterilization by ultraviolet irradiation in a clean bench, 100 μL of Escherichia coli and Staphylococcus aureus suspensions (1*10⁻⁶) were taken respectively. 8 Add CFU / mL to LB medium, spread evenly with a spreader to ensure complete coverage of the agar plate counting plate, then attach 10 mm diameter tissue patches to the medium and incubate at 37°C for 24 h. After 24 h of incubation, remove the medium to observe bacterial growth and record the diameter of the inhibition zone. The results are shown in Table 2.
[0131] Table 2. Diameter of the inhibition zone on tissue patches
[0132]
[0133] The results showed that no inhibition zone appeared in the tissue patch of Comparative Example 1, indicating that it did not have antibacterial properties. When the acryloyl polylysine component was introduced, an inhibition zone began to appear, and as the content of acryloyl polylysine increased, the inhibition zone became more and more obvious and the diameter of the inhibition zone became larger and larger. It can be seen that the antibacterial tissue patch of the present invention has good antibacterial properties.
[0134] It should be understood that the above embodiments are exemplary and are not intended to encompass all possible implementations included in the claims. Various modifications and changes can be made to the above embodiments without departing from the scope of this disclosure. Similarly, the various technical features of the above embodiments can be arbitrarily combined to form other embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments only illustrate several implementations of the present invention and do not limit the scope of protection of this patent.
Claims
1. An antibacterial tissue patch, the tissue patch comprising a carrier layer and an antibacterial tissue adhesion layer, characterized in that, The antimicrobial tissue adhesion layer comprises an antimicrobial component, an adhesion component, N-vinylpyrrolidone, and acrylic acid, wherein the antimicrobial component includes acryloyl polylysine; and the adhesion component is maleimide acrylate.
2. The tissue patch according to claim 1, characterized in that, The antimicrobial tissue adhesion layer is composed of acryloyl polylysine, maleimide acrylate, N-vinylpyrrolidone, and acrylic acid.
3. The tissue patch according to claim 1, characterized in that, The carrier layer is a polymer with film-forming properties.
4. The tissue patch according to claim 3, characterized in that, The carrier layer is a copolymer prepared from two or more of polylactic acid, polyglycolic acid, polycaprolactone, and polyhydroxyalkanoate.
5. The tissue patch according to claim 4, characterized in that, The carrier layer is a lactic acid-glycolic acid copolymer.
6. The tissue patch according to claim 2, characterized in that, The molar ratio of acrylic acid to maleimide acrylate is 10:1 to 1:
10.
7. The tissue patch according to claim 6, characterized in that, The molar ratio of acrylic acid to maleimide acrylate is 4:1 to 1:
4.
8. The tissue patch according to claim 7, characterized in that, The molar ratio of acrylic acid to maleimide acrylate is 1:
1.
9. The tissue patch according to claim 2, characterized in that, The molar ratio of N-vinylpyrrolidone to maleimide acrylate is 10:1 to 1:
1.
10. The tissue patch according to claim 9, characterized in that, The molar ratio of N-vinylpyrrolidone to maleimide acrylate is 5:1 to 5:
4.
11. The tissue patch according to claim 10, characterized in that, The molar ratio of N-vinylpyrrolidone to maleimide acrylate is 2:
1.
12. The tissue patch according to claim 2, characterized in that, The amount of acryloyl polylysine added is 0.05%-2% of the sum of the mass of N-vinylpyrrolidone, acrylic acid, and maleimide acrylate.
13. The tissue patch according to claim 12, characterized in that, The amount of acryloyl polylysine added is 0.1%-0.9% of the sum of the mass of N-vinylpyrrolidone, acrylic acid, and maleimide acrylate.
14. The tissue patch according to claim 13, characterized in that, The amount of acryloyl polylysine added is 0.7% of the sum of the mass of N-vinylpyrrolidone, acrylic acid, and maleimide acrylate.
15. A method for preparing a tissue patch according to any one of claims 1-14, characterized in that, The method includes: (a) Preparation of the carrier layer; (b) Preparation of an antibacterial tissue adhesion layer; (c) Preparation of antimicrobial tissue patches.
16. The method according to claim 15, characterized in that, Step (b) includes: (b1) Preparation of maleimide acrylate; (b2) Preparation of acryloyl polylysine; (b3) Prepare an antibacterial tissue adhesion layer solution.
17. The method according to claim 16, characterized in that: The preparation of the carrier layer in step (a) involves coating the film-forming polymer solution into a carrier layer and then drying it. The preparation of maleimide acrylate in step (b1) involves adding acrylic monomer to tetrahydrofuran, adding a dicyclohexylcarbodiimide solution of tetrahydrofuran while stirring, adding a hydroxyethylmaleimide solution dissolved in tetrahydrofuran after stirring, filtering under reduced pressure after the reaction is complete, rotary evaporating, adding diethyl ether, filtering again, rotary evaporating, and then drying. The preparation of acryloyl polylysine in step (b2) involves adding polylysine and acrylic acid monomer to MES buffer, dissolving them, and then adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide in MES buffer. After the reaction is complete, the mixture is dialyzed with purified water and then dried. The preparation of the antibacterial tissue adhesion layer solution in step (b3) involves adding N-vinylpyrrolidone, acrylic acid, maleimide acrylate and acryloyl polylysine to purified water in a certain proportion, stirring until uniform, adding a photoinitiator, and stirring until uniform in the dark. The preparation of the antibacterial tissue patch in step (c) involves coating the antibacterial tissue adhesion layer solution prepared in step (b3) onto the carrier layer prepared in step (a), irradiating it with ultraviolet light, and then drying it.
18. The use of a tissue patch according to any one of claims 1-14 in the preparation of tissue or organ repair products for humans or animals.
Citation Information
Patent Citations
Polymerizable composition for ophthalmic and medical use and antibacterial composition obtained by polymerizing same
CN103298495A
Tissue patch and preparation method thereof
CN111375084A
Preparation method and application of acrylic acid / epsilon-polylysine adhesive antibacterial hydrogel
CN112876694A
Bioabsorbable tissue sealing patch and preparation method thereof
CN114209873A